Silicate glass with high zirconium oxide content as well as preparation method and application of silicate glass
Through low alkali formula and oxidative atmosphere melting technology, silicate glass with high ZrO2 content was prepared, which solved the problems of poor melting uniformity and insufficient chemical stability in the prior art, and realized the preparation of glass with high zirconia content , has excellent chemical stability and mechanical properties, suitable for high temperature and high pressure and chemical corrosion resistance applications.
Patent Information
- Application Number
- CN202411130253.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-16
AI Technical Summary
The prior art is difficult to prepare silicate glass with a ZrO2 content greater than 5 wt.%, resulting in poor melting uniformity, easy crystallization, and difficulty in engineering preparation. The high boron oxide or high alkali metal content reduces the chemical stability of the glass and cannot meet the requirements. High-tech requirements for high temperature and high pressure resistance and chemical stability.
Using low-alkali formula, high-temperature calcination and dehydration treatment and oxidation atmosphere melting technology, the distribution ratio of nano-scale zirconium silicate powder and other oxide groups is optimized, and the OH-ion content in the glass is controlled to achieve a ZrO2 content of 15-19%. Preparation of silicate glass with high zirconia content.
A high zirconia content silicate glass with excellent chemical stability, suitable thermal expansion coefficient, high transition temperature and excellent mechanical properties has been obtained, which is suitable for high temperature and high pressure optical windows, optical glass and other applications.
Smart Images

Figure BDA0004997610040000021 
Figure BDA0004997610040000022 
Figure BDA0004997610040000031
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of special glass materials and preparation thereof, and in particular to silicate glass with high zirconium oxide content and a preparation method and application thereof. Background Art
[0002] Introducing a certain amount of ZrO2 into silicate glass can significantly improve the chemical stability and mechanical properties of the glass, such as acid resistance, alkali resistance, and water resistance. However, while introducing ZrO2 to improve the above properties of glass materials, it will bring many problems, such as increased glass melting temperature, increased glass viscosity at high temperature, which makes it difficult to remove bubbles, and increased glass crystallization tendency, which seriously affects the performance and quality of the glass. The content of ZrO2 in ordinary silicate glass is generally controlled below 5wt.%, which limits the use of ZrO2 in the glass. However, with the advancement of science and technology and the improvement of industrial level, the performance of glass with low ZrO2 content cannot meet the requirements of high-tech development, especially in optical glass with high temperature and pressure resistance and high chemical stability requirements, such as high temperature and pressure resistant window glass, sodium vapor resistant lampshade glass, etc. Therefore, it is urgent to develop silicate glass with high ZrO2 content.
[0003] In the prior art, the method for preparing silicate glass with a ZrO2 content greater than 5wt.% is mainly through increasing the glass melting temperature, prolonging the glass clarification time or using a high boron oxide or high alkali metal content method. However, in the above-mentioned glass with a ZrO2 content greater than 5wt.%, the glass melting viscosity is mainly reduced by high-content boron oxide fluxing or high-content alkali metal oxides destroying the glass network structure, and the ZrO2 content of the silicate glass prepared by these schemes is generally controlled at 5-10wt.%. However, high boron oxide or high alkali metal content will significantly reduce the chemical stability of the glass and is only suitable for low-viscosity glass melting. In silicate glass with a ZrO2 content ≥15wt.%, there are still problems such as poor glass melting uniformity, easy crystallization of the glass, and difficulty in engineering preparation. Summary of the invention
[0004] The purpose of the present invention is to overcome the shortcomings of the current prior art and provide a high zirconium oxide content silicate glass with a ZrO2 content greater than 15wt.%, excellent chemical stability and a suitable thermal expansion coefficient, a high glass transition temperature, excellent mechanical properties and the like, and a preparation method thereof.
