Method for recovering and powdering alloy coarse powder

Through the steps of screening, grinding and resmelting, the vacuum suspension smelting and atomization powdering technology of water-cooled copper crucibles was used to solve the problem that titanium alloy coarse powder could not be reused, and the low-cost preparation and finished products of titanium-aluminum alloy powder were achieved. Recycling with performance in compliance with requirements.

CN118989342APending Publication Date: 2024-11-22AEROSPACE HIWING HARBIN TITANIUM IND
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202310568933.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-19
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The by-products of titanium alloy powder produced during laser and electron beam 3D printing can no longer be used for printing, resulting in a backlog of inventory, and its low cost, high purity and ingredient uniformity cannot be effectively utilized, resulting in high raw material costs and low profit expectations The problem.

Method used

Through the steps of screening, grinding, cutting and resmelting, the titanium alloy coarse powder is mixed with the alloy condensation shell and high-purity elemental metal, and the vacuum suspension smelting and atomization powdering technology of water-cooled copper crucible is used to prepare titanium aluminum that meets the requirements. Alloy powder reduces raw material costs and controls component uniformity.

Benefits of technology

The low-cost preparation of titanium-aluminum alloy powder has been achieved, which reduces the cost of raw materials by about 95%, reduces waste powder inventory, and meets the finished product performance requirements of titanium-aluminum alloy parts in the aerospace field, realizing the recycling of coarse powder.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118989342A_ABST
    Figure CN118989342A_ABST
Patent Text Reader

Abstract

The invention discloses a method for recycling and powdering alloy coarse powder, and belongs to the technical field of low-cost recycling and re-powdering of alloy coarse powder. The method solves the problems that in the titanium-aluminum alloy powder preparation process, components of easily-burnt elements are controlled, and alloy coarse powder waste cannot be recycled. According to the method, the alloy coarse powder, the alloy skull and the high-purity elemental metal serve as raw materials, the alloy powder is prepared through a water-cooled copper crucible vacuum suspension smelting gas atomization powder preparation method, the recycled materials and the high-purity metal are adopted for replacing titanium ingot smelting powder preparation, and the raw material cost input can be reduced by about 95%; the raw material cost for preparing the titanium-aluminum alloy powder is greatly reduced, and the stock of waste powder is reduced. And the prepared alloy powder is uniform in component, the sphericity degree, the oxygen content, the fluidity and other powder properties all meet the use requirements of titanium-aluminum alloy parts needed in the aerospace field, and cyclic utilization of coarse powder is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for recovering and milling alloy coarse powder, and belongs to the technical field of low-cost recovery and re-milling of alloy coarse powder. Background Art

[0002] Laser and electron beam additive manufacturing (3D printing) is an important means of manufacturing complex structure titanium alloy parts by short process and near net shape, and is also a key technology to achieve low cost of titanium alloy parts. The particle size of spherical titanium alloy powder used in laser powder bed 3D printing is 15-53μm, and the particle size of spherical titanium alloy powder used in electron beam 3D printing is 53-150μm. Therefore, in the process of producing spherical titanium alloy powder for laser and electron beam 3D printing, enterprises will produce about 40% to 50% of coarse powder by-products, which can no longer be used for laser or electron beam 3D printing, resulting in an inventory backlog of coarse powder by-products.

[0003] Titanium alloy coarse powder byproducts have outstanding advantages of low cost, highly uniform composition, high purity, and uniform and fine microstructure. The oxygen content of spherical titanium alloy coarse powder is lower than that of fine powder, usually less than 0.09wt%. Compared with spherical titanium alloy fine powder for 3D printing, powder production companies have lower profit expectations for titanium alloy coarse powder byproducts and lower costs. These spherical titanium alloy coarse powder byproducts cannot be used for laser or electron beam 3D printing and are basically in a state of inventory backlog. Therefore, how to develop and reuse these coarse powder byproducts to manufacture high-quality and low-cost titanium alloy parts has important economic benefits and engineering application value. Summary of the invention

[0004] In order to solve the above technical problems, the present invention provides a method for recovering and milling alloy coarse powder.

[0005] The technical solution of the present invention:

[0006] One of the purposes of the present invention is to provide a method for recovering alloy coarse powder and preparing powder, the method comprising the following steps:

[0007] (1) After the alloy powder is prepared, the powder is sieved and accurately classified into three particle sizes of 15-53 μm, 53-106 μm, and 106-150 μm, and the remaining powder particle size is 150 μm-1 mm alloy coarse powder;

[0008] (2) After the alloy powder is prepared, the alloy condensate shell remaining on the inner wall of the water-cooled copper crucible is polished to remove the surface oxide scale;

[0009] (3) Cut the polished alloy shell into small pieces by wire cutting or other methods for later use;

[0010] (4) According to the element composition ratio of the alloy powder to be prepared, weigh the alloy coarse powder, alloy condensate shell, high-purity elemental metal, and pure titanium sheath for use;

[0011] (5) The raw materials weighed in (4) are respectively placed in a pure titanium sheath and placed in a water-cooled copper crucible, and a mixture of alloy coarse powder, alloy condensed shell, and high-purity elemental metal is naturally spread inside the sheath in the pure titanium sheath;

[0012] (6) melting and stirring the alloy melt uniformly;

[0013] (7) Use high-purity argon gas atomization to prepare powder to obtain alloy powder.

