Glass wool and production method thereof

By using hydrophobic acrylate adhesive and silicone grafted modified polyurethane, a hydrophobic film is formed, which solves the problem of high water absorption rate of glass wool, improves its service life and mechanical properties, and achieves an environmentally friendly and efficient waterproofing effect.

CN118993554APending Publication Date: 2024-11-22ANHUI JIYAO GLASS MICROFIBER CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411363127.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-27
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The high water absorption rate of glass wool leads to a decrease in thermal insulation and sound insulation effect, shortening service life, and traditional adhesives have problems of formaldehyde emissions and poor water resistance.

Method used

Hydrophobic acrylic adhesive is used to combine aqueous acrylic emulsion, aminosilane coupling agent and silicone graft-modified polyurethane to form a hydrophobic film to reduce water absorption, and improve the interface effect between the adhesive and the glass wool surface Improve waterproofing and mechanical strength.

Benefits of technology

It significantly reduces the water absorption rate of glass wool, extends the service life, and reduces the emission of volatile organic compounds through environmentally friendly hydrophobic treatment, and improves the durability and mechanical properties of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005065418700000111
    Figure BDA0005065418700000111
Patent Text Reader

Abstract

The invention discloses glass wool and a production method thereof, and belongs to the technical field of glass wool, the glass wool is prepared from the following raw materials in parts by mass: 65-75 parts of flat cullet, 3-5 parts of quartz sand, 5-10 parts of borax pentahydrate, 4-8 parts of feldspar, 2-5 parts of sodium carbonate, 1-3 parts of dolomite and 6-12 parts of a hydrophobization adhesive, and the hydrophobization adhesive is a hydrophobization acrylate adhesive. The raw materials of the hydrophobization adhesive comprise a water-based acrylic emulsion, an amino silane coupling agent, vinyl silicone oil and organic silicon graft modified polyurethane, the interface interaction between the adhesive and the glass wool is improved while the green and environment-friendly effects are guaranteed, excellent hydrophobicity is provided for the glass wool by adding a siloxane chain segment, and the hydrophobicity of the glass wool is improved. Wherein organic silicon grafted modified polyurethane enables organic silicon chain segments to be uniformly enriched on the surface of the glass wool, and also supports the mechanical property of the glass wool, so that the mechanical strength of the glass wool is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of glass wool, and in particular relates to glass wool and a production method thereof. Background Art

[0002] Glass wool is a man-made inorganic fiber, a type of glass fiber. It is a cotton-like material prepared by high-speed centrifugation or blowing after melting glass. It has many performance characteristics such as good molding, low volume density, low thermal conductivity, good thermal insulation performance, good sound absorption performance, corrosion resistance and stable chemical properties. It is used in many technical fields such as building insulation, HVAC, industrial equipment insulation, automobile sound insulation, pipeline protection, etc.

[0003] However, glass wool has a high water absorption rate and is easily affected by moisture. Long-term exposure to a humid environment may cause the thermal insulation and sound insulation effects of the glass wool to be greatly reduced. It may even become moldy and smelly after long-term use. Even after air-drying, it cannot recover to its original performance, which greatly reduces the service life of the glass wool. Summary of the invention

[0004] The object of the present invention is to provide a glass wool and a production method thereof, so as to solve the problems of high water absorption rate and shortened service life of the glass wool, and the obtained glass wool has high mechanical strength.

[0005] The purpose of the present invention can be achieved by the following technical solutions:

[0006] In a first aspect, the present application provides a glass wool comprising the following raw materials in parts by weight:

[0007] 65-75 parts of flat glass cullet;

[0008] 3-5 parts of quartz sand;

[0009] 5-10 parts of borax pentahydrate;

[0010] 4 to 8 parts of feldspar;

[0011] 2-5 parts of soda ash;

[0012] 1 to 3 parts of dolomite;

[0013] 6-12 parts of hydrophobic adhesive;

[0014] The hydrophobized adhesive is a hydrophobized acrylic adhesive.

[0015] Preferably, the particle size of the flat glass cullet is 0.5 to 1 mm.

[0016] By adopting the above-mentioned technical scheme, through the mutual cooperation of feldspar and soda ash, the content of alkali metal oxides in the system can be increased. Generating more free oxygen in the production process can increase the O-Si structure ratio in the glass wool structure, reduce the viscosity of the glass liquid, promote the emission of bubbles in the process, reduce defects in the glass wool, and improve the strength of the glass wool itself. In addition, the present application adopts borax pentahydrate to increase the content of boron oxide, which can accelerate the clarification process of the glass liquid and improve production efficiency.