[0005] The present invention also provides an application of silicate glass with a high zirconium oxide content. The silicate glass with a high zirconium oxide content has good chemical corrosion resistance and is suitable for high temperature and high pressure resistant optical windows, optical glass, window glass, pressure and temperature resistant optical containers, optoelectronic substrate glass, chemical industry observation windows, video or camera lenses, special glass fibers, etc.
[0006] In order to achieve the above object, the technical solution adopted by the present invention is:
[0007] A silicate glass with a high zirconium oxide content, comprising the following components in percentage by weight:
[0008]
[0009] Further, a silicate glass with a high zirconium oxide content is characterized in that it preferably includes the following components in percentage by weight:
[0010]
[0011]
[0012] A silicate glass with a high zirconium oxide content, characterized in that the silicate glass with a high zirconium oxide content substantially does not contain [OH] - Even if ions are present, they are brought in by impurities in the raw materials or preparation process. Strictly controlling the hydroxyl content in the glass has improved the optical and mechanical properties of the glass.
[0013] The present invention also provides a method for preparing silicate glass with a high zirconium oxide content, which is characterized by comprising the following steps:
[0014] (1) Glass batching: Before batching, the glass raw materials are subjected to high-temperature calcination and dehydration treatment, and then the high-purity raw materials are proportioned according to the designed components. The corresponding raw material weight is converted according to the weight percentage of each component, and then each raw material is weighed. Among them, the ZrO2 component is introduced by nano-scale zirconium silicate powder, and zirconium dioxide is not used.
[0015] (2) Glass melting: The glass batch materials are cooled, ground and mixed to form a mixture, and the mixture is placed in a platinum crucible and then heated in a glass melting furnace at 1560°C-1600°C for 4 to 8 hours; the glass mixture is melted in an oxidizing atmosphere, and the glass melt needs to be stirred several times during the melting process to make the glass melt uniform;
[0016] (3) Leakage molding: After the glass is evenly melted, the molten glass is poured into a specified shape and then placed in an annealing furnace for annealing at a temperature of 650-670°C for 6-10 hours. The glass is then cooled to room temperature in the furnace, and a silicate glass material with a high zirconium oxide content is obtained by cooling.
[0017] Furthermore, the zirconium silicate is a nano-scale powder with an average particle size of 50 nm. The zirconium silicate powder raw material needs to be stabilized before being used in glass batching, including powder homogenization and removal of harmful impurities such as Fe2O3.
[0018] Furthermore, the glass raw materials are subjected to a high-temperature burning dehydration treatment at 610-700° C., the dehydration treatment time is 12-23 hours, and the moisture and hydroxyl content of the raw materials are strictly controlled.
[0019] Furthermore, the glass is melted in an oxidizing atmosphere, that is, dry oxygen is blown into the molten glass using a platinum tube, and the flow rate of the oxygen blown is 0.9-1.5 L / min.
[0020] Furthermore, the discharge temperature in the leakage molding step is 1400°C-1450°C.
[0021] Compared with the prior art, the silicate glass with high zirconium oxide content described in the present invention adopts a low-alkali formula and has the following advantages:
[0022] (1) High ZrO2 content: the ZrO2 content of the silicate glass with high zirconium oxide content provided by the present invention is 15-19%;
[0023] (2) It has excellent chemical stability, with water resistance of Class I, acid resistance of Class II or above, and alkali resistance of Class I;
[0024] (3) It has excellent thermal properties, with a thermal expansion coefficient of (57-75)×10 at 30-300℃ -7 / ℃, glass transition temperature T g Greater than 650℃, good thermal shock resistance;
[0025] (4) It has excellent mechanical properties and its flexural strength is greater than 300MPa.
[0026] The present invention also provides an application of silicate glass with a high zirconium oxide content. The silicate glass with a high zirconium oxide content has good chemical corrosion resistance and is suitable for high temperature and high pressure resistant optical windows, optical glass, window glass, pressure and temperature resistant optical containers, optoelectronic substrate glass, chemical industry observation windows, video or camera lenses, special glass fibers, etc.
