Preparation method, product and application of boron carbide aerogel
The preparation of boron carbide aerogels by one-step method solves the complex process problems in the existing technology, achieves high compression strength and low thermal conductivity, and expands the application range of aerogels.
Patent Information
- Application Number
- CN202411078984.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-11-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The preparation method and process steps of boron carbide aerogel in the prior art are complex, and it is difficult to achieve a simple one-step preparation, which limits its application in high temperature environments.
By using a one-step method, the organic boric acid was dissolved in a mixed solvent and added a catalyst. After aging treatment, drying and pyrolysis reaction, boron carbide aerogel was successfully prepared. The method includes dissolving organic boric acid in a mixed solvent and adding a catalyst to form a B-C precursor sol, forming a wet gel after aging, forming an aerogel after drying, and performing carbon thermal reduction through a pyrolysis reaction to obtain boron carbide aerosol aerosol glue.
The process steps are simplified, and the obtained boron carbide aerogel has high compression strength, low density, low thermal conductivity and stable chemical properties, expanding the application space of aerogels.
Smart Images

Figure CN118993077A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of porous aerogel thermal insulation material preparation, and in particular to a preparation method, product and application of boron carbide aerogel. Background Art
[0002] Boron carbide has the advantages of low theoretical density, high melting point, high strength, excellent thermoelectric performance, stable high temperature and chemical properties, etc. It is widely used in the military field to prepare light armor, bulletproof vests, etc., and is also used as an important high temperature resistant material in the aerospace field. Aerogel is a nanoporous material with a three-dimensional network structure, light weight and heat insulation. Due to its porous nature, the mechanical strength of aerogel is not very ideal, and the skeleton is prone to collapse and destruction under high temperature conditions, which in turn affects its application in high temperature environments.
[0003] Taking advantage of the superior high temperature resistance and high strength of boron carbide, a method for preparing boron carbide aerogel is developed to expand the research scope of carbide aerogel and expand the application space of aerogel, which is of great significance to the technical field of porous aerogel thermal insulation material preparation. At present, the preparation method of boron carbide aerogel in the prior art has the problem of complex process steps (using a two-step method or even a more complex process). Therefore, providing a one-step method for preparing boron carbide aerogel with simple process steps is a technical problem that technicians in this field need to solve urgently. Summary of the invention
[0004] Based on the above content, the present invention provides a preparation method, product and application of boron carbide aerogel. The present invention successfully prepares boron carbide aerogel by a one-step method, and the process steps are simple.
[0005] To achieve the above object, the present invention provides the following solutions:
[0006] One of the technical solutions of the present invention is a method for preparing boron carbide aerogel, comprising the following steps:
[0007] Dissolving organic boronic acid in a mixed solvent, adding a catalyst, and obtaining a BC precursor sol;
[0008] After subjecting the BC precursor sol to an aging treatment, a BC precursor wet gel is obtained;
[0009] Drying the BC precursor wet gel to obtain a BC precursor aerogel;
[0010] The BC precursor aerogel is pyrolyzed and then subjected to a carbide thermal reduction reaction to obtain the boron carbide aerogel.
[0011] A second technical solution of the present invention is a boron carbide aerogel prepared according to the above-mentioned preparation method.
[0012] A third technical solution of the present invention is the application of the above-mentioned boron carbide aerogel in the field of aerospace.
[0013] The present invention discloses the following technical effects:
[0014] The method of the invention has a simple operation process and strong reproducibility. Organic boric acid is used as a raw material, a BC precursor gel is obtained through a sol-gel reaction, and a complete and crack-free block B4C aerogel is obtained through normal pressure drying and carbon thermal reduction reaction.
[0015] The boron carbide aerogel prepared by the method of the present invention has a density of 0.22-0.30 g / cm 3 , thermal conductivity 0.04 ~ 0.07W / (m K), high compression strength, and has the same characteristics as traditional aerogels: low density, low thermal conductivity, while also having the characteristics of stable chemical properties, excellent mechanical properties, etc. As a new type of carbide aerogel, it expands the research scope of carbide aerogels and expands the application space of aerogels. Compared with the prior art, the present invention has significant progress and application value. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0017] Figure 1 This is a physical photo of the boron carbide (B4C) aerogel prepared in Example 1. DETAILED DESCRIPTION
[0018] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0019] It should be understood that the terms described in the present invention are only for describing a particular embodiment and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0020] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0021] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to the skilled artisan. The present invention description and examples are exemplary only.
