Welding process of FPSO (floating production storage and offloading) riser system

By performing bevel processing, preheating and multi-stage welding processes on the surfacing composite pipelines and surfacing composite flanges of the FPSO riser system, combining manual and automatic welding technology, and post-weld heat treatment, the weld performance is solved and Welding cracks have improved welding efficiency and quality.

CN118989530APending Publication Date: 2024-11-22YANTAI TIEZHONGBAO STEEL PROCESSING CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411300317.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-18
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

In the welding process of surfacing composite pipes and surfacing composite flanges in the FPSO riser system, there are problems such as insufficient weld performance, easy welding cracks and low welding efficiency.

Method used

A welding process is adopted, including bevel processing, preheating, manual tungsten argon arc welding and automatic tungsten argon arc welding, the specific steps are base welding, thermal welding, Fill welding and cover welding, and post-weld heat treatment is performed after welding is completed.

Benefits of technology

It effectively solves the problems of insufficient weld performance and welding crack defects, reduces the quantity demand for welders, reduces costs, and improves welding quality and production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118989530A_ABST
    Figure CN118989530A_ABST
Patent Text Reader

Abstract

The invention relates to a welding process of an FPSO (floating production storage and offloading) vertical pipe system. The welding process comprises the step of performing groove processing on a surfacing composite pipeline and a surfacing composite flange according to a preset groove size. And the groove end of the surfacing composite pipeline and the groove end of the surfacing composite flange are assembled. And a groove area formed by assembling is preheated. And the preheated surfacing composite pipeline and surfacing composite flange are welded, and the welding sequence is that backing welding is conducted firstly, then hot welding is conducted, refilling welding is conducted, and cosmetic welding is conducted finally. Manual welding is adopted for backing welding and hot welding, and automatic welding is adopted for filling welding and cosmetic welding. And after welding is completed, postweld heat treatment is conducted immediately. By means of the welding process, the problems that the performance of the FPSO vertical pipe system pipeline and flange weld joint is insufficient and the welding crack defect exists can be effectively solved. Semi-automatic welding is adopted in the welding process, the requirement for the number of welders is reduced, and cost is reduced. Welding process parameters can be accurately controlled through automatic welding, and the welding quality is improved; the welding time is shortened, and the production efficiency is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of marine engineering, and in particular to a welding process for an FPSO riser system. Background Art

[0002] Floating Production Storage and Offloading (FPSO) is a large-scale offshore oil production base that separates oil and gas from the extracted oil, treats oily wastewater, generates power, provides heat, and stores and transports crude oil products, and integrates personnel accommodation and production command systems. Compared with other forms of oil production platforms, FPSO has the advantages of strong wind and wave resistance, wide range of adaptability to water depths, large storage / unloading capacity, and transferability and reusability. It is widely suitable for the development of deep sea, shallow sea areas and marginal oil fields far from the coast, and has become the mainstream production method for offshore oil and gas field development.

[0003] Thanks to their low cost and excellent corrosion resistance, cladding composite pipes and cladding composite flanges are increasingly used in FPSO riser systems. Among them, cladding composite pipes include a base pipe located on the outside and a cladding layer located on the inside. The base pipe is generally low-carbon steel, which plays a role in pressure bearing and support to ensure the overall mechanical properties of the composite pipe; the cladding layer uses a nickel-based alloy with excellent corrosion resistance. The flanges in the FPSO riser system have higher strength grade requirements than the pipelines, so cladding composite flanges generally use medium-carbon alloy steel as the base material and a nickel-based alloy as the cladding layer.

[0004] In the FPSO riser system, the welding of cladding composite pipes and cladding composite flanges involves three materials: low carbon steel, medium carbon alloy steel, and nickel-based alloy, and the welding process is complicated. In addition, the nickel-based alloy cladding layer has poor weldability, which can easily lead to insufficient weld performance; alloy steel flanges are prone to welding cracks; cladding composite pipes and cladding composite flanges have thick walls, and manual welding efficiency is low. Summary of the invention

[0005] One purpose of the present invention is to solve the problems existing in the prior art, such as insufficient weld performance, easy generation of welding cracks and low welding efficiency, and to provide a welding process for a FPSO riser system. To solve the above technical problems, the present invention adopts the following technical solutions:

[0006] A welding process for an FPSO riser system is used for welding the FPSO riser system, wherein the FPSO riser system comprises a cladding composite pipe and a cladding composite flange; the welding process comprises:

[0007] Beveling of cladding composite pipes and cladding composite flanges is performed according to preset bevel dimensions;

[0008] Assemble the groove end of the cladding composite pipe and the groove end of the cladding composite flange;

[0009] Preheating the groove area formed by the cladding composite pipe and the cladding composite flange assembly;

[0010] Welding the preheated cladding composite pipe and cladding composite flange;

[0011] The welding sequence is to first use manual tungsten inert gas welding to perform the base welding between the cladding composite pipe and the cladding composite flange; then use manual tungsten inert gas welding to perform the hot welding between the cladding composite pipe and the cladding composite flange; then use automatic tungsten inert gas welding to perform the filling welding between the cladding composite pipe and the cladding composite flange; finally use automatic tungsten inert gas welding to perform the cover welding between the cladding composite pipe and the cladding composite flange;

[0012] After welding is completed, post-weld heat treatment is carried out immediately.