[0027] In the present invention, SiO2 is the main component of the glass skeleton structure and is the main component in the glass skeleton. The weight percentage (wt.%) of SiO2 is 39-49%. When the content of SiO2 is lower than 39wt.%, it is difficult to obtain glass with excellent thermal stability and the chemical resistance of the glass will be reduced; when the content of SiO2 is higher than 49wt.%, the high-temperature viscosity of the glass will increase, resulting in excessively high melting temperature of the glass and reduced chemical resistance.
[0028] Al2O3 is an intermediate oxide of glass, and its content cannot be too much. Al2O3 is introduced by alumina powder instead of aluminum hydroxide. The chemical bond strength of Al-O is relatively small, which is beneficial to improve the transmittance performance of glass. When there is enough oxygen in the glass, by introducing an appropriate amount of Al2O3, aluminum oxygen tetrahedron [AlO4] is formed, which can repair the internal broken network structure and form a continuous, uniform and unified network with silicon oxygen tetrahedron, so that the broken network in the glass is reduced, which is beneficial to improve the chemical stability of the glass and reduce the tendency of glass crystallization. The weight percentage of Al2O3 is 0.5-5wt.%. When the content of Al2O3 is lower than 0.5wt.%, the chemical stability and mechanical properties of the glass will be reduced. When the content of Al2O3 is higher than 5wt.%, the high temperature viscosity of the glass will be increased, resulting in excessive melting temperature of the glass.
[0029] B2O3 is a glass-forming oxide and a component of the glass skeleton. It is also a flux that reduces the viscosity of the glass melt. In an oxidizing atmosphere, B 3+ There is a tendency to capture free oxygen to form boron-oxygen tetrahedron [BO4], making the glass structure more compact, thereby improving the chemical resistance of the glass. The weight percentage of B2O3 is 6-11wt.%, and when the content of B2O3 is lower than 6wt.%, it cannot play a role in fluxing. When the content of B2O3 is higher than 11wt.%, the chemical stability of the glass will be reduced.
[0030] Na2O is an external oxide in the glass structure network, which can increase the dissolution content of ZrO2 in the glass. The weight percentage of Na2O is 0.5-1.9wt.%. If the content of Na2O is greater than 1.9wt.%, the chemical resistance of the glass will be reduced.
[0031] CaO is an external oxide of the glass structure network, and the weight percentage of CaO is 1-3wt.%. If the CaO content is lower than 1wt.%, the glass forming ability will be reduced. If the CaO content is higher than 3wt.%, the chemical resistance of the glass will be reduced and the crystallization tendency of the glass will be increased.
[0032] The introduction of ZrO2 is to enhance the chemical resistance and mechanical properties of the glass. The weight percentage of ZrO2 is 15-19wt.%. When the introduced amount of ZrO2 is less than 15wt.%, it is not easy to obtain glass with excellent chemical resistance and excellent mechanical properties. When the introduced amount of ZrO2 is greater than 19wt.%, it is easy to make the glass difficult to melt and increase the crystallization tendency of the glass.
[0033] TiO2 is used to lower the crystallization temperature of glass. 4+ When combined with alkaline earth metal oxides, it can capture free oxygen to form a uniform and unified network of [TiO4], which reduces the number of broken networks in the glass and is beneficial to reducing crystallization; when the weight percentage of TiO2 is 1-3wt.%, when the TiO2 content is greater than 3wt.%, the mechanical properties of the glass will be reduced.
[0034] Gd2O3 is a rare earth oxide. 3+ The large ion radius and strong electric field produce a strong aggregation effect in the glass, which can increase the mass of cations and improve the chemical resistance of the glass. The weight percentage of Gd2O3 is 4-10wt.%. When the content of Gd2O3 is less than 4wt.%, the chemical resistance and mechanical properties of the glass will be reduced. However, when the content of Gd2O3 is greater than 10wt.%, the thermal expansion coefficient of the glass will increase and the transition temperature of the glass will be reduced.