[0014] It is further defined that the sum of the mass of the alloy coarse powder and the alloy shell in (4) is 60% to 64% of the total mass of the alloy powder to be obtained.

[0015] It is further defined that the purity of the high-purity elemental metal in (4) is 99.9%.

[0016] It is further defined that the smelting in (6) is to place (5) into a water-cooled copper crucible and start a vacuum pump in the smelting chamber to make the vacuum degree reach 1Pa.

[0017] It is further defined that (6) the smelting chamber and the atomizing chamber are less than 150 Pa / h.

[0018] It is further defined that during the smelting in (6), the melt temperature is 1750-1800°C and the temperature is maintained for 3 minutes.

[0019] It is further defined that the atomization powder making in (7) is to turn on the fan system and the pressure of the atomization chamber reaches 80-90KPa.

[0020] It is further defined that the atomization powder making in (7) is high-purity argon atomization, and the argon atomization pressure is 4±0.5 MPa.

[0021] It is further defined that the atomization powder in (7) is made of high-purity argon gas, and the purity of the argon gas is 99.999%.

[0022] The second object of the present invention is to provide a titanium-aluminum alloy powder obtained by the above method, specifically the titanium-aluminum alloy powder is composed of the following element content ratio: Al 30-35wt%, Cr 2-3wt%, Nb 4-5wt%, Mo 1-2wt%, V0.5-1wt%, and the balance is Ti.

[0023] It is further defined that the particle size of the titanium aluminum alloy powder is in the range of 1 μm-1 mm.

[0024] It is further defined that the oxygen content of the titanium aluminum alloy powder is ≤ 0.09 wt %.

[0025] Compared with the prior art, the present invention has the following beneficial effects:

[0026] (1) The present invention uses gold coarse powder, alloy shell and high-purity elemental metal powder as raw materials for remelting and powdering, instead of smelting and powdering titanium ingots, which can reduce the raw material cost input by about 95%, greatly reduce the raw material cost of titanium aluminum alloy powder preparation, and reduce waste powder inventory.

[0027] (2) The present invention prepares alloy powder by a water-cooled copper crucible vacuum suspension melting gas atomization powder making method. Since low-melting-point metals burn out during the melting process, the present invention increases the pure metal content of easily burnt metal elements according to their burnout amount during the batching process, thereby further controlling the chemical composition of the alloy powder and avoiding the problem that the alloy powder composition does not meet the standard chemical composition due to element burnout.

[0028] (3) The present invention utilizes a water-cooled copper crucible vacuum suspension smelting gas atomization technology to prepare powder. Specifically, after the alloy melt is stirred evenly, high-purity argon gas is used for powder atomization, so that the composition of the prepared alloy powder is uniform, and the powder properties such as sphericity, oxygen content, and fluidity meet the use requirements of titanium aluminum alloy parts in the aerospace field, thereby realizing the recycling of coarse powder. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 This is a schematic diagram of the raw materials loading furnace in Example 1;

[0030] Figure 2 This is a physical picture of the alloy powder obtained in Example 1. DETAILED DESCRIPTION

[0031] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with the embodiments of the specification.

[0032] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.

[0033] Secondly, the term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The term "in one embodiment" that appears in different places in this specification does not necessarily refer to the same embodiment, nor does it refer to a separate or selective embodiment that is mutually exclusive with other embodiments.

[0034] The experimental methods used in the following examples are conventional methods unless otherwise specified. The materials, reagents, methods and instruments used are conventional materials, reagents, methods and instruments in the art unless otherwise specified, and can be obtained through commercial channels by those skilled in the art.

[0035] Example 1

[0036] This embodiment provides a method for preparing titanium-aluminum alloy powder using titanium-aluminum alloy coarse powder. The equipment adopts a 25kg-level water-cooled copper tongs pot. Taking the production of 20kg of feed as an example, the method specifically includes the following steps:

[0037] (1) Weigh 5kg of alloy coarse powder, 1kg of alloy condensate, 8.75kg of pure titanium sheath + titanium sponge, 4.2kg of aluminum metal, and 0.28kg of chromium metal powder for later use. The particle size of the alloy coarse powder is 150μm-1mm; the alloy condensate is polished to remove the oxide scale on the surface of the alloy condensate, clean the surface of the alloy condensate, and effectively reduce the oxygen content of the finished alloy powder.