[0022] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0023] The invention provides a method for preparing boron carbide aerogel by using an organic boric acid sol-gel method; the method has a simple process, and the prepared boron carbide aerogel has excellent performance and good thermal insulation performance and mechanical strength.
[0024] The first aspect of the present invention provides a method for preparing a boron carbide aerogel, comprising the following steps:
[0025] Dissolving organic boronic acid in a mixed solvent, adding a catalyst, and obtaining a BC precursor sol;
[0026] After subjecting the BC precursor sol to an aging treatment, a BC precursor wet gel is obtained;
[0027] Drying the BC precursor wet gel to obtain a BC precursor aerogel;
[0028] The BC precursor aerogel is pyrolyzed and then subjected to a carbide thermal reduction reaction to obtain the boron carbide aerogel.
[0029] In some embodiments of the present invention, the organic boronic acid is at least one of 4,4-azodiphenylboronic acid, sec-butylboric acid, and n-propaneboric acid; and the concentration of the organic boronic acid in the mixed solvent is 0.5 to 2 mol / L.
[0030] The reasons why the concentration of the organic boronic acid is limited to the above parameters in the present invention are as follows: if the concentration of the organic boronic acid is too low, the formed network structure is loose, a large number of macropores exist in the system, and after drying, the mechanical strength of the obtained boron carbide aerogel is low, and even the skeleton collapses after drying; if the concentration of the organic boronic acid is too high, the concentration of the precursor undergoing condensation polymerization per unit volume is too high, the condensation polymerization rate is too fast, and agglomeration is likely to occur, resulting in uneven stress distribution inside the aerogel, and cracking is likely to occur after supercritical drying.
[0031] In some embodiments of the present invention, the catalyst is at least one of citric acid, acetic acid and oxalic acid; the amount of the catalyst added is such that the pH of the mixed system is 2-3.
[0032] In the present invention, the catalyst plays a complexing role, and an organic acid is selected as a complexing agent to form a complex with boric acid. When the relative molecular mass increases, the solubility will decrease, thus forming a sol, i.e., micelles. The sol will further polymerize to form a gel.
[0033] In the present invention, an organic acid is used as a catalyst. If the amount of the catalyst added is too much, the rate of complex formation is too fast, resulting in too fast gelation speed of the system, serious agglomeration, uneven internal stress distribution, cracking of the sample after supercritical drying, and a significant decrease in thermal insulation performance; if the amount of the catalyst added is too little, the cross-linking reaction is insufficient to fully proceed, the gel skeleton is fragile, and the mechanical strength of the sample after supercritical drying is not ideal or even skeleton collapse occurs. Therefore, the preferred amount of the catalyst added in the present invention is limited to a pH of 2 to 3 for the mixed system.
[0034] In some embodiments of the present invention, the step of stirring at 30 to 70° C. for 30 to 60 min after adding the catalyst is further included. More preferably, stirring at 40 to 70° C. for 30 to 60 min.
[0035] In some embodiments of the present invention, the mixed solvent is a mixture of ethanol and water in a volume ratio of 2 to 8:1.
[0036] The reason why the ratio of ethanol to water is limited to the above parameter range in the present invention is as follows: deionized water and ethanol can be mutually soluble in any ratio, and boric acid is easily soluble in water but difficult to dissolve in alcohol. In order to improve the solubility of organic boronic acid, the solvent is selected as a mixed solution of ethanol and deionized water. If the amount of water added is insufficient, it is difficult for organic boronic acid to dissolve in the solvent; if the proportion of water is too large, the strength of the aerogel obtained will gradually decrease.
[0037] In some embodiments of the present invention, the aging treatment is carried out at a temperature of 50 to 100° C. and for a time of 10 to 72 hours.
[0038] In the present invention, aging is to allow the functional groups on the gel skeleton to undergo further cross-linking, which plays a structural strengthening role on the gel skeleton. If the aging time is insufficient, the reaction is insufficient, and it is easy for the reaction to continue during the supercritical process due to the increase in temperature, resulting in sample deformation and even skeleton collapse; if the aging time is too long, the gel particles will fully grow during the aging process, the particle size will be too large, and the efficiency of solid-phase heat conduction will increase, which is not conducive to improving the thermal insulation performance of the aerogel.