[0017] Due to the porous structure of glass wool and the hydrophilicity of its surface, the water absorption rate of glass wool is high, which in turn affects the performance and service life of glass wool. The adhesive used in this application is a hydrophobic adhesive, specifically, a hydrophobic acrylic adhesive. Compared with traditional phenolic resin adhesives or melamine resin adhesives, acrylic adhesives do not produce substances harmful to health such as formaldehyde, and are environmentally friendly; and the hydrophobic acrylic adhesive can not only solve the problem of poor water resistance of acrylic adhesives themselves, while improving material performance while being green and environmentally friendly, but also can form a hydrophobic film on the surface through the hydrophobic acrylic adhesive, thereby preventing water from penetrating and affecting glass wool, improving the hydrophobic performance of glass wool, and the good bonding performance between the hydrophobic acrylic adhesive and glass wool, and can also improve the durability of the hydrophobic performance of glass wool and extend the service life of glass wool.

[0018] Preferably, the hydrophobic adhesive comprises the following raw materials in parts by weight:

[0019] 100 parts of water-based acrylic emulsion;

[0020] 4-6 parts of aminosilane coupling agent;

[0021] 5-10 parts of vinyl silicone oil;

[0022] 8 to 12 parts of silicone grafted modified polyurethane.

[0023] Preferably, the acrylic monomer of the aqueous acrylic emulsion includes a combination of two or more of methyl methacrylate, methyl acrylate, styrene, hydroxypropyl acrylate, ethyl acrylate, isooctyl acrylate, hydroxyethyl acrylate, n-butyl acrylate, and ethyl methacrylate.

[0024] Preferably, the aminosilane coupling agent includes a combination of one or more of γ-aminopropyltriethoxysilane, γ-aminopropyltrimethoxysilane, N-β (aminoethyl)-γ-aminopropylmethyldimethoxysilane, N-β (aminoethyl)-γ-aminopropyltrimethoxysilane, and N-β (aminoethyl)-γ-aminopropyltriethoxysilane.

[0025] By adopting the above technical solution, the raw material matrix of the hydrophobic adhesive of the present application adopts water-based acrylic emulsion without other organic solvents, which can reduce the emission of volatile organic compounds during production or use. At the same time, in order to improve the adhesion between the acrylic emulsion and the glass wool, an aminosilane coupling agent is also added to the system, which can improve the interface between the inorganic interface, i.e., the surface of the glass wool, and the organic matter, i.e., the water-based acrylic emulsion, and help the adhesive to form a stable network structure on the surface of the glass wool.

[0026] The introduction of siloxane segments in the aminosilane coupling agent can also cooperate with vinyl silicone oil to jointly improve the hydrophobic properties of glass wool. The siloxane main chain in the vinyl silicone oil has excellent hydrophobicity and chemical stability, which can reduce the wettability of the glass wool surface and improve the waterproof performance. In addition, the high flexibility of vinyl silicone oil can make the stretching of the composite material more uniform, reduce the hysteresis of the adhesive hydrophobic film, and thus improve the hydrophobic properties, which can effectively improve the moisture resistance of the glass wool and extend its service life.

[0027] In addition, silicone grafted modified polyurethane is added to the hydrophobic acrylate adhesive. On the one hand, the polyurethane chain segment contains isocyanate groups, which can react and link with the water-based acrylic emulsion. While increasing the curing speed of the acrylate adhesive, it can also increase the cross-linking density of the adhesive on the surface of the glass wool and improve the adhesion performance. At the same time, the polyurethane chain segment, as a part of the cross-linked network bonded to the surface of the glass wool, can also serve as a support for the mechanical properties of the material, which is beneficial to improve the mechanical strength of the glass wool. On the other hand, the use of silicone grafted modified polyurethane can introduce more silicone segments into the cross-linked network structure of the adhesive, improve the uniform enrichment of silicone segments on the surface of the glass wool, and significantly improve the hydrophobicity of the glass wool.

[0028] Preferably, the raw materials of the organosilicon grafted modified polyurethane include diisocyanate, polyether diol, dihydroxymethyl acid and terminal isocyanate polysiloxane in a mass ratio of 1: (4.5-5.5): (0.3-0.4): (0.025-0.035).

[0029] Preferably, the diisocyanate includes one or more of isophorone diisocyanate, hexamethylene diisocyanate, and diphenylmethane diisocyanate.

[0030] Preferably, the dimethylol acid is one or a combination of dimethylolpropionic acid and dimethylolbutanoic acid.