[0038] (2) The raw materials weighed in (1) are respectively placed in a pure titanium sheath and placed in a water-cooled copper crucible. In the pure titanium sheath, a mixture of alloy coarse powder, alloy condensed shell, and high-purity elemental metal is naturally spread inside the sheath. Figure 1 shown.

[0039] (3) Melting and stirring the alloy melt evenly; the specific melting process is to turn on the vacuum pump in the melting chamber to make the vacuum degree reach 1Pa; check the leakage rate of the melting chamber, the melting chamber and the atomization chamber are less than 150Pa / h; test the melt temperature, the melt temperature reaches 1750-1800℃ and keeps warm for 3 minutes.

[0040] (4) Using high-purity argon gas atomization to make powder, specifically, the atomization powder making includes turning on the fan system, the atomization chamber pressure reaches 80-90 KPa; high-purity argon gas atomization, the argon gas atomization pressure is 4±0.5 MPa; the argon gas purity is 99.999%.

[0041] The alloy powder prepared is composed of the following element content ratios: Al31.2wt%, Cr2.65wt%, Nb4.33wt%, Mo 1.88wt%, V0.57wt%, and the balance is Ti. The obtained alloy powder has an oxygen content of 0.085wt%, such as Figure 2 The obtained alloy powder has uniform composition, and the powder properties such as sphericity, oxygen content, and fluidity all meet the use requirements of titanium aluminum alloy parts in the aerospace field.

[0042] Although the present invention has been disclosed as above in the preferred embodiment, it is not intended to limit the present invention. Anyone familiar with this technology can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention should be based on the definition of the claims.

Claims

1. A method for recovering and milling alloy coarse powder, characterized in that: include: (1) After the alloy powder is prepared, the powder is sieved and accurately classified into three particle sizes of 15-53 μm, 53-106 μm, and 106-150 μm, and the remaining powder particle size is 150 μm-1 mm alloy coarse powder; (2) After the alloy powder is prepared, the alloy condensate shell remaining on the inner wall of the water-cooled copper crucible is polished to remove the surface oxide scale; (3) Cut the polished alloy shell into small pieces by wire cutting or other methods for later use; (4) According to the element composition ratio of the alloy powder to be prepared, weigh the alloy coarse powder, alloy condensate shell, high-purity elemental metal, and pure titanium sheath for use; (5) The raw materials weighed in (4) are respectively placed in a pure titanium sheath and placed in a water-cooled copper crucible, and a mixture of alloy coarse powder, alloy condensed shell, and high-purity elemental metal is naturally spread inside the sheath in the pure titanium sheath; (6) melting and stirring the alloy melt uniformly; (7) Use high-purity argon gas atomization to prepare powder to obtain alloy powder.

2. The method for recovering and milling alloy coarse powder according to claim 1, characterized in that: (4) The sum of the masses of the alloy coarse powder and the alloy shell is 60% to 64% of the total mass of the alloy powder to be produced.

3. The method for recovering and milling alloy coarse powder according to claim 1, characterized in that: (4) The purity of medium- and high-purity elemental metals is ≥99.9%.

4. The method for recovering and milling alloy coarse powder according to claim 1, characterized in that: (6) For medium smelting, the vacuum pump is turned on in the smelting chamber to make the vacuum degree reach 1Pa; the smelting chamber and the atomizing chamber are less than 150Pa / h.

5. The method for recovering and milling alloy coarse powder according to claim 1, characterized in that: (6) The melt temperature reaches 1750-1800°C and is kept at this temperature for 3 minutes.

6. The method for recovering and milling alloy coarse powder according to claim 1, characterized in that: (7) For medium atomization powder making, the fan system is turned on, and the pressure of the atomization chamber reaches 80-90KPa; high-purity argon gas, argon purity 99.999%, and the atomization pressure is 4±0.5MPa.

7. A titanium aluminum alloy powder obtained by the method according to any one of claims 1 to 7, characterized in that The alloy is composed of the following element content ratios: Al 30-35wt%, Cr 2-3wt%, Nb 4-5wt%, Mo 1-2wt%, V 0.5-1wt%, and the balance is Ti.

8. The titanium aluminum alloy powder according to claim 8, characterized in that The particle size of the powder is in the range of 1 μm to 1 mm.

9. The titanium aluminum alloy powder according to claim 8, characterized in that The oxygen content is ≤0.09wt%.

Citation Information

Cited By

  • Method for preparing spherical metal fine powder from coarse / waste powder through ultrasonic atomization

    CN121339455A