[0035] Y2O3 can increase the mass of cations, reduce the number of non-bridging oxygen in the glass network structure, and strengthen the network structure of the glass, thereby making the atomic arrangement in the glass structure more compact, and can significantly improve the bending strength and mechanical properties of the glass. The weight percentage of Y2O3 is 11-17wt.%. When the content of Y2O3 is less than 11wt.%, the mechanical properties of the glass will be reduced. When the content of Y2O3 is greater than 17wt.%, the chemical resistance of the glass will be reduced.
[0036] The silicate glass with high zirconium oxide content described in the present invention substantially does not contain [OH] - Here, “substantially free of a specific component” means that it is not intentionally added, and does not exclude extremely small amounts of impurities that are inevitably mixed in from raw material impurities, etc., but the amount contained will not affect the desired properties. Even if an extremely small amount is contained, it is brought in by other glass raw materials.
[0037] The present invention successfully prepares a silicate glass material with high zirconium oxide content, which has the advantages of excellent chemical stability, suitable thermal expansion coefficient, high glass transition temperature, excellent mechanical properties and the like.
[0038] The present invention also provides an application of silicate glass with a high zirconium oxide content. The silicate glass with a high zirconium oxide content has good chemical corrosion resistance and is suitable for high temperature and high pressure resistant optical windows, optical glass, window glass, pressure and temperature resistant optical containers, optoelectronic substrate glass, chemical industry observation windows, video or camera lenses, special glass fibers, etc. DETAILED DESCRIPTION
[0039] In order to make the purpose, technical solution and advantages of the present invention clearer, the implementation mode of the present invention is further described in detail below. However, the specific embodiments given by the applicant cannot and should not be regarded as limitations on the technical solution of the present invention. Any changes to the definitions of components or technical features and / or formal but not substantial changes to the overall structure should be regarded as the scope of protection defined by the technical solution of the present invention.
[0040] Table 1 lists in detail the glass chemical composition (wt. %) and glass chemical resistance of the examples.
[0041] First, glass raw materials are selected and batched according to the glass composition of the embodiment in Table 1, wherein the raw materials are required to be acid-washed quartz sand (150 μm sieve material is less than 1%, 45 μm sieve material is less than 30%, Fe2O3 content is less than 0.01wt.%), aluminum oxide powder (analytical pure, average particle size 50 μm), anhydrous boric acid (analytical pure, 400 μm sieve material is less than 10%, 63 μm sieve material is less than 10%), sodium carbonate (analytical pure, average particle size 50 μm), calcium nitrate (analytical pure, average particle size 250 μm), nano zirconium silicate (analytical pure, average particle size 50 μm), titanium oxide (analytical pure, average particle size 50 μm), gadolinium oxide (5N, average particle size 50 μm), yttrium oxide (5N, average particle size 50 μm), and Fe2O3 in the glass raw materials is strictly controlled and is required to be less than 100 ppm. The clarifier adopts a conventional clarifier in a conventional amount, such as antimony trioxide.
[0042] Among them, the thermal expansion coefficient and glass transition temperature of the glass were tested with reference to the method of GB / T 7962.16-2010 "Test method for colorless optical glass Part 16: Linear expansion coefficient, transition temperature and sag temperature"; the flexural strength of the glass was tested with reference to GB / T 37781-2019 "Test method for flexural strength of glass materials"; the water resistance stability of silicate glass with high zirconium oxide content was tested with reference to the method of GB / T 6582-2021 "Test method and classification of water resistance of glass particles at 98°C"; the acid resistance stability of silicate glass with high zirconium oxide content was tested with reference to the method of GB / T 15728-2021 "Weight test method and classification of glass resistance to boiling hydrochloric acid corrosion"; the alkali resistance stability of silicate glass with high zirconium oxide content was tested with reference to the method of GB / T 6580-2021 "Test method and classification of glass resistance to corrosion by boiling mixed alkali aqueous solution".