[0013] In one embodiment, in the step of preheating the groove area formed by the cladding composite pipe and the cladding composite flange assembly, the preheating temperature is 120°C to 150°C.

[0014] In one embodiment, the process parameters of the base welding include: welding current 90A-110A, welding voltage 9.5V-11V, welding speed 50mm / min-70mm / min, and interlayer temperature 130°C-160°C.

[0015] In one embodiment, the process parameters of thermal welding include: welding current 110A-130A, welding voltage 10V-13V, welding speed 70mm / min-90mm / min, and interlayer temperature 130°C-160°C.

[0016] In one of the embodiments, the process parameters of the filling welding include: peak current 230A~250A, base current 160A~180A, pulse frequency 2.5HZ, welding voltage 11V~13V, welding speed 160mm / min~180mm / min, wire feeding speed 1200mm / min~1300mm / min, and interlayer temperature 135℃~175℃.

[0017] In one embodiment, the process parameters of the cover welding include: welding current 220A~240A, welding voltage 11V~13V, welding speed 150mm / min~170mm / min, wire feeding speed 1100mm / min~1200mm / min, and interlayer temperature 135℃~165℃.

[0018] In one embodiment, the number of fill welding passes is multiple, and when automatic tungsten inert gas arc welding is used for fill welding, the multiple weld passes are sequentially stacked from the cladding composite pipe toward the cladding composite flange, and sequentially stacked from the inner wall of the pipe toward the outer wall of the pipe;

[0019] There are multiple weld passes for the cover welding. When automatic tungsten inert gas welding is used for the cover welding, multiple weld passes are superimposed in sequence from the cladding composite pipe toward the cladding composite flange.

[0020] In one embodiment, after welding is completed, in the step of post-weld heat treatment immediately, the heat treatment temperature is 610° C. to 630° C., and the holding time is not less than 1.25 hours.

[0021] In one embodiment, the groove of the cladding composite pipe and the groove of the cladding composite flange respectively include a first groove, a second groove and a blunt edge, and the first groove, the second groove and the blunt edge are arranged in sequence from the outer wall of the pipe to the inner wall of the pipe, the groove angle of the first groove is 7.5° to 12.5°, the groove angle of the second groove is 35° to 40°, and the thickness of the blunt edge is 1mm to 2mm.

[0022] In one embodiment, in the step of assembling the groove end of the cladding composite pipe and the groove end of the cladding composite flange, the gap between the blunt edge of the cladding composite pipe and the blunt edge of the cladding composite flange is 4 mm to 5 mm, and the error is ≤1 mm.

[0023] In one embodiment, after the step of performing groove processing on the cladding composite pipe and the cladding composite flange according to the preset groove size, the method further includes:

[0024] Pre-clean the groove and surrounding areas of the cladding composite pipe and cladding composite flange before welding to remove oil, dirt, paint and rust from the groove and surrounding areas.

[0025] In one embodiment, before the step of preheating the groove area formed by the cladding composite pipe and the cladding composite flange assembly, the method further includes:

[0026] The groove area formed by the cladding composite pipe and the cladding composite flange assembly is protected by back argon gas.

[0027] It can be seen from the above technical solution that the present invention has at least the following advantages and positive effects:

[0028] In the present invention, by designing the groove, preheating the groove area, and designing the welding sequence, the problems of insufficient performance of weld joints and welding crack defects of the cladding composite pipe and cladding composite flange of the FPSO riser system can be effectively solved.

[0029] In addition, manual welding is used for base welding and hot welding, and automatic welding is used for filling welding and capping welding. The entire welding process adopts semi-automatic welding, which reduces the demand for welders and reduces costs. Automatic welding is used for filling welding and capping welding, which can accurately control the welding process parameters, reduce the influence of human factors, and make the welding quality stable and reliable. In addition, automatic welding can shorten the welding time and help improve production efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 It is a schematic diagram of the state of the groove area of ​​the FPSO riser system before welding according to one embodiment of the present invention.

[0031] Figure 2 The figure is a schematic flow chart of a welding process for a FPSO riser system according to an embodiment of the present invention.