[0039] In some embodiments of the present invention, the drying method is ethanol supercritical drying.
[0040] In some embodiments of the present invention, the pyrolysis temperature is 600-1000° C. and the time is 1-5 hours.
[0041] The pyrolysis process is to heat up in a vacuum or inert atmosphere to convert the organic components in the aerogel into carbon, also known as carbonization reaction, which usually occurs at a temperature of 600°C or above. The present invention selects 600-1000°C as the pyrolysis temperature range because within this range, the organic components in the sample can be completely pyrolyzed without carbon thermal reduction reaction.
[0042] In some embodiments of the present invention, the carbon thermal reduction reaction is specifically carried out at 1200-1700° C. for 1-5 hours under an inert atmosphere or vacuum conditions.
[0043] The present invention does not impose any particular limitation on the heating rate of the carbon thermal reduction reaction, and the conventional heating rate of 3-10° C. / min in the art may be adopted.
[0044] The reactants of the carbothermal reduction reaction are carbon and oxides, so the precursor aerogel must first be converted into carbon-boron oxide aerogel through a pyrolysis reaction, and then the temperature is raised to a temperature at which carbothermal reduction can occur, and carbon and boron oxide react to form boron carbide aerogel. Therefore, pyrolysis must be performed first, and after reaching the pyrolysis temperature, it must be maintained for a period of time to complete the pyrolysis and provide reactants for the subsequent carbothermal reduction.
[0045] A second aspect of the present invention provides a boron carbide aerogel prepared according to the above preparation method.
[0046] A third aspect of the present invention provides an application of the boron carbide aerogel in the field of aerospace.
[0047] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0048] Example 1
[0049] A method for preparing boron carbide aerogel by an organic boric acid sol-gel method, the steps are as follows:
[0050] Dissolve 4,4-azodiphenylboronic acid in a mixed solution of ethanol and deionized water (the volume ratio of ethanol to deionized water is 3:1), wherein the concentration of 4,4-azodiphenylboronic acid is 2 mol / L. Stir until a transparent and uniform solution is obtained, add citric acid, adjust the pH of the solution to 2-3, then stir at 65°C for 45 minutes, and age the obtained BC precursor sol in a 95°C oven for 48 hours to obtain a BC precursor wet gel; then supercritically dry it with ethanol to obtain a BC precursor aerogel. The prepared BC precursor aerogel is pyrolyzed at 700°C for 2 hours to obtain a black block aerogel, which is then heated to 1700°C at a heating rate of 5°C / min in a vacuum atmosphere and maintained for 3 hours to cause a carbon thermal reduction reaction to obtain a boron carbide aerogel (the actual photo is shown in the figure). Figure 1 As shown by Figure 1 It can be seen that the boron carbide aerogel prepared in this embodiment is a complete block).
[0051] The density of the boron carbide aerogel prepared in this embodiment is 0.30 g / cm 3 , thermal conductivity 0.063W / (m·K), compressive strength 2.25MPa.
[0052] Example 2
[0053] A method for preparing boron carbide aerogel by an organic boric acid sol-gel method, the steps are as follows:
[0054] The sec-butyl boric acid was dissolved in a mixed solution of ethanol and deionized water (the volume ratio of ethanol to deionized water was 3:1), wherein the concentration of the sec-butyl boric acid was 2 mol / L. Stirring to obtain a transparent and uniform solution, adding citric acid, adjusting the pH of the solution to 2-3, then stirring at 65°C for 45 minutes, and aging the obtained BC precursor sol in a 95°C oven for 48 hours to obtain a BC precursor wet gel; then supercritical drying of ethanol was performed to obtain a BC precursor aerogel. The obtained BC precursor aerogel was pyrolyzed at 700°C for 2 hours to obtain a black block aerogel, and then heated to 1700°C at a heating rate of 5°C / min in a vacuum atmosphere and maintained for 3 hours, and a carbon thermal reduction reaction occurred to obtain a boron carbide aerogel.
[0055] The density of the boron carbide aerogel prepared in this embodiment is 0.23 g / cm 3 , thermal conductivity 0.048W / (m·K), compressive strength 1.21MPa.