[0043] Table 1 Chemical composition (wt.%) and glass properties of the examples
[0044]
[0045] Example 1
[0046] The glass raw materials were selected according to the components of Example 1 and prepared, and subjected to high-temperature calcination dehydration treatment at 610°C for 23 hours to reduce the moisture and hydroxyl content of the glass raw materials. The moisture and hydroxyl content of the raw materials were strictly controlled, and then the high-purity raw materials were proportioned according to the glass chemical composition of Table 1, and then the raw materials were weighed, ground and mixed evenly to form a mixture, and the mixture was placed in a platinum crucible, and then placed in a glass melting furnace at 1600°C and heated for 4 hours; the glass mixture was melted in an oxidizing atmosphere, and Oxygen is blown into the glass melt with a platinum tube at a flow rate of 0.9 L / min; the glass melt is stirred 2 to 3 times during the glass melting process to make it uniform; after the glass is melted uniformly, the molten glass is cooled to 1450°C and poured into a preheated heat-resistant steel mold to be cast into a specified test sample required to be formed, and then placed in an annealing furnace for annealing treatment at a temperature of 670°C for 6 hours, and a silicate glass material with a high zirconium oxide content is obtained with furnace cooling. Its test performance is shown in Table 1 Example 1.
[0047] Example 2
[0048] The actual composition of the glass is shown in Table 1 Example 2. The same raw materials and raw material requirements as those in Example 1 are used, and the raw materials are subjected to a high-temperature calcination dehydration treatment at 700°C for 12 hours, and a melting process system of melting at 1560°C for 8 hours. Oxygen is blown into the molten glass using a platinum tube, and the flow rate of oxygen blown is 1.5L / min. After the glass is evenly melted, the molten glass is cooled to 1430°C and poured into a preheated heat-resistant steel mold to be cast into the specified test sample requirements, and then placed in an annealing furnace for annealing treatment. The annealing temperature is 650°C, and the annealing time is 10 hours. A silicate glass material with a high zirconium oxide content is obtained as the furnace cools. The same test conditions as in Example 1 are used, and its test performance is shown in Table 1.
[0049] As shown in Example 2.
[0050] Example 3
[0051] The actual composition of the glass is shown in Table 1 Example 3. The same raw materials and raw material requirements as those in Example 1 are used, and the glass raw materials are subjected to high-temperature burning and dehydration treatment at 650°C for 18 hours to reduce the moisture and hydroxyl content of the glass raw materials, and the moisture and hydroxyl content of the raw materials are strictly controlled. In addition, a melting process system of melting at 1580°C for 6 hours is adopted, and oxygen is blown into the glass melt using a platinum tube, and the flow rate of oxygen blowing is 1.2L / min. After the glass is melted uniformly, the molten glass liquid is cooled to 1400°C and the material is poured into a preheated heat-resistant steel mold to be cast into the specified test sample requirements, and then placed in an annealing furnace for annealing treatment, using an annealing temperature of 660°C, an annealing time of 8 hours, and the same test conditions as those in Example 1. Its test performance is shown in Table 1 Example 3.
[0052] Example 4
[0053] The actual composition of the glass refers to Example 4 in Table 1. The same raw materials and raw material requirements as those in Example 1 are used, and the same melting process system, annealing process system and test conditions are adopted. Its test performance is shown in Example 4 in Table 1.
[0054] Example 5
[0055] The actual composition of the glass refers to Example 5 in Table 1, using the same raw materials and raw material requirements as Example 1, and adopting the same melting process system, annealing process system and test conditions. Its test performance is shown in Example 5 in Table 1.
[0056] The present invention successfully prepares a silicate glass material with high zirconium oxide content, which has the advantages of excellent chemical stability, suitable thermal expansion coefficient, high glass transition temperature, excellent mechanical properties and the like.