[0031] Preferably, the average molecular weight of the polyether diol is 1500-2000.

[0032] Preferably, the organosilicon grafted modified polyurethane is prepared according to the following method:

[0033] Preparation of terminal isocyanate polysiloxane: after isophorone diisocyanate and single-terminated dihydroxy polydimethylsiloxane are uniformly mixed, an organic bismuth catalyst is added, the temperature is raised to 80-90° C., and the isocyanate-terminated polysiloxane is obtained after stirring and reacting for 6-8 hours.

[0034] Preparation of organosilicon grafted modified polyurethane: After diisocyanate, polyether diol and terminal isocyanate polysiloxane are evenly mixed, an organic bismuth catalyst is added, and under a nitrogen atmosphere, the temperature is increased to 80-90°C, dihydroxymethyl acid is added, and the reaction is stirred for 5-6 hours, and then filtered and dried to obtain the organosilicon grafted modified polyurethane.

[0035] Preferably, the average molecular weight of the single-ended dihydroxy polydimethylsiloxane is 3000-3500.

[0036] Preferably, the mass ratio of the single-ended dihydroxy polydimethylsiloxane to isophorone diisocyanate is 100:(4.3-5).

[0037] By adopting the above technical scheme, a polysiloxane containing an isocyanate group at the terminal is obtained by reacting the isocyanate group in isophorone diisocyanate with the terminal hydroxyl group in single-ended dihydroxy polydimethylsiloxane; further, an isocyanate-terminated polysiloxane is introduced into the process of forming polyurethane by reaction and polymerization between diisocyanate and diol, and the isocyanate group at the terminal is used as a reactive group to participate in the polymerization process of polyurethane, and an organosilicon segment is introduced into the side group of the main chain of the polyurethane without affecting the main chain structure performance of the polyurethane, and the isocyanate group contained can react with the active group in the aqueous acrylic emulsion to accelerate curing and improve the overall mechanical strength, and the introduced organosilicon side chain is linked in the cross-linked network structure and can be more evenly enriched on the surface of the glass wool, thereby reducing the water absorption rate of the glass wool, and can maintain the hydrophobicity of the glass wool for a long time, improve the durability of the hydrophobic glass wool, and extend the service life of the glass wool.

[0038] Preferably, the hydrophobic adhesive is prepared according to the following steps: add aminosilane coupling agent, vinyl silicone oil and silicone grafted modified polyurethane into water, stir and mix at 10-15°C for 10-20 minutes, then add water-based acrylic emulsion, and continue stirring for 30-40 minutes to obtain the hydrophobic adhesive.

[0039] By adopting the above technical solution, each auxiliary agent is mixed with the water-based acrylic emulsion at a low temperature, so that the direct curing reaction of acrylic acid can be inhibited or reduced.

[0040] In a second aspect, the present application also provides a method for producing glass wool, comprising the following process steps:

[0041] S1. Weigh the corresponding mass fractions of flat glass, quartz sand, borax pentahydrate, feldspar, soda ash and dolomite and mix them evenly, and dry them at 70 to 80 ° C for 1 to 2 hours to obtain a mixed powder;

[0042] S2. The obtained mixed powder is preheated at 300-400°C for 2-3h, and then the temperature is raised to 1200-1400°C, and kept warm until the mixed powder is completely melted to obtain a transparent glass liquid;

[0043] S3. The glass liquid is centrifugally blown at a centrifugal speed of 3500 to 4000 r / min and a temperature of 800 to 850° C., and finally stretched to obtain glass wool fiber filaments;

[0044] S4. Spray the hydrophobic adhesive onto the surface of the glass wool fiber, dry and solidify at 60-80° C. to obtain glass wool.

[0045] Beneficial effects of the present invention:

[0046] 1. The glass wool obtained by using a suitable powder ratio in the present application has high mechanical strength. At the same time, a hydrophobic acrylic adhesive is added during the production process. The water-based acrylic emulsion as the main adhesive matrix does not produce formaldehyde compared to traditional adhesives, thereby reducing the emission of volatile organic compounds; the aminosilane coupling agent can improve the interface between the adhesive and the surface of the glass wool, and cooperate with the vinyl silicone oil to form a hydrophobic film on the surface to improve the waterproof performance of the glass wool.

