Ammonium carnallite dehydration method
Through the three-stage dehydration process, the moisture in ammonium halide is gradually removed, and the temperature and mass ratio are controlled, which solves the problems of high energy consumption and unstable product in the existing methods, and achieves low energy consumption and high efficiency ammonium halide dehydration. , suitable for industrial production.
Patent Information
- Application Number
- CN202411125876.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-22
AI Technical Summary
The existing ammonium halide dehydration method has the problems of large ammonium chloride consumption, high energy consumption and long operating cycles, especially in high-temperature one-time dehydration method, which leads to industrial production costs and efficiency challenges.
The three-stage dehydration process is adopted to gradually remove free water and crystallized water by controlling the temperature and mass ratio, reducing energy consumption, ensuring product stability and particle size, and preventing moisture adsorption.
It effectively reduces the energy consumption of ammonium halide dehydration, ensures the stability and particle size of the product, is suitable as a raw material for fluidized beds, reduces the risk of moisture adsorption, and improves the efficiency and cost-effectiveness of industrial production.
Smart Images

Figure BDA0004996396580000031
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of ammonium carnallite dehydration, and particularly relates to an ammonium carnallite dehydration method. Background Art
[0002] Ammonium carnallites are the intermediate raw materials for the preparation of anhydrous magnesium chloride, which can be used for the electrolytic preparation of magnesium metal. The main process route is to use magnesium chloride and ammonium chloride, which are byproducts of salt lakes, as raw materials to prepare ammonium carnallites. The ammonium carnallites are dehydrated to obtain anhydrous magnesium chloride, which is used as the raw material for the electrolytic preparation of magnesium metal.
[0003] In the existing technology, the dehydration method of ammonium carnallite mainly includes dehydration under nitrogen protection, high-temperature one-time dehydration method, etc. For example, Zhou Ningbo et al. described in detail in "Preparation of Anhydrous Magnesium Chloride by Gas-Solid Reaction of Hydrochloric Acid from Hydrochloric Acid from Salt Lake Hydrochloric Acid at 135°C for 2h under nitrogen protection to prepare low-hydrated hydrochloric acid bismuth (MgCl2·nH2O, n=1.6). However, the main problem with this method is that the consumption of ammonium chloride is large, because the dehydration reaction of ammonium carnallite is a complex thermodynamic equilibrium process, and excessive ammonium chloride is required to promote the reaction to the right to improve the dehydration efficiency. In addition, the energy consumption of the dehydration process under nitrogen protection is relatively high, and the operation cycle is long, which poses challenges to the cost and efficiency of industrial production. In addition, the high-temperature one-time dehydration method is usually carried out at a higher temperature of more than 200°C. Although this method can complete the dehydration process of ammonium carnallite at one time, and the dehydration speed is fast, the operation cycle is short, and it is suitable for large-scale industrial production, but the higher temperature demand brings higher energy consumption. Summary of the invention
[0004] In order to solve all or part of the above technical problems, the present invention provides the following technical solutions:
[0005] One of the objects of the present invention is to provide a method for dehydrating ammonium carnallites, the method comprising:
[0006] Performing a first-stage dehydration on the highly hydrated ammonium carnallites to remove at least a portion of free water in the highly hydrated ammonium carnallites to obtain first ammonium carnallites;
[0007] subjecting the first ammonium carnallites to a second stage of dehydration to remove a portion of crystal water in the first ammonium carnallites to obtain second ammonium carnallites;
[0008] The second ammonium carnallites and the first ammonium carnallites are mixed in a mass ratio of 1:8-10 to form a mixture, and the mixture is subjected to a third stage of dehydration to obtain low-hydrated ammonium carnallites.
[0009] The invention provides a three-stage ammonium carnallite dehydration process, which can reduce the energy consumption of ammonium carnallite dehydration by controlling the dehydration temperature of the three stages; and the second stage dehydration product (i.e., the second ammonium carnallite) and the first stage dehydration raw material (i.e., the first ammonium carnallite) are mixed according to a certain mass ratio and then the third stage dehydration is carried out, so that the stability of the third stage dehydration raw material can be ensured and free water can be prevented from being adsorbed again.
