Concrete micro-foam air entraining agent

By using the micro-foam gas induction agent of composite foam stabilizer in concrete, the poor bubble stability caused by polycarboxylic acid water reducing agent is solved, the uniform distribution of bubbles and the improvement of the durability of concrete are achieved, and the quality of concrete hardened body is solved question.

CN118993606APending Publication Date: 2024-11-22LANZHOU RESOURCES & ENVIRONMENT VOC TECH COLLEGE +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410916134.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-09
Publication Date
2024-11-22

Smart Images

  • Figure CN118993606A_ABST
    Figure CN118993606A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of engineering material preparation, and particularly discloses a concrete micro-foam air entraining agent which is prepared from the following components in parts by weight: 8-10 parts of fatty alcohol-polyoxyethylene ether sodium sulfate, 10-12 parts of alpha-sodium olefin sulfonate, 8-10 parts of maltodextrin, 10-12 parts of carboxymethyl starch and 60 parts of water. The invention aims to solve the technical problems that bubbles of high-fluidity concrete prepared from a polycarboxylate superplasticizer are easy to migrate and float and are gathered and communicated to form inferior large bubbles, and the fracture loss is serious. The concrete foam stabilizer is compounded in the concrete air entraining agent prepared by the research of the project, so that the bubble strength is improved, and the breakage rate is reduced. Meanwhile, the foam stabilizer can improve the viscoplasticity of the concrete, prevent the bubbles from floating and migrating, prevent the bubbles from being communicated and combined, and play a role in protecting the bubbles. The technical problem of poor bubble stability of the concrete in a large fluidity state is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of engineering material preparation, and in particular relates to a concrete micro-foam air entraining agent. Background Art

[0002] Concrete is one of the important engineering materials. With the rapid development of concrete technology, the quality of concrete materials has been continuously improved. Micro-foam bubbles can improve the workability and fluidity of concrete, reduce non-measurement indicators such as water seepage, sedimentation and segregation of concrete, and are the main technical measures to cut off inherent defects such as capillary channels of concrete and improve the durability of concrete such as crack resistance, impermeability and frost resistance. Therefore, air entrainment technology is one of the important technical ways to improve the quality of concrete. At present, there are clear requirements for the addition of air-entraining agents in the design specifications for pumped concrete, hydraulic and port engineering concrete, and nuclear engineering concrete.

[0003] In recent years, polycarboxylate water-reducing agents have been widely used in concrete mixing. The concrete is in a state of high fluidity, resulting in poor bubble stability, easy migration and floating, forming large bubbles, and serious bubble rupture losses. Therefore, it is difficult to introduce high-quality micro-foam bubbles into concrete. This causes serious quality problems such as honeycomb surface, through cracks, and strength loss in the hardened concrete. Summary of the invention

[0004] The invention aims to provide a concrete micro-foam air entraining agent, wherein a concrete foam stabilizer is compounded in the ingredients, so that the bubble strength is improved and the bubbles are not easy to break. At the same time, the foam stabilizer can improve the viscosity and plasticity of the concrete, prevent the bubbles from floating and migrating, prevent the bubbles from connecting and merging, and protect the bubbles, thereby introducing a large number of evenly distributed micro-foam bubbles of 200-800 μm in the concrete mixing process.

[0005] In order to achieve the above object, the technical solution adopted by the present invention is: A concrete micro-foam air-entraining agent is composed of the following parts by weight: 8-10 parts of sodium fatty alcohol polyoxyethylene ether sulfate, 10-12 parts of sodium alpha-olefin sulfonate, 8-10 parts of maltodextrin, 10-12 parts of carboxymethyl starch and 60 parts of water.

[0006] Preferably, the concrete micro-foam air-entraining agent is composed of the following parts by weight: 9 parts of sodium fatty alcohol polyoxyethylene ether sulfate, 11 parts of sodium α-olefin sulfonate, 9 parts of maltodextrin, 11 parts of carboxymethyl starch, and 60 parts of water.

[0007] Preferably, the preparation method of the concrete micro-foam air-entraining agent comprises the following steps: adding water to sodium sulfate of fatty alcohol polyoxyethylene ether, sodium α-olefin sulfonate, maltodextrin, carboxymethyl starch and stirring for 100-120 minutes, and the concrete micro-foam air-entraining agent can be obtained after mixing evenly.

[0008] Preferably, when the air entraining agent is used, 3-5 kg ​​of concrete micro-foam air entraining agent is added to each ton of water-reducing agent product in the compounding stage of the water-reducing agent product.