[0032] Figure 3 yes Figure 2 A specific flow chart of step S60 in the process shown.

[0033] Figure 4 It is a schematic diagram of the state of the groove area of ​​the FPSO riser system after welding according to one embodiment of the present invention.

[0034] The following are the descriptions of the reference numerals:

[0035] 100-welding composite pipe; 110-base pipe; 120-pipe cladding layer;

[0036] 200-welding composite flange; 210-base material flange; 220-flange cladding layer;

[0037] 300-bevel;

[0038] 310-first groove; 320-second groove; 330-blunt edge. DETAILED DESCRIPTION

[0039] Typical embodiments that embody the features and advantages of the present invention will be described in detail in the following description. It should be understood that the present invention can have various changes in different embodiments without departing from the scope of the present invention, and the descriptions and illustrations therein are essentially used for illustration purposes rather than for limiting the present invention.

[0040] In the description of the present application, it should be understood that in the embodiments shown in the drawings, the indications of directions or positional relationships (such as up, down, left, right, front and back, etc.) are only for the convenience of describing the present application and simplifying the description, rather than indicating or implying that the devices or elements referred to must have a specific orientation, be constructed and operate in a specific orientation. These descriptions are appropriate when these elements are in the positions shown in the drawings. If the descriptions of the positions of these elements change, the indications of these directions also change accordingly.

[0041] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Thus, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of this application, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.

[0042] The welding process of the riser system of the floating production storage and offloading device FPSO (Floating Production Storage and Offloading) according to the embodiment of the present invention is used for welding the riser system of the FPSO. Figure 1 As shown, the FPSO riser system includes a cladding composite pipe 100 and a cladding composite flange 200 .

[0043] The cladding composite pipe 100 includes a base pipe 110 and a pipe cladding layer 120, and the pipe cladding layer 120 is disposed on the inner wall of the base pipe 110. The base pipe 110 may be made of low carbon steel, and the pipe cladding layer 120 may be made of a nickel-based alloy.

[0044] The cladding composite flange 200 includes a base flange 210 and a flange cladding layer 220, wherein the flange cladding layer 220 is disposed on the inner wall of the base flange 210. The base flange 210 may be made of medium carbon alloy steel, and the flange cladding layer 220 may be made of nickel-based alloy.

[0045] See also Figure 2 As shown, the welding process includes: S10, performing groove processing on the cladding composite pipe 100 and the cladding composite flange 200 according to the preset groove size. In S10, a special pipe end groove machine can be used to perform groove processing on the cladding composite pipe 100 and the cladding composite flange 200 to be welded.

[0046] like Figure 1As shown, in one embodiment, the groove 300 of the cladding composite pipe 100 and the groove 300 of the cladding composite flange 200 respectively include a first groove 310, a second groove 320 and a blunt edge 330, and the first groove 310, the second groove 320 and the blunt edge 330 are arranged in sequence from the outer wall of the pipe to the inner wall of the pipe.

[0047] Specifically, in S10, the preset groove dimensions may be: the groove angle A1 of the first groove 310 is 7.5° to 12.5°, the groove angle A2 of the second groove 320 is 35° to 40°, and the thickness T of the blunt edge 330 is 1 mm to 2 mm.

[0048] See also Figure 2 In one embodiment, after step S10, that is, after the groove processing is completed, it also includes S20: pre-cleaning the groove 300 and the surrounding area of ​​the cladding composite pipe 100 and the cladding composite flange 200 before welding, including cleaning the groove 300 and the surrounding area of ​​the cladding composite pipe 100, and the groove 300 and the surrounding area of ​​the cladding composite flange 200. Harmful substances such as oil, dirt, paint and rust are cleaned, so as to ensure welding quality.

[0049] See also Figure 2 The welding process further includes: S30, assembling the groove end of the cladding composite pipe 100 and the groove end of the cladding composite flange 200. Figure 1 As shown, after the cladding composite pipe 100 and the cladding composite flange 200 are assembled, a roughly V-shaped groove area can be formed. In the embodiment of the present invention, the design of the V-shaped composite groove area is adopted, so that the filling amount of the weld metal is significantly reduced. This is conducive to reducing welding time and saving costs.

[0050] For example, in S30, when the groove end of the cladding composite pipe 100 and the groove end of the cladding composite flange 200 are assembled, the gap L between the blunt edge 330 of the cladding composite pipe 100 and the blunt edge 330 of the cladding composite flange 200 can be 4 mm to 5 mm, and the error amount is ≤1 mm.