[0047] 2. The hydrophobic acrylate adhesive used in the present application is also added with silicone grafted modified polyurethane. The isocyanate group in the polyurethane chain segment can accelerate the curing speed of the adhesive, improve the crosslinking density and adhesion performance, and can also serve as a support for the mechanical properties of the material to improve the mechanical strength of the glass wool; and the silicone segment is introduced into the side group of the polyurethane, which can be linked with the polyurethane in the cross-linked network structure formed by the adhesive, so that the silicone segment can be evenly enriched on the surface of the glass wool, significantly reducing the water absorption rate of the material and increasing the hydrophobic durability of the glass wool. DETAILED DESCRIPTION

[0048] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0049] Preparation Example

[0050] Preparation Example 1 Water-based acrylic emulsion

[0051] Preparation Example 1-1, an aqueous acrylic emulsion, is prepared according to the following method:

[0052] Take 10g of methyl methacrylate, 25g of ethyl acrylate and 5g of hydroxyethyl acrylate and mix them evenly to obtain a mixed monomer. Add 1.5g of sodium dodecyl sulfate to 40g of water, raise the temperature to 40°C after mixing, drop the mixed monomer, and keep warm for 30 minutes after the addition is completed to obtain a pre-emulsion. Add 15g of water, 1g of sodium dodecyl sulfate and 1.5g of ammonium persulfate to the pre-emulsion, adjust the pH to 6.5 with ammonia water, raise the temperature to 80°C, stir and react for 1.5h, then drop 0.5g of sodium dodecyl sulfate and 0.5g of ammonium persulfate, keep the temperature unchanged and add 1g of n-dodecyl mercaptan, stir and react for 30min to obtain a water-based acrylic emulsion.

[0053] Preparation Example 2 Silicone Grafted Modified Polyurethane

[0054] Preparation Example 2-1, a silicone grafted modified polyurethane, is prepared according to the following method:

[0055] Preparation of terminal isocyanate polysiloxane: 4.6 g of isophorone diisocyanate and 100 g of single-terminated dihydroxy polydimethylsiloxane (average molecular weight of 3200) were mixed evenly, and 0.5 g of organic bismuth catalyst (model MB20) was added. The temperature was raised to 85°C, and the reaction was stirred for 7 hours to obtain terminal isocyanate polysiloxane.

[0056] Preparation of silicone grafted modified polyurethane: 10g of isophorone diisocyanate, 50g of polyether diol (average molecular weight of 2000) and 0.3g of terminal isocyanate polysiloxane were mixed evenly, and 0.1g of organic bismuth catalyst (model MB20) was added. Under a nitrogen atmosphere, the temperature was raised to 80°C, 3.5g of dihydroxymethylpropionic acid was added, and the reaction was stirred for 6h, and then filtered and dried to obtain silicone grafted modified polyurethane.

[0057] Preparation Example 2-2, a silicone grafted modified polyurethane, is different from Preparation Example 2-1 only in that the added amount of polyether diol is 45 g, the added amount of terminal isocyanate polysiloxane is 0.25 g, and the added amount of dimethylol propionic acid is 4 g.

[0058] Preparation Example 2-3, a silicone grafted modified polyurethane, is different from Preparation Example 2-1 only in that the added amount of polyether diol is 55 g, the added amount of terminal isocyanate polysiloxane is 0.35 g, and the added amount of dimethylol propionic acid is 3 g.

[0059] Preparation Example 2-4, a silicone grafted modified polyurethane, is different from Preparation Example 2-1 only in that the amount of terminal isocyanate polysiloxane added is 0.15 g.

[0060] Preparation Example 2-5, a silicone grafted modified polyurethane, is different from Preparation Example 2-1 only in that the amount of terminal isocyanate polysiloxane added is 0.45 g.

[0061] Preparation Example 2-6, a silicone grafted modified polyurethane, was prepared according to the following method:

[0062] 10 g of isophorone diisocyanate and 50 g of polyether diol (average molecular weight of 2000) were mixed evenly, and 0.1 g of an organic bismuth catalyst (model MB20) was added. Under a nitrogen atmosphere, the temperature was raised to 80°C, 3.5 g of dihydroxymethylpropionic acid was added, and the mixture was stirred for 6 hours and then filtered and dried to obtain an organosilicon-grafted modified polyurethane.

[0063] Preparation Example 3 Hydrophobic Adhesive

[0064] Preparation Example 3-1, a hydrophobic adhesive, prepared according to the following method:

[0065] Add 5g of γ-aminopropyltriethoxysilane, 8g of vinyl silicone oil (model KF-99) and 10g of the silicone grafted modified polyurethane prepared in Preparation Example 2-1 to 50g of water, stir and mix at 10°C for 15min, then add the aqueous acrylic emulsion prepared in Preparation Example 1, and continue stirring for 30min to obtain a hydrophobic adhesive.