[0057] The present invention also provides an application of silicate glass with a high zirconium oxide content. The silicate glass with a high zirconium oxide content has good chemical corrosion resistance and is suitable for high temperature and high pressure resistant optical windows, optical glass, window glass, pressure and temperature resistant optical containers, optoelectronic substrate glass, chemical industry observation windows, video or camera lenses, special glass fibers, etc.
[0058] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A silicate glass with a high zirconium oxide content, It is characterized in that The composition comprises the following weight percentages:
2. A silicate glass with a high zirconium oxide content according to claim 1, It is characterized in that Preferably include the following weight percentage components:
3. A silicate glass with a high zirconium oxide content according to claim 1 or 2, It is characterized in that Contains virtually no [OH] - Even if ions are present, they are brought in by impurities from the raw materials or during the preparation process. The hydroxyl content in the glass is strictly controlled.
4. A method for preparing a silicate glass with a high zirconium oxide content according to any one of claims 1 to 2, It is characterized in that The following steps are involved: (1) Glass batching: Before batching, the glass raw materials are subjected to high-temperature burning and dehydration treatment, and then the high-purity raw materials are proportioned according to the designed components. According to the weight percentage of each component, the corresponding raw material weight is converted, and then each raw material is weighed. Among them, ZrO 2 The components are introduced by nano-scale zirconium silicate powder, without using zirconium dioxide; (2) Glass melting: The glass batch materials are cooled, ground and mixed to form a mixture, and the mixture is placed in a platinum crucible and then heated in a glass melting furnace at 1560°C-1600°C for 4 to 8 hours; the glass mixture is melted in an oxidizing atmosphere, and the glass melt needs to be stirred several times during the melting process to make the glass melt uniform; (3) Leakage molding: After the glass is evenly melted, the molten glass is poured into a specified shape and then placed in an annealing furnace for annealing at a temperature of 650-670°C for 6-10 hours. The glass is then cooled to room temperature in the furnace, and a silicate glass material with a high zirconium oxide content is obtained by cooling.
5. The method for preparing silicate glass with high zirconium oxide content according to claim 4, It is characterized in that The zirconium silicate is a nanometer-grade powder, and the average particle size of the powder is 50 nm.
6. The method for preparing silicate glass with high zirconium oxide content according to claim 4, It is characterized in that The glass raw materials are subjected to high-temperature burning and dehydration treatment at 610-700° C. for 12-23 hours, and the moisture and hydroxyl content of the raw materials are strictly controlled.
7. The method for preparing silicate glass with high zirconium oxide content according to claim 4, It is characterized in that The oxidizing atmosphere melting during the melting is to blow dry oxygen into the molten glass using a platinum tube, and the flow rate of the oxygen blown is 0.9-1.5 L / min.
8. The method for preparing silicate glass with high zirconium oxide content according to claim 4, It is characterized in that The discharge temperature in the leakage molding step is 1400°C-1450°C.
9. The silicate glass with a high zirconium oxide content according to any one of claims 1 to 8, It is characterized in that The silicate glass with a high zirconium oxide content has the advantages of excellent chemical stability, suitable thermal expansion coefficient, high glass transition temperature, excellent mechanical properties and the like.
10. The silicate glass with a high zirconium oxide content according to any one of claims 1 to 9, It is characterized in that The silicate glass with high zirconium oxide content has good chemical corrosion resistance and is suitable for high temperature and high pressure resistant optical windows, optical glass, window glass, pressure and temperature resistant optical containers, optoelectronic substrate glass, chemical industry observation windows, video or camera lenses, special glass fibers, etc.
Citation Information
Patent Citations
High-zirconium alkali-proof glass and application thereof
CN110156327A
Glass, and preparation method and application thereof
CN112047638A
Optical glass
CN112125511A
Starting glass, lithium silicate glass with core, preparation method and application thereof
CN112694253A
Soda-lime-silica glass compositions and uses thereof
CN1140443A