[0051] See also Figure 2 , the welding process also includes: S50, preheating the groove area formed by the cladding composite pipe 100 and the cladding composite flange 200. The preheating temperature can be 120°C to 150°C. The preheating range can include the groove 300 of the cladding composite pipe 100 and a certain range of its groove end, and the groove 300 of the cladding composite flange 200 and a certain range of its groove end. The preheating method can be selected according to the pipe diameter and the configuration of the construction site equipment, such as induction heating, electric heating or flame heating. By preheating, the temperature gradient can be reduced, the crack tendency of the flange can be eliminated, and the welding quality can be improved.

[0052] In S50, a contact temperature measuring instrument may be used to measure the temperature of the groove end of the cladding composite pipe 100 and the groove end of the cladding composite flange 200. Specifically, four temperature measuring points may be evenly arranged around the groove end of the cladding composite pipe 100. Four temperature measuring points may be evenly arranged around the groove end of the cladding composite flange 200. By measuring the temperature, it is ensured that the preheating temperature is reached, and the accuracy and uniformity of the preheating are guaranteed.

[0053] See also Figure 2 In one embodiment, before S50, it also includes: S40, performing argon protection on the back of the groove area formed by the cladding composite pipe 100 and the cladding composite flange 200. The specific method can be to seal the 200mm position of the groove end of the cladding composite pipe 100 and the cladding composite flange 200, and use high-temperature resistant tin foil to seal the outer surface of the weld. The back of the weld is filled with argon gas from bottom to top to exhaust the air, and the argon flow rate is 20L / min~25L / min, ensuring that the oxygen content is less than 500ppm. By performing argon protection on the back of the welding area, poor forming and welding defects can be avoided.

[0054] In the embodiment of the present application, when the preheating temperature reaches the preset temperature, the cladding composite pipe 100 and the cladding composite flange 200 can be welded. Figure 2 The welding process further includes: S60, welding the preheated cladding composite pipe 100 and the cladding composite flange 200.

[0055] like Figure 3 As shown, S60 specifically includes:

[0056] S61, firstly, manual tungsten inert gas arc welding is used to perform base welding between the cladding composite pipe 100 and the cladding composite flange 200. The welding wire may be ERNiCrMo-3 solid welding wire, and the diameter of the welding wire may be 2.4 mm.

[0057] In one embodiment, the process parameters of the base welding include: welding current 90A-110A, welding voltage 9.5V-11V, welding speed 50mm / min-70mm / min, and interlayer temperature 130°C-160°C.

[0058] In S61, a contact temperature measuring instrument may be used to measure the temperature of the groove end of the cladding composite pipe 100 and the groove end of the cladding composite flange 200. Specifically, four temperature measuring points may be evenly arranged around the groove end of the cladding composite pipe 100. Four temperature measuring points may be evenly arranged around the groove end of the cladding composite flange 200. By measuring the temperature, it is possible to ensure that the interlayer temperature is reached, and the accuracy and uniformity of the interlayer temperature are guaranteed.

[0059] S62, using manual tungsten inert gas arc welding to perform thermal welding between the cladding composite pipe 100 and the cladding composite flange 200. The welding wire may be ERNiCrMo-3 solid welding wire, and the diameter of the welding wire may be 2.4 mm.

[0060] In one embodiment, the process parameters of thermal welding include: welding current 110A-130A, welding voltage 10V-13V, welding speed 70mm / min-90mm / min, and interlayer temperature 130°C-160°C.

[0061] In S62, a contact temperature measuring instrument may be used to measure the temperature of the groove end of the cladding composite pipe 100 and the groove end of the cladding composite flange 200. Specifically, four temperature measuring points may be evenly arranged around the groove end of the cladding composite pipe 100. Four temperature measuring points may be evenly arranged around the groove end of the cladding composite flange 200. By measuring the temperature, it is possible to ensure that the interlayer temperature is reached, and the accuracy and uniformity of the interlayer temperature are guaranteed.

[0062] S63, automatic tungsten inert gas arc welding is used to perform filling welding between the cladding composite pipe 100 and the cladding composite flange 200. The automatic welding equipment can be a heavy-duty pipeline welding machine. The welding wire can be ERNiCrMo-3 solid welding wire, and the diameter of the welding wire can be 1.2 mm.

[0063] In one embodiment, the filling welding can be performed using the pulse welding mode of the automatic welding equipment. The pulse welding mode is conducive to stirring the molten pool and preventing the molten pool from becoming sticky and causing pores and unfused defects. The process parameters of the filling welding include: peak current 230A-250A, base current 160A-180A, pulse frequency 2.5HZ, welding voltage 11V-13V, welding speed 160mm / min-180mm / min, wire feeding speed 1200mm / min-1300mm / min, and interlayer temperature 135°C-175°C.