[0056] Example 3
[0057] A method for preparing boron carbide aerogel by an organic boric acid sol-gel method, the steps are as follows:
[0058] Dissolve n-propyboric acid in a mixed solution of ethanol and deionized water (the volume ratio of ethanol to deionized water is 3:1), wherein the concentration of n-propyboric acid is 2 mol / L. Stir until a transparent and uniform solution is obtained, add citric acid, adjust the pH of the solution to 2-3, then stir at 65°C for 45 minutes, and age the obtained BC precursor sol in a 95°C oven for 48 hours to obtain a BC precursor wet gel; then supercritically dry it with ethanol to obtain a BC precursor aerogel. The obtained BC precursor aerogel is pyrolyzed at 700°C for 2 hours to obtain a black block aerogel, and then heated to 1700°C at a heating rate of 5°C / min in a vacuum atmosphere and maintained for 3 hours, and a carbon thermal reduction reaction occurs to obtain a boron carbide aerogel.
[0059] The density of the boron carbide aerogel prepared in this embodiment is 0.27 g / cm 3 , thermal conductivity 0.052W / (m·K), compressive strength 1.30MPa.
[0060] Example 4
[0061] A method for preparing boron carbide aerogel by an organic boric acid sol-gel method, the steps are as follows:
[0062] 4,4-azodiphenylboronic acid was dissolved in a mixed solution of ethanol and deionized water (the volume ratio of ethanol to deionized water was 3:1), wherein the concentration of 4,4-azodiphenylboronic acid was 0.5 mol / L. Stirring to obtain a transparent and uniform solution, adding oxalic acid, adjusting the pH of the solution to 2-3, then stirring at 40°C for 50 min, and aging the obtained BC precursor sol in a 50°C oven for 72 h to obtain a BC precursor wet gel; then supercritical drying of ethanol was performed to obtain a BC precursor aerogel. The obtained BC precursor aerogel was pyrolyzed at 600°C for 2 h to obtain a black block aerogel, and then heated to 1200°C at a heating rate of 5°C / min in a vacuum atmosphere and maintained for 3 h, a carbon thermal reduction reaction occurred, and a boron carbide aerogel was obtained.
[0063] The density of the boron carbide aerogel prepared in this embodiment is 0.22 g / cm 3 , thermal conductivity 0.043W / (m·K), compressive strength 1.35MPa.
[0064] Example 5
[0065] A method for preparing boron carbide aerogel by an organic boric acid sol-gel method, the steps are as follows:
[0066] Sec-butyl boric acid was dissolved in a mixed solution of ethanol and deionized water (the volume ratio of ethanol to deionized water was 3:1), wherein the concentration of sec-butyl boric acid was 0.5 mol / L. Stirring to obtain a transparent and uniform solution, adding oxalic acid, adjusting the pH of the solution to 2-3, then stirring at 40°C for 50 min, and aging the obtained BC precursor sol in a 50°C oven for 72 h to obtain a BC precursor wet gel; then supercritical drying of ethanol was performed to obtain a BC precursor aerogel. The obtained BC precursor aerogel was pyrolyzed at 600°C for 2 h to obtain a black block aerogel, and then heated to 1200°C at a heating rate of 5°C / min in a vacuum atmosphere and maintained for 3 h, a carbon thermal reduction reaction occurred, and a boron carbide aerogel was obtained.
[0067] The density of the boron carbide aerogel prepared in this embodiment is 0.23 g / cm 3 , thermal conductivity 0.049W / (m·K), compressive strength 1.19MPa.
[0068] Example 6
[0069] A method for preparing boron carbide aerogel by an organic boric acid sol-gel method, the steps are as follows:
[0070] Dissolve n-propyl boric acid in a mixed solution of ethanol and deionized water (the volume ratio of ethanol to deionized water is 3:1), wherein the concentration of n-propyl boric acid is 1 mol / L. Stir until a transparent and uniform solution is obtained, add oxalic acid, adjust the pH of the solution to 2-3, then stir at 70°C for 30 minutes, age the obtained BC precursor sol in a 100°C oven for 10 hours to obtain a BC precursor wet gel; then supercritically dry it to obtain a BC precursor aerogel. The obtained BC precursor aerogel is pyrolyzed at 600°C for 2 hours to obtain a black block aerogel, and then heated to 1500°C at a heating rate of 5°C / min in a vacuum atmosphere and maintained for 3 hours, a carbon thermal reduction reaction occurs, and a boron carbide aerogel is obtained.