[0009] Compared with the prior art, the beneficial effects of the present invention are: 1. The commercial concrete station is easy to use. In the compounding section of the water-reducing agent product, the water-reducing agent manufacturer will compound the air-entraining agent into the water-reducing agent product in an appropriate amount according to the requirements of the concrete air entrainment amount. When producing concrete, only the amount of water-reducing agent needs to be measured and added to the concrete, which reduces deviation errors.

[0010] 2. The main components of the air entraining agent and the water reducing agent are well compatible. The foam stabilizing components of the air entraining agent are maltodextrin and carboxymethyl starch, which are alkali-resistant and salt-resistant. Its solution has good dispersion, suspension, water retention, and anti-sedimentation effects. The solution viscosity is stable, thick but not sticky or thin. When compounded in the water reducing agent, it does not undergo adsorption, flocculation, separation, or precipitation with the water reducing agent. It has been widely used in the building materials industry and is often used as a cement slurry stabilizer and water retaining agent.

[0011] 3. The present invention aims at the technical problem that bubbles in high-fluidity concrete prepared with polycarboxylic acid water-reducing agent are easy to migrate and float, aggregate and collude to form inferior large bubbles, and cause serious rupture losses. This project studies the preparation of concrete air entraining agent and compounded concrete foam stabilizer, which increases the bubble strength and reduces the breakage rate. At the same time, the foam stabilizer can improve the viscosity and plasticity of concrete, prevent bubbles from floating and migrating, prevent bubbles from colluding and merging, and play a protective role on bubbles. It solves the technical problem of poor bubble stability of concrete in a high-fluidity state.

[0012] 4. The method of the present invention can introduce a proper amount of evenly distributed closed-cell micro-foam bubbles with a pore size range of 200-800 μm during the concrete mixing process. A proper amount of micro-foam bubbles can fill and block the pores in the concrete, thereby cutting off the connectivity of the capillary channels, reducing the through-pore defects inside the concrete, and effectively improving the durability of the concrete, such as impermeability, frost resistance, and resistance to salt ion erosion.

[0013] 5. The product of the method of the present invention has good performance, stable quality and broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 This is a scanning electron microscope photograph of a hardened concrete sample of the present invention. DETAILED DESCRIPTION

[0015] The specific implementation modes of the present invention are further described in detail below in conjunction with the accompanying drawings.

[0016] The raw materials and test methods in the embodiments of the present invention are as follows:

Raw materials for testing

[0017] Concrete raw materials: gravel, sand, cement PO42.5, fly ash, polycarboxylic acid high-performance water reducing agent.

[0018] in: Cement: P·O42.5 grade ordinary Portland cement; Stone: Crushed stone for construction, in accordance with the technical index requirements of GB / T 14685-2011 "Pebbles and Crushed Stones for Construction", with a nominal particle size of 5-32mm; Sand: Conforms to the medium sand index requirements specified in GB / T 14684-2011 "Construction Sand", with a fineness modulus of 3.1; Fly ash: The technical indicators meet the Class III requirements specified in GB / T 1596-2017 "Fly ash used in cement and concrete".

[0019]

Test method

[0020] 3-5kg of air entraining agent is added to each ton of water reducing agent. The expected air content of concrete is 3.0-5.0%, and the slump of concrete is controlled within the range of 210-230mm.

[0021] The concrete test is carried out according to the test method specified in GB / T 8076-2008 "Concrete Admixtures". The concrete mix ratio is: Cement: 400kg, gravel: 1000kg, sand: 850kg, fly ash: 50kg, water: 178kg, polycarboxylate water reducer dosage: 8.0kg.

[0022] Example 1 Concrete mix ratio: cement: 400kg, gravel: 1000kg, sand: 850kg, fly ash: 50kg, water: 178kg, polycarboxylate water reducer dosage: 8.0kg, add 3kg of micro foam air entraining agent per ton of water reducer. The ingredients and production method of the air entraining agent are 8 parts of AES, 12 parts of AOS, 8 parts of maltodextrin, 12 parts of carboxymethyl starch, 60 parts of water, add water and stir for 100 minutes.

[0023] Example 2 Concrete mix ratio: cement: 400kg, gravel: 1000kg, sand: 850kg, fly ash: 50kg, water: 178kg, polycarboxylate water reducer dosage: 8.0kg, add 4kg of microfoam air entraining agent per ton of water reducer. The ingredients and production method of the air entraining agent are 8 parts of AES, 12 parts of AOS, 8 parts of maltodextrin, 12 parts of carboxymethyl starch, 60 parts of water, add water and stir for 100 minutes.

[0024] Example 3 Concrete mix ratio: cement: 400kg, gravel: 1000kg, sand: 850kg, fly ash: 50kg, water: 178kg, polycarboxylate water reducer dosage: 8.0kg. 4kg of microfoam air entraining agent is added per ton of water reducer. The ingredients and production method of the air entraining agent are 10 parts of AES, 10 parts of AOS, 10 parts of maltodextrin, 10 parts of carboxymethyl starch, 60 parts of water, and stir for 110 minutes.