[0064] In S63, a contact temperature measuring instrument may be used to measure the temperature of the groove end of the cladding composite pipe 100 and the groove end of the cladding composite flange 200. Specifically, four temperature measuring points may be evenly arranged around the groove end of the cladding composite pipe 100. Four temperature measuring points may be evenly arranged around the groove end of the cladding composite flange 200. By measuring the temperature, it is possible to ensure that the interlayer temperature is reached, and the accuracy and uniformity of the interlayer temperature are guaranteed.

[0065] See also Figure 4As shown, in one embodiment, the number of fill welding passes is multiple. When automatic tungsten inert gas arc welding is used for fill welding, multiple weld passes are sequentially stacked from the cladding composite pipe 100 to the cladding composite flange 200, and sequentially stacked from the inner wall of the pipe to the outer wall of the pipe. Among them, from the cladding composite pipe 100 to the cladding composite flange 200, the arc starting or arc ending positions between adjacent weld passes are staggered.

[0066] For example, Figure 4 As shown, the number of filler welding welds is multiple, and the multiple welds can be represented as 4-1, 4-2, 5-1, 5-2...13-1, 13-2, 13-3. Among them, 4-1 and 4-2 are sequentially stacked from the cladding composite pipe 100 to the cladding composite flange 200...13-1, 13-2, 13-3 are sequentially stacked from the cladding composite pipe 100 to the cladding composite flange 200. At the same time, 4, 5...13 are sequentially stacked from the inner wall of the pipe to the outer wall of the pipe. That is, in this embodiment, 4-1 and 4-2 are sequentially stacked from the cladding composite pipe 100 to the cladding composite flange 200 to form a weld layer, and then 5-1 is superimposed on the weld layer formed by 4-1 and 4-2, and 5-1 and 5-2 are sequentially stacked from the cladding composite pipe 100 to the cladding composite flange 200 to form another weld layer. The layers are stacked in this way, and the welding direction of each weld in each weld layer is stacked in sequence along the direction from the cladding composite pipe 100 to the cladding composite flange 200 .

[0067] By providing a plurality of weld passes and stacking the plurality of weld passes in sequence from the cladding composite pipe 100 toward the cladding composite flange 200 and stacking them in sequence from the inner wall of the pipe toward the outer wall of the pipe, the hardenability of the flange can be reduced and the toughness of the weld can be improved.

[0068] See also Figure 3 As shown, S60 also includes S64, which uses automatic tungsten inert gas arc welding to perform cover welding between the cladding composite pipe 100 and the cladding composite flange 200. Among them, the automatic welding equipment can be a heavy-duty pipeline welding machine. The welding wire can be ERNiCrMo-3 solid welding wire, and the welding wire diameter can be 1.2mm.

[0069] In one embodiment, the cap welding can be performed using a DC welding mode of an automatic welding device. The process parameters of the cap welding include: welding current 220A-240A, welding voltage 11V-13V, welding speed 150mm / min-170mm / min, wire feeding speed 1100mm / min-1200mm / min, and interlayer temperature 135°C-165°C.

[0070] In S64, a contact temperature measuring instrument may be used to measure the temperature of the groove end of the cladding composite pipe 100 and the groove end of the cladding composite flange 200. Specifically, four temperature measuring points may be evenly arranged around the groove end of the cladding composite pipe 100. Four temperature measuring points may be evenly arranged around the groove end of the cladding composite flange 200. By measuring the temperature, it is possible to ensure that the interlayer temperature is reached, and the accuracy and uniformity of the interlayer temperature are guaranteed.

[0071] like Figure 4 As shown, in one embodiment, the number of weld passes for the cap welding is multiple. When the cap welding is performed by automatic tungsten inert gas arc welding, multiple weld passes are sequentially superimposed from the cladding composite pipe 100 to the cladding composite flange 200. Among them, from the cladding composite pipe 100 to the cladding composite flange 200, the arc starting or arc ending positions between adjacent weld passes are staggered.

[0072] For example, Figure 4 As shown, the number of weld passes for cap welding is multiple, and the multiple weld passes can be represented as 14-1, 14-2, 14-3, and 14-4, respectively. Among them, 14-1, 14-2, 14-3, and 14-4 are formed by stacking one another from the cladding composite pipe 100 toward the cladding composite flange 200. By providing multiple weld passes and stacking one another from the cladding composite pipe 100 toward the cladding composite flange 200, the hardenability of the flange can be reduced and the toughness of the weld can be improved.

[0073] See also Figure 2 The welding process further includes: S70, after welding is completed, immediately performing post-weld heat treatment. For example, in S70, the heat treatment temperature can be 610°C to 630°C. The holding time is not less than 1.25h. Through post-weld heat treatment, the structure can be homogenized, the welding stress can be eliminated or reduced, and the crack tendency can be eliminated.