[0071] The density of the boron carbide aerogel prepared in this embodiment is 0.24 g / cm 3 , thermal conductivity 0.041W / (m·K), compressive strength 1.16MPa.
[0072] Comparative Example 1
[0073] A two-step method for preparing boron carbide aerogel, the steps are as follows:
[0074] Mix 1 mol of resorcinol, 2 mol of formaldehyde and 8.5 mol of anhydrous ethanol and stir to obtain solution A. Ultrasonic disperse 0.5 mol of boric acid, 0.005 mol of anhydrous sodium carbonate, 10 mol of deionized water and 4.25 mol of anhydrous ethanol, heat and stir at 40°C to obtain solution B. Mix solution B with solution A, add 0.5 mol of anhydrous citric acid and stir to obtain a sol solution. Pour into a mold, let stand for 30 minutes, put it in a 40°C oven for aging for 5 hours, add anhydrous ethanol for solvent replacement, replace it every 8 hours, and replace it 4 times in total. The replaced wet gel is subjected to CO2 supercritical drying treatment, where the kettle pressure is controlled at 12MPa, the temperature is controlled at 50°C, and the drying time is 8 hours to obtain a boron carbide precursor. The obtained boron carbide precursor was heated to 1350°C at a heating rate of 3°C / min under the protection of an argon atmosphere, and the heat preservation time was 5 hours. Then the temperature was reduced to 600°C, the argon was replaced with air, and the heat preservation was continued for 3 hours for decarbonization. After cooling to room temperature, boron carbide aerogel was obtained.
[0075] Although the boron carbide aerogel prepared in this embodiment is a block, it cracks in the middle and a complete block boron carbide aerogel cannot be obtained. This may be because: the comparative document uses a two-step method to prepare boron carbide aerogel, preparing carbon source and boron source sols respectively. The carbon source sol is weakly alkaline and the boron source sol is acidic. The two-component sol will undergo phase separation, which is one of the reasons for the aerogel cracking. In addition, too low aging temperature is also one of the reasons for the cracking of aerogel: the gel particles carry functional groups on their surface, which will further react during the aging process and play a role in strengthening the gel skeleton. If the aging temperature is too low, the strength of the gel skeleton is insufficient and it is easy to crack.
[0076] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.
Claims
1. A method for preparing boron carbide aerogel, characterized in that: The following steps are involved: Dissolving organic boronic acid in a mixed solvent, adding a catalyst, and obtaining a BC precursor sol; After subjecting the BC precursor sol to an aging treatment, a BC precursor wet gel is obtained; Drying the BC precursor wet gel to obtain a BC precursor aerogel; The BC precursor aerogel is pyrolyzed and then subjected to a carbide thermal reduction reaction to obtain the boron carbide aerogel.
2. The method for preparing boron carbide aerogel according to claim 1, characterized in that: The organic boronic acid is at least one of 4,4-azodiphenylboronic acid, sec-butylboric acid and n-propaneboric acid; and the concentration of the organic boronic acid in the mixed solvent is 0.5-2 mol / L.
3. The method for preparing boron carbide aerogel according to claim 1, characterized in that: The catalyst is at least one of citric acid, acetic acid and oxalic acid; the amount of the catalyst added is such that the pH of the mixed system is 2-3.
4. The method for preparing boron carbide aerogel according to claim 1, characterized in that: The mixed solvent is a mixture of ethanol and water in a volume ratio of 2 to 8:
1.
5. The method for preparing boron carbide aerogel according to claim 1, characterized in that: The temperature of the aging treatment is 50-100° C., and the time is 10-72 hours.
6. The method for preparing boron carbide aerogel according to claim 1, characterized in that: The drying method is ethanol supercritical drying.
7. The method for preparing boron carbide aerogel according to claim 1, characterized in that: The pyrolysis temperature is 600-1000° C. and the time is 1-5 hours.
8. The method for preparing boron carbide aerogel according to claim 1, characterized in that: The carbon thermal reduction reaction is specifically: keeping the temperature at 1200-1700° C. for 1-5 hours under an inert atmosphere or vacuum conditions.
9. A boron carbide aerogel prepared according to the preparation method according to any one of claims 1 to 8.
10. Use of the boron carbide aerogel according to claim 9 in the field of aerospace.