[0010] Furthermore, within the mass ratio range of 1:8 to 10 of the second ammonium carnallite to the first ammonium carnallite, not only can the dehydration process be more stable, but also the generated product has a suitable particle size, and the proportion of powdered products is low, so that the generated low-hydrated ammonium carnallite can be directly used as a fluidized bed raw material, and the generated product has a lower porosity, so it is not easy to adsorb free water during the transfer process.
[0011] In addition, the research results on the dehydration mechanism of ammonium carnallite showed that the binding energy of highly hydrated ammonium carnallite to the first four crystal waters is 0.86eV, the binding energy to the fifth crystal water is 1.17eV, and the binding energy to the sixth crystal water is 1.40eV. This result shows that the staged dehydration technology of highly hydrated ammonium carnallite is reliable and feasible.
[0012] In some embodiments, the crystal water content of the highly hydrated ammonium carnallite of the present invention is 45.1-45.7 wt %.
[0013] In some embodiments, the temperature of the first stage of dehydration is sufficient to remove free water from the highly hydrated ammonium carnallite but not the crystal water therein.
[0014] In some embodiments, the temperature of the first stage dehydration is 30-50°C.
[0015] In some embodiments, the first stage of dehydration lasts for 1 to 2 hours.
[0016] In some embodiments, the second ammonium carnallite obtained by the second stage of dehydration has a crystal water content of 28.0-28.8 wt %.
[0017] In some embodiments, the temperature of the second stage dehydration is 90-170°C.
[0018] In some embodiments, the second stage of dehydration lasts for 2 to 4 hours.
[0019] In some embodiments, the crystal water content of the low-hydrated ammonium carnallite obtained by the third stage of dehydration is 3.52-7.03 wt %.
[0020] In some embodiments, the temperature of the third stage dehydration is 175-199°C.
[0021] In some embodiments, the third stage dehydration time is 1 to 2 hours.
[0022] In some embodiments, the heating rate of the second stage dehydration and the third stage dehydration is 15° C. / min to 25° C. / min.
[0023] In some embodiments, before dehydration, the average particle size of the highly hydrated ammonium carnallite is controlled at 300-400 μm. Controlling the relatively uniform average particle size of the highly hydrated ammonium carnallite is beneficial to the stability of process operation, product batch stability, and energy saving and consumption reduction.
[0024] The second object of the present invention is to provide low-hydrated ammonium carnallites obtained by the ammonium carnallites dehydration method according to any one of the technical solutions.
[0025] Compared with the prior art, the present invention has at least the following beneficial effects: the present invention provides a three-stage ammonium carnallite dehydration process, in which at least part of the free water is removed in the first stage, and part of the crystal water is removed in the second and third stages to obtain low-hydrated ammonium carnallite, and the dehydration method can reduce the energy consumption of ammonium carnallite dehydration by controlling the dehydration temperature of the three stages; the dehydration method provided by the present invention mixes the second-stage dehydration product (i.e., the second ammonium carnallite) and the first-stage dehydration raw material (i.e., the first ammonium carnallite) in a certain mass ratio and then performs the third-stage dehydration, which can ensure the stability of the third-stage dehydration raw material and prevent it from adsorbing free water again. DETAILED DESCRIPTION
[0026] The technical solution of the present invention is described in detail below in conjunction with specific embodiments so that those skilled in the art can better understand and implement the technical solution of the present invention. The specific functional details disclosed herein should not be interpreted as limiting, but only as the basis for the claims and as a representative basis for teaching those skilled in the art to adopt the present invention in different ways in any appropriate detailed embodiment.
[0027] In the specific implementation manner of the present invention, unless otherwise specified, the percentages (%) are all mass percentages.