[0074] See also Figure 4 As shown, in the embodiment of the present application, the number of weld passes for base welding can be 1, and 1 weld pass can form 1 weld layer. The number of weld passes for hot welding can be 2-4, and 2-4 weld passes can form 2-4 weld layers respectively. The number of weld passes for filling welding is multiple, and multiple weld passes can form multiple weld layers. The number of weld passes for cap welding can be 4-6, and 4-6 weld passes can form 1 weld layer. After welding is completed, the weld cap can be 0mm to 2mm higher than the outer wall of the pipe, that is, H2 is 0mm to 2mm.

[0075] In the embodiments of the present application, by designing each welding process and process parameter, and designing the welding sequence and weld direction arrangement, the problems of insufficient performance of weld joints and welding crack defects of the FPSO riser system cladding composite pipe 100 and cladding composite flange 200 can be effectively solved.

[0076] In the embodiment of the present application, manual welding is used for base welding and hot welding, and automatic welding is used for filling welding and capping welding. Semi-automatic welding is used for the entire welding process, which reduces the demand for the number of welders and reduces costs. Automatic welding is used for filling welding and capping welding, which can accurately control the welding process parameters, reduce the influence of human factors, and make the welding quality stable and reliable. In addition, automatic welding can shorten the welding time, which is conducive to improving production efficiency.

[0077] In the embodiment of the present application, the material of the welding wire is the same as that of the pipe cladding layer 120 and the flange cladding layer 220, which can ensure good fusion on both sides of the groove during base welding and hot welding, thereby facilitating improving welding quality.

[0078] like Figure 1 As shown, in a specific embodiment of the present application, the welding of a Φ219mm*25mm (substrate 22mm+surfacing layer 3mm) surfacing composite pipe 100 and a surfacing composite flange 200 is taken as an example for description. The substrate of the surfacing composite pipe 100 is API 5L X65QS low carbon steel, the substrate of the surfacing composite flange 200 is AISI 4130 75K medium carbon alloy steel, and the materials of the pipe surfacing layer 120 and the flange surfacing layer 220 are both ERNiCrMo-3 nickel-based alloy.

[0079] The specific implementation is as follows:

[0080] The cladding composite pipe 100 and the cladding composite flange 200 are grooved. The dimensions of the grooves of the cladding composite pipe 100 and the cladding composite flange 200 can be: the groove angle A1 of the first groove 310 is 10°. The groove angle A2 of the second groove 320 is 37.5°. The thickness T of the blunt edge 330 is 1.5 mm. The distance H1 between the intersection of the first groove 310 and the second groove 320 and the inner wall of the pipe is 18 mm to 20 mm. After the groove processing is completed, the grooves and surrounding areas of the cladding composite pipe 100 and the cladding composite flange 200 are cleaned until the metallic luster is revealed to remove impurities such as oil, dirt, paint and rust that may affect the welding quality.

[0081] The groove end of the cladding composite pipe 100 and the groove end of the cladding composite flange 200 are assembled. In the assembled state, the gap L between the blunt edge 330 of the cladding composite pipe 100 and the blunt edge 330 of the cladding composite flange 200 is 5 mm, and the deviation is 0.3 mm.

[0082] After the cladding composite pipe 100 and the cladding composite flange 200 are assembled, the groove area formed by the cladding composite pipe 100 and the cladding composite flange 200 is protected by back argon gas.

[0083] Before welding begins, the groove area formed by the cladding composite pipe 100 and the cladding composite flange 200 is preheated, wherein the preheating temperature may be 125°C.

[0084] When the preheating temperature reaches the preset temperature, the cladding composite pipe 100 and the cladding composite flange 200 are welded. Specifically, manual tungsten inert gas arc welding is first used to perform base welding on the grooves of the preheated cladding composite pipe 100 and the cladding composite flange 200. Among them, the welding wire uses ERNiCrMo-3 solid core welding wire with a diameter of 2.4mm. The process parameters of the base welding are: welding current 90A, welding voltage 9.5V, welding speed 50mm / min, and interlayer temperature 135℃.

[0085] Then, manual tungsten inert gas arc welding is used to perform hot welding on the grooves of the cladding composite pipe 100 and the cladding composite flange 200 after the base welding. Among them, the welding wire uses ERNiCrMo-3 solid welding wire with a diameter of 2.4mm. The process parameters of hot welding are: welding current 110A, welding voltage 11.5V~11.7V, welding speed 70mm / min, and interlayer temperature 136℃~159℃. Before the hot welding is completed, the groove area is continuously protected by back argon gas.