[0025] Example 4 Concrete mix ratio: cement: 400kg, gravel: 1000kg, sand: 850kg, fly ash: 50kg, water: 178kg, polycarboxylate water reducer dosage: 8.0kg. 5kg of microfoam air entraining agent is added per ton of water reducer. The ingredients and production method of the air entraining agent are 10 parts of AES, 10 parts of AOS, 10 parts of maltodextrin, 10 parts of carboxymethyl starch, 60 parts of water, and stir for 110 minutes.

[0026] Example 5 Concrete mix ratio: cement: 400kg, gravel: 1000kg, sand: 850kg, fly ash: 50kg, water: 178kg, polycarboxylate water reducer dosage: 8.0kg. Add 5kg of microfoam air entraining agent per ton of water reducer. The ingredients and production method of the air entraining agent are 9 parts of AES, 11 parts of AOS, 9 parts of maltodextrin, 11 parts of carboxymethyl starch, 60 parts of water, add water and stir for 120 minutes. Example 6 Concrete mix ratio: cement: 400kg, gravel: 1000kg, sand: 850kg, fly ash: 50kg, water: 178kg, polycarboxylate water reducer dosage: 8.0kg. Add 3kg of microfoam air entraining agent per ton of water reducer. The ingredients and production method of the air entraining agent are 9 parts of AES, 11 parts of AOS, 9 parts of maltodextrin, 11 parts of carboxymethyl starch, 60 parts of water, add water and stir for 120 minutes.

[0027] The concrete prepared by the method of the present invention was tested according to GB / T 8076-2008 "Concrete Admixtures". The test results are shown in Table 1.

[0028] Table 1: Test results of concrete technical indicators It can be seen from the test data in Table 1 that with the increase in the amount of air entraining agent, the air content of concrete increases steadily. This shows that the air entraining agent has a good foaming effect and can stably introduce an appropriate amount of micro-foam bubbles into the concrete, which is convenient for production control. This can solve the problems of poor foam stability of high-fluidity concrete in engineering production, easy floating and intermingling of bubbles after concrete pouring, resulting in uneven distribution of concrete binder, aggregate and bubbles in three dimensions, and honeycomb surface of concrete.

[0029] From the changes in concrete strength in Table 1, it can be seen that when the strength can increase or decrease steadily with the air content, it means that the size and distribution of the bubbles are uniform and stable. The foam introduced by the air-entraining agent is of good quality, which is convenient for the strength design of concrete with a specific air content.

[0030] Figure 1 It is the microscopic morphology of air-entrained concrete. Figure 1 It can be seen that there are no through-holes in the concrete section, the surface is not smooth, and there is no honeycomb phenomenon. The bubbles in the concrete are evenly distributed and of uniform size, and the diameter of the micro-foam bubbles is about 200-800μm. An appropriate amount of micro-foam bubbles can not only improve the workability and fluidity of concrete, but also fill and block the pores in the concrete, cut off the capillary channels, and reduce the through-holes inside the concrete, thereby effectively improving the durability of the concrete such as impermeability, frost resistance, and resistance to salt ion erosion.

Claims

1. A concrete micro-foam air-entraining agent, characterized in that The invention is composed of the following parts by weight: 8-10 parts of sodium fatty alcohol polyoxyethylene ether sulfate, 10-12 parts of sodium α-olefin sulfonate, 8-10 parts of maltodextrin, 10-12 parts of carboxymethyl starch and 60 parts of water.

2. A concrete micro-foam air-entraining agent according to claim 1, characterized in that The invention is composed of the following parts by weight: 9 parts of sodium fatty alcohol polyoxyethylene ether sulfate, 11 parts of sodium α-olefin sulfonate, 9 parts of maltodextrin, 11 parts of carboxymethyl starch and 60 parts of water.

3. A concrete micro-foam air-entraining agent according to claim 1 or 2, characterized in that The preparation method comprises the following steps: adding water to fatty alcohol polyoxyethylene ether sodium sulfate, alpha-olefin sodium sulfonate, maltodextrin and carboxymethyl starch and stirring for 100-120 minutes, and after uniform mixing, concrete micro-foam air entraining agent can be prepared.

4. A concrete micro-foam air-entraining agent according to claim 1 or 2, characterized in that: When the air entraining agent is used, 3-5 kg ​​of concrete micro-foam air entraining agent is added to each ton of water-reducing agent product in the compounding process of the water-reducing agent product.

Citation Information

Cited By

  • Microcapsule concrete with temperature control and anti-freezing dual functions and preparation method thereof

    CN122916537A