[0066] Preparation Example 3-2, a hydrophobic adhesive, differs from Preparation Example 3-1 only in that the added amount of γ-aminopropyltriethoxysilane is 4 g, the added amount of vinyl silicone oil is 5 g, and the added amount of the silicone grafted modified polyurethane prepared in Preparation Example 2-2 is 12 g.

[0067] Preparation Example 3-3, a hydrophobic adhesive, differs from Preparation Example 3-1 only in that the added amount of γ-aminopropyltriethoxysilane is 6 g, the added amount of vinyl silicone oil is 10 g, and the added amount of the silicone grafted modified polyurethane prepared in Preparation Example 2-3 is 8 g.

[0068] Preparation Example 3-4 is a hydrophobic adhesive, which is different from Preparation Example 3-1 only in that the organosilicon grafted modified polyurethane prepared in Preparation Example 2-1 is replaced by an equal amount of the organosilicon grafted modified polyurethane prepared in Preparation Example 2-4.

[0069] Preparation Example 3-5, a hydrophobic adhesive, is different from Preparation Example 3-1 only in that the organosilicon grafted modified polyurethane prepared in Preparation Example 2-1 is replaced by an equal amount of the organosilicon grafted modified polyurethane prepared in Preparation Example 2-5.

[0070] Preparation Example 3-6, a hydrophobic adhesive, is different from Preparation Example 3-1 only in that the organosilicon grafted modified polyurethane prepared in Preparation Example 2-1 is replaced by an equal amount of the organosilicon grafted modified polyurethane prepared in Preparation Example 2-6.

[0071] Preparation Example 3-7, a hydrophobic adhesive, is different from Preparation Example 3-1 only in that the added amount of the organosilicon grafted modified polyurethane prepared in Preparation Example 2-1 is 5 g.

[0072] Preparation Example 3-8, a hydrophobic adhesive, is different from Preparation Example 3-1 only in that the added amount of the silicone grafted modified polyurethane prepared in Preparation Example 2-1 is 15 g.

[0073] Preparation Example 3-9 is a hydrophobic adhesive, which is different from Preparation Example 3-1 only in that the silicone grafted modified polyurethane prepared in Preparation Example 2-1 is not added.

[0074] Preparation Example 3-10 is a hydrophobic adhesive, which is different from Preparation Example 3-1 only in that no vinyl silicone oil is added.

[0075] Preparation Example 3-11 is a hydrophobic adhesive, which is different from Preparation Example 3-1 only in that γ-aminopropyltriethoxysilane is not added.

[0076] Preparation Example 3-12 is a hydrophobic adhesive, which is different from Preparation Example 3-1 only in that vinyl silicone oil and the organosilicon-modified grafted polyurethane prepared in Preparation Example 2-1 are not added.

[0077] Example

[0078] Embodiment 1, a glass wool, is prepared by the following production method:

[0079] S1. Weigh 700g of flat glass (average particle size of 0.6mm), 40g of quartz sand (average particle size of 120 mesh), 80g of borax pentahydrate (average particle size of 35 mesh), 60g of feldspar (whose composition includes 72.23% silicon dioxide, 15.58% aluminum oxide, 5% sodium oxide, 4.15% potassium oxide, 0.27% iron oxide and impurities), 40g of soda ash and 20g of dolomite (whose composition includes 32.42% calcium oxide, 18.45% magnesium oxide and 49.13% carbon dioxide) and mix them evenly, and dry them at 80°C for 2h to obtain a mixed powder;

[0080] S2. The obtained mixed powder was preheated at 350°C for 3h, and then the temperature was raised to 1300°C and kept warm until the mixed powder was completely melted to obtain a transparent glass liquid;

[0081] S3. The glass liquid is centrifugally blown at a centrifugal speed of 3600 r / min and a temperature of 800° C., and finally stretched to obtain glass wool fiber filaments;

[0082] S4. Spray 100 g of the hydrophobic adhesive prepared in Preparation Example 3-1 on the surface of the glass wool fiber, dry and solidify at 65° C. to obtain glass wool.

[0083] Embodiment 2 and embodiment 3 are glass wool, which differ from embodiment 1 only in that the ratio of raw materials is changed, as shown in Table 1:

[0084] Table 1 Formulations of Examples 1 to 3

[0085] Flat glass Quartz sand Borax Pentahydrate Feldspar soda ash dolomite Hydrophobic adhesive Example 1 700 40 80 60 40 20 100 Example 2 650 50 50 40 50 10 60 Example 3 750 30 100 80 20 30 120

[0086] The hydrophobic adhesives used in Examples 1 to 3 are all the hydrophobic adhesives prepared in Preparation Example 3-1.