[0028] Example 1
[0029] This embodiment provides a method for dehydrating ammonium carnallite. The raw material to be dehydrated is ammonium carnallite MgCl2·NH4CI·6H2O (denoted as S1), and its chemical composition is shown in Table 1:
[0030] Table 1 Chemical composition of ammonium carnallite ore used in this embodiment
[0031]
[0032] The above-mentioned ammonium carnallite raw material is subjected to three-stage dehydration, which is specifically as follows:
[0033] (1) First stage dehydration: 1000 g of S1 was weighed and placed in a dryer. The first dehydration temperature was set to 30° C. After reaching the first dehydration temperature, the temperature was kept for 2 h to obtain the mineral S2 after free water was removed. S2 was taken out, weighed and calculated to obtain: S2 weight 972 g, water content 42.2%;
[0034] (2) Second stage dehydration: 1000 g of S2 was weighed and placed in a muffle furnace. The second dehydration temperature was set to 90° C. The temperature was raised to 90° C. at a rate of 15° C. / min. After reaching the second dehydration temperature, the temperature was kept at 90° C. for 4 h to obtain S3. S3 was taken out, weighed, and calculated to obtain: the weight of S3 was 719 g, and the water content was 16.5%. S3 was ammonium carnallite MgCl2·NH4Cl·4H2O containing four crystal waters;
[0035] (3) The third stage of dehydration: S3 and S2 were mixed in a mass ratio of 1:8 to form a mixed raw material. A total of 700 g of the mixed raw material was placed in a muffle furnace. The third dehydration temperature was set to 175°C. The temperature was increased to 175°C at a heating rate of 25°C / min. After reaching the third dehydration temperature, the temperature was kept for 2 h to obtain low-hydrated ammonium carnallite. The low-hydrated ammonium carnallite was then taken out, weighed, and calculated to obtain: the weight of the low-hydrated ammonium carnallite was 614 g, and the water content was 5.7%, which was ammonium carnallite MgCl2·NH4Cl·0.5H2O containing 0.5 crystal waters.
[0036] The energy consumption of the dehydration method of this embodiment was calculated. The energy consumption of dehydrating 100 g of ammonium carnallite ore S1 to prepare MgCl2·NH4Cl·0.5H2O was 171 KJ / mol.
[0037] Example 2
[0038] The ammonium carnallite ore MgCl2·NH4C1·6H2O (S1) used in Example 2 is the same as that in Example 1, and the ammonium carnallite raw material is subjected to three-stage dehydration, specifically as follows:
[0039] (1) First stage dehydration: 1000 g of S1 was weighed and placed in a dryer. The first dehydration temperature was set to 50° C. After reaching the first dehydration temperature, the temperature was kept for 1 h to obtain the mineral S2 after free water was removed. S2 was taken out, weighed and calculated to obtain: the weight of S2 was 969 g and the water content was 42.0%;
[0040] (2) Second stage dehydration: 1000 g of S2 was weighed and placed in a muffle furnace. The second dehydration temperature was set to 170° C. The temperature was raised to 170° C. at a rate of 15° C. / min. After reaching the second dehydration temperature, the temperature was kept at that temperature for 2 h to obtain S3. S3 was taken out and weighed and calculated to obtain: the weight of S3 was 718 g, and the water content was 16.4%. S3 was ammonium carnallite MgCl2·NH4C1·4H2O containing four crystal waters;
[0041] (3) The third stage of dehydration: S3 and S2 were mixed in a mass ratio of 1:10 to form a mixed raw material. The mixed raw material (700 g in total) was placed in a muffle furnace. The third dehydration temperature was set to 195°C. The temperature was increased to 195°C at a heating rate of 20°C / min. After reaching the third dehydration temperature, the mixture was kept warm for 1 hour to obtain low-hydrated ammonium carnallite. The low-hydrated ammonium carnallite was then taken out, weighed, and calculated to obtain: the weight of the low-hydrated ammonium carnallite was 613 g, and the water content was 5.6%, which was ammonium carnallite MgCl2·NH4Cl·0.5H2O containing 0.5 crystal waters.
[0042] The energy consumption of the dehydration method of this embodiment was calculated. The energy consumption of dehydrating 100 g of ammonium carnallite ore S1 to prepare MgCl2·NH4Cl·0.5H2O was 170 KJ / mol.
[0043] Example 3
[0044] The ammonium carnallite ore MgCl2·NH4C1·6H2O (S1) used in Example 3 is the same as that in Example 1, and the ammonium carnallite raw material is subjected to three-stage dehydration, specifically as follows:
[0045] (1) First stage dehydration: 1000 g of S1 was weighed and placed in a dryer. The first dehydration temperature was set to 40° C. After reaching the first dehydration temperature, the temperature was kept for 1.5 h to obtain the mineral S2 after free water was removed. S2 was taken out, weighed and calculated to obtain: the weight of S2 was 970 g and the water content was 42.1%;
[0046] (2) Second stage dehydration: 1000 g of S2 was weighed and placed in a muffle furnace, and the second dehydration temperature was set to 170° C. The temperature was raised to 170° C. at a heating rate of 15° C. / min. After reaching the second dehydration temperature, the temperature was kept at that temperature for 3 h to obtain S3. S3 was taken out, weighed, and calculated. The weight of S3 was 720 g, and the water content was 16.5%. S3 was ammonium carnallite MgCl2·NH4Cl·4H2O containing four crystal waters;
[0047] (3) The third stage of dehydration: S3 and S2 were mixed in a mass ratio of 1:9 to form a mixed raw material. A total of 700 g of the mixed raw material was placed in a muffle furnace. The third dehydration temperature was set to 195°C. The temperature was increased to 190°C at a heating rate of 25°C / min. After reaching the third dehydration temperature, the temperature was kept for 1.5 hours to obtain low-hydrated ammonium carnallite. The low-hydrated ammonium carnallite was then taken out, weighed and calculated. The weight of the low-hydrated ammonium carnallite was 613 g, and the water content was 5.7%, which was ammonium carnallite MgCl2·NH4Cl·0.5H2O containing 0.5 crystal waters.