[0086] Then, the pulse welding mode of the automatic welding equipment is used to perform fill welding on the grooves of the heat-welded composite pipe 100 and the cladding composite flange 200. Among them, the welding wire uses ERNiCrMo-3 solid wire with a wire diameter of 1.2mm. The process parameters of the filling welding are: peak current 250A, base current 180A, pulse frequency 2.5HZ, welding voltage 11.3V, welding speed 170mm / min, wire feeding speed 1300mm / min, and interlayer temperature 143℃~171℃.

[0087] Finally, the DC welding mode of the automatic welding equipment is used to perform cap welding on the grooves of the cladding composite pipe 100 and the cladding composite flange 200 after filling welding. Among them, the welding wire uses ERNiCrMo-3 solid welding wire with a wire diameter of 1.2mm. The process parameters of the cap welding are: welding current 230A, welding voltage 11.3V, welding speed 160mm / min, wire feeding speed 1200mm / min, and interlayer temperature 158℃~165℃.

[0088] After welding, post-weld heat treatment is immediately carried out, wherein the heat treatment temperature is 620℃ and the holding time is 1.25h.

[0089] The state after welding can be found in detail. Figure 4 As shown. Figure 4As shown, the number of weld passes for base welding is 1. The number of weld passes for hot welding is 2. The number of weld passes for filling welding is 27. The number of weld passes for cover welding is 4. After welding, the distance H2 of the weld cover above the outer wall of the pipe is 1 mm.

[0090] In the whole welding process, the process parameters of each welding step can be specifically shown in Table 1. The process parameters of the heat treatment after welding can be specifically shown in Table 2.

[0091]

[0092]

[0093] Table 1

[0094]

[0095]

[0096] Table 2

[0097] The process parameters used in the embodiment of the present invention are relatively optimized welding process parameters summarized after multiple welding tests. During use, the welding process parameters can be adjusted accordingly according to the diameter of the pipe to be welded, the wall thickness, the fusion of the arc on both sides of the groove, etc.

[0098] The welded parts of the cladding composite pipe 100 and the cladding composite flange 200 welded by the welding process of the FPSO riser system of the embodiment of the present invention are subjected to mechanical property tests, visual, penetration and radiographic non-destructive tests. Specifically, a tensile test is carried out in accordance with the welding and brazing assessment standard ASME BPVC IX 2021. The specimen breaks at the position of the API 5L X65QS parent material, and the tensile strength exceeds 660Mpa, meeting the technical requirements.

[0099] The bending test was carried out in accordance with the welding and brazing assessment standard ASME BPVC IX 2021, and no defects were found in the specimen after bending.

[0100] According to the mechanical property evaluation standard ASTM A370 for metal materials, low-temperature impact tests were carried out on the weld center and the heat-affected zone of API 5LX65QS and AISI 4130 75K at -46°C, and the impact energy all met the technical requirements.

[0101] In accordance with the welding and brazing assessment standard ASME BPVC IX 2021 and the pressure vessel construction rules ASME BPVCVIII 2021, visual, penetration and radiographic non-destructive testing were carried out on it, and no defects were found.

[0102] According to the test method for macroscopic corrosion of metals and alloys ASTM E340, a macroscopic metallographic examination was performed on the weld area of ​​the cladding composite pipe 100 and the cladding composite flange 200, and no defects such as cracks, pores, slag inclusions, and lack of fusion were found.

[0103] The weld area of ​​the cladding composite pipe 100 and the cladding composite flange 200 was micro-metallographically examined in accordance with ASTM E407, the standard operating specification for micro-etching of metals and alloys, and no precipitates and intermetallic phases were found, and no micro-cracks were found at the fusion line.

[0104] According to the standard test method ASTM G28 for intergranular corrosion sensitivity detection of forged high nickel-chromium bearing alloys, intergranular corrosion was carried out on the weld areas of the cladding composite pipe 100 and the cladding composite flange 200. The samples were subjected to a 120-hour boiling test in a ferrous sulfate-sulfuric acid solution, and the corrosion rate of the samples was 0.80 mm / Y, which met the technical requirements.

[0105] According to the standard test method for chemical analysis of steel products ASTM A751, the composition of the inner wall of the weld of the cladding composite pipe and the cladding composite flange was checked, and the Fe element content was 0.17%, which met the technical requirements.

[0106] The above embodiments are merely exemplary descriptions of the structures. The structures in the embodiments are not fixed combination structures. In the absence of structural conflicts, the structures in multiple embodiments can be used in any combination.

[0107] Although the present invention has been described with reference to several typical embodiments, it should be understood that the terms used are illustrative and exemplary, rather than restrictive. Since the present invention can be embodied in a variety of forms without departing from the spirit or essence of the invention, it should be understood that the above embodiments are not limited to any of the foregoing details, but should be interpreted broadly within the spirit and scope defined by the appended claims, so all changes and modifications falling within the scope of the claims or their equivalents should be covered by the appended claims.