[0087] Example 4, a glass wool, is different from Example 1 only in that the hydrophobic adhesive prepared in Preparation Example 3-1 is replaced by an equal amount of the hydrophobic adhesive prepared in Preparation Example 3-2.

[0088] Example 5, a glass wool, is different from Example 1 only in that the hydrophobic adhesive prepared in Preparation Example 3-1 is replaced by an equal amount of the hydrophobic adhesive prepared in Preparation Example 3-3.

[0089] Example 6, a glass wool, is different from Example 1 only in that the hydrophobic adhesive prepared in Preparation Example 3-1 is replaced by an equal amount of the hydrophobic adhesive prepared in Preparation Example 3-4.

[0090] Example 7, a glass wool, is different from Example 1 only in that the hydrophobic adhesive prepared in Preparation Example 3-1 is replaced by an equal amount of the hydrophobic adhesive prepared in Preparation Example 3-5.

[0091] Example 8, a glass wool, is different from Example 1 only in that the hydrophobic adhesive prepared in Preparation Example 3-1 is replaced by an equal amount of the hydrophobic adhesive prepared in Preparation Example 3-7.

[0092] Example 9, a glass wool, is different from Example 1 only in that the hydrophobic adhesive prepared in Preparation Example 3-1 is replaced by an equal amount of the hydrophobic adhesive prepared in Preparation Example 3-8.

[0093] Comparative Example

[0094] Comparative Example 1 is a glass wool, which is different from Example 1 only in that the amount of the hydrophobic adhesive prepared in Preparation Example 3-1 added is 40 g.

[0095] Comparative Example 2, a glass wool, is different from Example 1 only in that the amount of the hydrophobic adhesive prepared in Preparation Example 3-1 added is 150 g.

[0096] Comparative Example 3 is a glass wool, which is different from Example 1 only in that the hydrophobic adhesive prepared in Preparation Example 3-1 is replaced by an equal amount of the hydrophobic adhesive prepared in Preparation Example 3-6.

[0097] Comparative Example 4 is a glass wool, which is different from Example 1 only in that the hydrophobic adhesive prepared in Preparation Example 3-1 is replaced by an equal amount of the hydrophobic adhesive prepared in Preparation Example 3-9.

[0098] Comparative Example 5 is a glass wool, which is different from Example 1 only in that the hydrophobicized adhesive prepared in Preparation Example 3-1 is replaced by an equal amount of the hydrophobicized adhesive prepared in Preparation Example 3-10.

[0099] Comparative Example 6, a glass wool, is different from Example 1 only in that the hydrophobicized adhesive prepared in Preparation Example 3-1 is replaced by an equal amount of the hydrophobicized adhesive prepared in Preparation Example 3-11.

[0100] Comparative Example 7, a glass wool, is different from Example 1 only in that the hydrophobicized adhesive prepared in Preparation Example 3-1 is replaced by an equal amount of the hydrophobicized adhesive prepared in Preparation Example 3-12.

[0101] Comparative Example 8, a glass wool, is different from Example 1 only in that the hydrophobic adhesive prepared in Preparation Example 3-1 is replaced by an equal amount of the aqueous acrylic emulsion prepared in Preparation Example 1-1.

[0102] Performance testing

[0103] 1. Water repellency test: The water repellency of the glass wool obtained in the examples and comparative examples was tested according to the relevant records in GB / T10299-2011 "Water repellency test method for thermal insulation materials". The samples were baked at 250°C for 24 hours to test the attenuation rate of the water repellency of the glass wool.

[0104] 2. Mechanical strength test: According to the relevant records in GB / T13480-2014 "Determination of compression properties of thermal insulation products for building", the compressive strength of the glass wool obtained in the examples and comparative examples was tested to characterize the mechanical strength properties of the glass wool.

[0105] The above test results are shown in Table 2:

[0106] Table 2 Glass wool performance test results

[0107]

[0108] According to Table 2, in combination with Example 1, Example 2 to Example 5, it can be seen that the hydrophobicity, baking attenuation rate and compressive strength of Example 2 to Example 5 are not significantly changed compared with Example 1, indicating that the hydrophobicity, hydrophobic durability, thermal stability and mechanical strength of Example 2 to Example 5 are not significantly changed compared with Example 1. The difference between Example 2 to Example 5 and Example 1 is only that the ratio of raw materials and the raw materials are changed within the required range, indicating that changing the raw material ratio parameters within the required range has little effect on the performance of the material.