[0048] The energy consumption of the dehydration method of this embodiment is calculated. The energy consumption of dehydrating 100g of ammonium carnallite ore S1 to prepare MgCl2·NH4Cl·0.5H2O is 173KJ / mol.
[0049] Comparative Example 1
[0050] The difference between Comparative Example 1 and Example 1 is that Comparative Example 1 adopts a two-stage dehydration method, which is as follows:
[0051] The ammonium carnallite ore MgCl2·NH4Cl·6H2O (S1) used in Comparative Example 1 is the same as that in Example 1, and the ammonium carnallite raw material is subjected to two-stage dehydration, specifically as follows:
[0052] (1) First stage dehydration: 1000 g of S1 was weighed and placed in a dryer. The first dehydration temperature was set to 165°C. After reaching the first dehydration temperature, the temperature was kept for 3.0 h to obtain mineral S2. S2 was taken out, weighed and calculated to obtain: S2 weight 720 g, water content 14.1%;
[0053] (2) Second stage dehydration: 1000 g of S2 was weighed and placed in a muffle furnace. The second dehydration temperature was set to 200 °C. The temperature was raised to 200 °C at a rate of 18 °C / min and kept at 200 °C for 5 h to obtain low-hydrated ammonium carnallite. The low-hydrated ammonium carnallite was then taken out, weighed and calculated. The weight of the low-hydrated ammonium carnallite was 645 g and the water content was 7.6%, which was ammonium carnallite MgCl2·NH4Cl·H2O containing 1 crystal water.
[0054] The energy consumption of the dehydration method of this embodiment is calculated. The energy consumption of dehydrating 100g of ammonium carnallite ore S1 to prepare MgCl2·NH4Cl·H20 is 200KJ / mol.
[0055] Comparative Example 2
[0056] The ammonium carnallite ore MgCl2·NH4C1·6H2O (S1) used in Comparative Example 2 is the same as that in Example 1, and the ammonium carnallite raw material is subjected to three-stage dehydration, specifically as follows:
[0057] (1) First stage dehydration: 1000 g of S1 was weighed and placed in a dryer. The first dehydration temperature was set to 30° C. After reaching the first dehydration temperature, the temperature was kept for 2 h to obtain the mineral S2 after free water was removed. S2 was taken out, weighed and calculated to obtain: S2 weight 972 g, water content 42.2%;
[0058] (2) Second stage dehydration: 1000 g of S2 was weighed and placed in a muffle furnace. The second dehydration temperature was set to 90° C. The temperature was raised to 90° C. at a rate of 15° C. / min. After reaching the second dehydration temperature, the temperature was kept at 90° C. for 4 h to obtain S3. S3 was taken out, weighed, and calculated to obtain: the weight of S3 was 719 g, and the water content was 16.5%. S3 was ammonium carnallite MgCl2·NH4Cl·4H2O containing four crystal waters;
[0059] (3) Third stage dehydration: 700 g of S3 was placed in a muffle furnace, the third dehydration temperature was set to 175 °C, the temperature was raised to 175 °C at a rate of 25 °C / min, and the temperature was kept at that temperature for 2 h after reaching the third dehydration temperature. It was found that directly subjecting the product obtained from the second stage dehydration to the third stage dehydration would result in the sample being very easy to absorb moisture and having a small particle size, which was extremely unfavorable for the next electrolysis process.