Claims

1. A welding process for an FPSO riser system, for welding an FPSO riser system, wherein the FPSO riser system comprises a cladding composite pipe and a cladding composite flange; It is characterized in that The welding process includes: Performing groove processing on the cladding composite pipe and the cladding composite flange according to a preset groove size; Assembling the groove end of the cladding composite pipe and the groove end of the cladding composite flange; Preheating the groove area formed by the cladding composite pipe and the cladding composite flange assembly; Welding the preheated cladding composite pipe and the cladding composite flange; The welding sequence is as follows: firstly, manual tungsten inert gas welding is used to perform the base welding between the cladding composite pipe and the cladding composite flange; then, manual tungsten inert gas welding is used to perform the thermal welding between the cladding composite pipe and the cladding composite flange; then, automatic tungsten inert gas welding is used to perform the filling welding between the cladding composite pipe and the cladding composite flange; finally, automatic tungsten inert gas welding is used to perform the cover welding between the cladding composite pipe and the cladding composite flange; After welding is completed, post-weld heat treatment is carried out immediately.

2. The welding process of the FPSO riser system according to claim 1, It is characterized in that In the step of preheating the groove area formed by the cladding composite pipe and the cladding composite flange assembly, the preheating temperature is 120°C to 150°C.

3. The welding process of the FPSO riser system according to claim 1, It is characterized in that The process parameters of the base welding include: welding current 90A-110A, welding voltage 9.5V-11V, welding speed 50mm / min-70mm / min, and interlayer temperature 130°C-160°C.

4. The welding process of the FPSO riser system according to claim 1, It is characterized in that The process parameters of the thermal welding include: welding current 110A-130A, welding voltage 10V-13V, welding speed 70mm / min-90mm / min, and interlayer temperature 130°C-160°C.

5. The welding process of the FPSO riser system according to claim 1, It is characterized in that The process parameters of the filling welding include: peak current 230A~250A, base current 160A~180A, pulse frequency 2.5HZ, welding voltage 11V~13V, welding speed 160mm / min~180mm / min, wire feeding speed 1200mm / min~1300mm / min, and interlayer temperature 135℃~175℃.

6. The welding process of the FPSO riser system according to claim 1, It is characterized in that The process parameters of the cap welding include: welding current 220A-240A, welding voltage 11V-13V, welding speed 150mm / min-170mm / min, wire feeding speed 1100mm / min-1200mm / min, and interlayer temperature 135°C-165°C.

7. The welding process of the FPSO riser system according to claim 1, It is characterized in that The number of weld passes of the filling welding is multiple, and when the filling welding is performed by automatic tungsten inert gas welding, the multiple weld passes are sequentially stacked from the cladding composite pipe toward the cladding composite flange, and sequentially stacked from the inner wall of the pipe toward the outer wall of the pipe; The number of weld passes for the cap welding is multiple. When the cap welding is performed by automatic tungsten inert gas welding, multiple weld passes are sequentially superimposed from the cladding composite pipe toward the cladding composite flange.

8. The welding process of the FPSO riser system according to claim 1, It is characterized in that After welding is completed, the post-weld heat treatment step is immediately carried out. The heat treatment temperature is 610℃~630℃, and the insulation time is not less than 1.25h.

9. The welding process of the FPSO riser system according to claim 1, It is characterized in that The groove of the cladding composite pipe and the groove of the cladding composite flange respectively include a first groove, a second groove and a blunt edge, the first groove, the second groove and the blunt edge are arranged in sequence from the outer wall of the pipe to the inner wall of the pipe, the groove angle of the first groove is 7.5° to 12.5°, the groove angle of the second groove is 35° to 40°, and the thickness of the blunt edge is 1mm to 2mm.

10. The welding process of the FPSO riser system according to claim 1, It is characterized in that In the step of assembling the groove end of the cladding composite pipe and the groove end of the cladding composite flange, the gap between the blunt edge of the cladding composite pipe and the blunt edge of the cladding composite flange is 4 mm to 5 mm, and the error is ≤1 mm.

11. The welding process of the FPSO riser system according to claim 1, It is characterized in that After the step of performing groove processing on the cladding composite pipe and the cladding composite flange according to the preset groove size, the method further includes: The grooves and surrounding areas of the cladding composite pipe and the cladding composite flange are pre-cleaned before welding to clean the oil, dirt, paint and rust on the grooves and surrounding areas.

12. The welding process of the FPSO riser system according to claim 1, It is characterized in that Before the step of preheating the groove area formed by the cladding composite pipe and the cladding composite flange assembly, the method further includes: The groove area formed by the cladding composite pipe and the cladding composite flange assembly is protected by back argon gas.