[0109] Combining Example 1, Example 6, Example 7 and Comparative Example 3, it can be seen that the hydrophobicity of Example 6, Example 7 and Comparative Example 3 is lower than that of Example 1, among which Comparative Example 3 is significantly lower, indicating that the hydrophobicity of Example 6, Example 7 and Comparative Example 3 is lower than that of Example 1. The only difference between Example 6, Example 7 and Comparative Example 3 and Example 1 is that the content of the organosilicon side chain of the organosilicon grafted modified polyurethane in the hydrophobic adhesive changes. Specifically, the organosilicon content in Example 6 decreases, the enrichment degree on the surface of the glass wool decreases, and the enhancement effect of the siloxane main chain on the hydrophobicity of the material decreases, resulting in a decrease in the hydrophobicity of the glass wool. In Comparative Example 3, there is no grafted organosilicon segment on the molecular chain of the polyurethane, and the hydrophobicity decreases significantly. In Example 7, the content of the organosilicon segment increases, and the interaction between the glass wool and the polyurethane is limited. Excessive organosilicon segments will be buried deep in the cross-linked network, and the hydrophobicity decreases.

[0110] Combining Example 1, Example 8, Example 9 and Comparative Example 4, it can be seen that the hydrophobicity, baking attenuation rate and compressive strength of Example 8, Example 9 and Comparative Example 4 are reduced compared with Example 1, among which Comparative Example 4 is significantly reduced, indicating that the hydrophobicity, durability and mechanical strength of Example 8, Example 9 and Comparative Example 4 are all reduced compared with Example 1. The difference between Example 8, Example 9 and Comparative Example 4 and Example 1 is only that the amount of silicone grafted modified polyurethane added in the adhesive is changed. Specifically, the amount of modified polyurethane added in Example 8 is reduced. In addition to the corresponding reduction of silicone segments for hydrophobic modification, the decrease in polyurethane content will lead to an increase in the curing speed of the adhesive, a decrease in the cross-linking density of the formed cross-linked network, and a decrease in the adhesion performance between the adhesive and the glass wool surface after film formation, resulting in a decrease in durability. In addition, polyurethane can serve as a mechanical performance support for glass wool. The mechanical strength of glass wool is also reduced by reducing the content of modified polyurethane. The adhesive of Comparative Example 4 does not add modified polyurethane, and the performance decrease is more obvious. In Example 9, the amount of modified polyurethane added was increased, and excessive addition of rigid segments was not conducive to improving material performance.

[0111] Combining Example 1, Comparative Example 1 and Comparative Example 2, it can be seen that the hydrophobicity and compressive strength of Comparative Example 1 and Comparative Example 2 have decreased, and the baking attenuation rate of Comparative Example 2 has also decreased, indicating that the hydrophobicity and mechanical strength of Comparative Example 1 and Comparative Example 2 have decreased. The difference between Comparative Example 1 and Comparative Example 2 compared with Example 1 is only the difference in the amount of adhesive added. In Comparative Example 1, the amount of hydrophobicized adhesive added is reduced, and the hydrophobic modification effect is reduced accordingly. In addition, there is no interface effect between the adhesive and the glass wool, and the mechanical properties of the glass wool are reduced. In Comparative Example 2, the amount of hydrophobicized adhesive added is increased, and the large increase in hydrophobic segments is not conducive to the improvement of the adhesion between the adhesive and the glass wool, resulting in a decrease in the durability of the hydrophobic material.

[0112] Combined with Example 1, Comparative Examples 5 to 8, it can be seen that the hydrophobicity, post-baking attenuation rate and compression strength of Comparative Examples 5 to 8 are significantly reduced compared with those of Example 1, indicating that the hydrophobicity and mechanical strength of Comparative Examples 5 to 8 are significantly reduced. Specifically, no vinyl silicone oil is added to the hydrophobic adhesive of Comparative Example 5, the adhesive is unevenly stretched on the surface of the glass wool, and the hydrophobic effect is reduced; no aminosilane coupling agent is added to the hydrophobic adhesive of Comparative Example 6, the interface effect between the glass wool and the adhesive is significantly reduced, the adhesion ability is reduced, and the hydrophobic durability is significantly reduced; neither vinyl silicone oil nor silicone grafted modified polyurethane is added to the hydrophobic adhesive of Comparative Example 7, resulting in a significant decrease in the content of hydrophobic segments on the surface of the glass wool, a very significant decrease in hydrophobicity, and a lack of mechanical performance support of polyurethane, the mechanical strength of the material is also significantly reduced; the hydrophobic adhesive of Comparative Example 8 is only a water-based acrylic emulsion, and the hydrophobic performance of the glass wool is more significantly reduced.