[0060] Comparative Example 3
[0061] The only difference between Comparative Example 3 and Example 1 is that during the third stage of dehydration, S3 and S2 are mixed in a mass ratio of 1:4, and the rest is implemented in the same way as Example 1. It is found that compared with Example 1, the particle size of the product becomes smaller during the dehydration process, and the proportion of the powdered product increases, which increases the specific surface area, resulting in the particle size failing to meet the set requirements when used as a fluidized bed raw material in the later stage.
[0062] Comparative Example 4
[0063] The only difference between Comparative Example 4 and Example 1 is that during the third stage of dehydration, S3 and S2 are mixed in a mass ratio of 4:1, and the rest is implemented in the same manner as Example 1. It is found that compared with Example 1, the porosity of the product is increased. This result will lead to more stringent requirements for subsequent processes. The product must be quickly transferred to the next process link, otherwise the product will easily adsorb free water due to the increase in pore adsorption.
[0064] The various aspects, embodiments, features and examples of the present invention should be considered as illustrative in all aspects and are not intended to limit the present invention, the scope of the present invention is defined only by the claims. Other embodiments, modifications and uses will be apparent to those skilled in the art without departing from the spirit and scope of the claimed invention.
[0065] In addition, the inventors of this case also referred to the aforementioned embodiments and conducted experiments with other raw materials, process operations, and process conditions described in this specification, and obtained relatively ideal results.
[0066] Although the present invention has been described with reference to illustrative embodiments, it will be appreciated by those skilled in the art that various other changes, omissions and / or additions may be made without departing from the spirit and scope of the present invention and that the elements of the embodiments may be replaced by substantial equivalents. In addition, many modifications may be made without departing from the scope of the present invention to adapt specific circumstances or materials to the teachings of the present invention. Therefore, it is not intended herein to limit the present invention to the disclosed specific embodiments for performing the present invention, but it is intended that the present invention will include all embodiments within the scope of the appended claims. In addition, unless specifically stated, any use of the terms first, second, etc. does not indicate any order or importance, but rather uses the terms first, second, etc. to distinguish one element from another.
Claims
1. A method for dehydrating ammonium carnallite, characterized in that: include: Performing a first-stage dehydration on the highly hydrated ammonium carnallites to remove at least a portion of free water in the highly hydrated ammonium carnallites to obtain first ammonium carnallites; subjecting the first ammonium carnallites to a second stage of dehydration to remove a portion of crystal water in the first ammonium carnallites to obtain second ammonium carnallites; The second ammonium carnallites and the first ammonium carnallites are mixed in a mass ratio of 1:8-10 to form a mixture, and the mixture is subjected to a third stage of dehydration to obtain low-hydrated ammonium carnallites.
2. The ammonium carnallite dehydration method according to claim 1, wherein: The temperature of the first stage of dehydration is sufficient to remove free water from the highly hydrated ammonium carnallite but not remove the crystal water therein.
3. The ammonium carnallite dehydration method according to claim 1 or 2, characterized in that: The temperature of the first stage dehydration is 30-50° C.; and / or the time of the first stage dehydration is 1-2 hours.
4. The ammonium carnallite dehydration method according to claim 1, wherein: The crystal water content of the second ammonium carnallite obtained by the second stage of dehydration is 28.0-28.8 wt %.
5. The method for dehydrating ammonium carnallite according to claim 1 or 4, characterized in that: The temperature of the second stage dehydration is 90-170° C.; and / or the time of the second stage dehydration is 2-4 hours.
6. The ammonium carnallite dehydration method according to claim 1, wherein: The crystal water content of the low-hydrated ammonium carnallite obtained by dehydration in the third stage is 3.52-7.03 wt %.
7. The method for dehydrating ammonium carnallite according to claim 1 or 6, characterized in that: The dehydration temperature in the third stage is 175-199° C.; and / or, the dehydration time in the third stage is 1-2 hours.
8. The ammonium carnallite dehydration method according to claim 1, wherein: The heating rates of the second stage dehydration and the third stage dehydration are 15°C / min to 25°C / min.
9. The ammonium carnallite dehydration method according to claim 1, characterized in that: Before dehydration, the average particle size of the highly hydrated ammonium carnallite is controlled to be 300-400 μm.
10. Low-hydrated ammonium carnallites obtained by the ammonium carnallites dehydration method according to any one of claims 1 to 9.
Citation Information
Cited By
Low water ammonium carnallite and method for producing the same
CN123061981A