[0113] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0114] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A glass wool, characterized in that: Including the following raw materials by mass: 65-75 parts of flat glass cullet; 3-5 parts of quartz sand; 5-10 parts of borax pentahydrate; 4 to 8 parts of feldspar; 2-5 parts of soda ash; 1 to 3 parts of dolomite; 6-12 parts of hydrophobic adhesive; The hydrophobized adhesive is a hydrophobized acrylic adhesive.

2. The glass wool according to claim 1, characterized in that: The hydrophobic adhesive comprises the following raw materials in parts by weight: 100 parts of water-based acrylic emulsion; 4-6 parts of aminosilane coupling agent; 5-10 parts of vinyl silicone oil; 8 to 12 parts of silicone grafted modified polyurethane.

3. The glass wool according to claim 2, characterized in that: The raw materials of the organosilicon grafted modified polyurethane include diisocyanate, polyether diol, dihydroxymethyl acid and terminal isocyanate polysiloxane in a mass ratio of 1: (4.5-5.5): (0.3-0.4): (0.025-0.035).

4. The glass wool according to claim 3, characterized in that: The diisocyanate includes one or more of isophorone diisocyanate, hexamethylene diisocyanate, and diphenylmethane diisocyanate.

5. The glass wool according to claim 3, characterized in that: The dimethylol acid is one or a combination of dimethylol propionic acid and dimethylol butyric acid.

6. The glass wool according to claim 3, characterized in that: The organosilicon graft modified polyurethane is prepared according to the following method: Preparation of terminal isocyanate polysiloxane: after isophorone diisocyanate and single-terminated dihydroxy polydimethylsiloxane are uniformly mixed, an organic bismuth catalyst is added, the temperature is raised to 80-90° C., and the reaction is stirred for 6-8 hours to obtain terminal isocyanate polysiloxane; Preparation of organosilicon grafted modified polyurethane: After diisocyanate, polyether diol and terminal isocyanate polysiloxane are evenly mixed, an organic bismuth catalyst is added, and under a nitrogen atmosphere, the temperature is increased to 80-90°C, dihydroxymethyl acid is added, and the reaction is stirred for 5-6 hours, and then filtered and dried to obtain the organosilicon grafted modified polyurethane.

7. The glass wool according to claim 2, characterized in that: The acrylic monomer of the aqueous acrylic emulsion includes a combination of two or more of methyl methacrylate, methyl acrylate, styrene, hydroxypropyl acrylate, ethyl acrylate, isooctyl acrylate, hydroxyethyl acrylate, n-butyl acrylate, and ethyl methacrylate.

8. The glass wool according to claim 2, characterized in that: The aminosilane coupling agent includes one or more combinations of γ-aminopropyltriethoxysilane, γ-aminopropyltrimethoxysilane, N-β (aminoethyl)-γ-aminopropylmethyldimethoxysilane, N-β (aminoethyl)-γ-aminopropyltrimethoxysilane, and N-β (aminoethyl)-γ-aminopropyltriethoxysilane.

9. The glass wool according to claim 2, characterized in that: The hydrophobic adhesive is prepared according to the following steps: adding aminosilane coupling agent, vinyl silicone oil and silicone grafted modified polyurethane into water, stirring and mixing at 10-15° C. for 10-20 minutes, adding water-based acrylic emulsion, and continuing stirring for 30-40 minutes to obtain the hydrophobic adhesive.

10. A method for producing glass wool according to any one of claims 1 to 9, characterized in that: The process steps include: S1. Weigh the corresponding mass fractions of flat glass, quartz sand, borax pentahydrate, feldspar, soda ash and dolomite and mix them evenly, and dry them at 70 to 80 ° C for 1 to 2 hours to obtain a mixed powder; S2. The obtained mixed powder is preheated at 300-400°C for 2-3h, and then the temperature is raised to 1200-1400°C, and kept warm until the mixed powder is completely melted to obtain a transparent glass liquid; S3. The glass liquid is centrifugally blown at a centrifugal speed of 3500 to 4000 r / min and a temperature of 800 to 850° C., and finally stretched to obtain glass wool fiber filaments; S4. Spray the hydrophobic adhesive onto the surface of the glass wool fiber, dry and solidify at 60-80° C. to obtain glass wool.

Citation Information

Cited By

  • Flux-added glass wool raw material and glass wool preparation method

    CN122444430A