CO2 curing prefabricated regenerated inverted filter layer and preparation method thereof
Through the CO2 curing method of prefabricated recycled inverted filter layer, combined with recycled aggregate and spinel carbon cementitious material, the problem of poor mechanical properties and durability of the inverted filter layer is solved, and efficient and environmentally friendly inverted filter layer production is achieved, improving the production of inverted filter layer. The compressive strength and durability solve the problem of industrial exhaust gas and construction waste utilization.
Patent Information
- Application Number
- CN202410940505.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-11-22
AI Technical Summary
The existing regenerated inverted filter layer has poor mechanical properties, durability and volume stability, which leads to low compressive strength, blocked slurry sinking and poor durability in actual applications, which limits its construction in sponge cities. Application.
The prefabricated regenerated backfilter layer method is adopted by using 50 to 80 parts of regenerated aggregate, 5 to 15 parts of regenerated sand, 35 to 65 parts of cement, 10 to 30 parts of water, and 0.05 to 2 parts of polycarboxylic acid water reducing agent , 0 to 0.05 parts of cellulose ether and 0 to 0.02 parts of sodium polyacrylate, combined with spinel carbon cementitious material and industrial solid waste, high-temperature calcination and CO2 curing are carried out to improve the strength and durability of the inverted filter layer.
It significantly improves the compressive strength and durability of the backfilter layer, reduces energy consumption, effectively utilizes industrial exhaust gas and construction waste, realizes efficient and environmentally friendly backfilter layer production, and solves the problems of industrial exhaust gas emissions and construction waste storage .
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to a CO2-cured prefabricated regenerated filter layer and a preparation method thereof, belonging to the technical field of preparation of carbon-fixing gelling materials. Background Art
[0002] Permeable concrete is an important pavement material for my country's sponge city construction. In the past decade, research on permeable concrete has become increasingly in-depth. Regenerated filter layer is a type of permeable concrete that can not only improve surface runoff conditions but also absorb CO2 in the air to achieve carbon sequestration.
[0003] The inverted filter layer is a concrete product that allows water to pass easily. It is usually composed of cement, coarse aggregate, a small amount of fine sand, water and admixtures. The road surface paved with the inverted filter layer can reduce rainwater runoff, increase groundwater and alleviate urban waterlogging. However, it also has disadvantages such as low compressive strength, slurry sinking and blockage, and poor durability, which greatly affect the practical application of the inverted filter layer. Therefore, preventing slurry from sinking and blockage during construction and improving strength and durability have become the key research directions of the inverted filter layer. The regenerated inverted filter layer is a type of permeable concrete. Its main feature is that the components of the coarse aggregate and fine sand used to prepare the inverted filter layer are all recycled coarse aggregate and recycled sand, which reduces energy consumption.
[0004] At present, the defects of recycled aggregate in the filter layer affect the interface transition zone and pore structure of the recycled aggregate in the system. Such microstructural defects lead to poor mechanical properties, durability, volume stability, etc. of the filter layer containing recycled aggregate, thus limiting the application of recycled aggregate. Summary of the invention
[0005] In view of the problems existing in the prior art, the present invention provides a CO2-cured prefabricated regenerated filter layer, which can consume a large amount of steel slag, ferrochrome slag, fluorite tailings, blast furnace slag and CO2, effectively solving the problems of industrial exhaust gas emissions and construction waste storage.
[0006] The present invention also provides a method for preparing the above-mentioned CO2-cured prefabricated regenerated filter layer, which solves the problems of slow strength growth, low strength and poor durability during the curing process of the filter layer, and the method has strong controllability.
[0007] The technical solution adopted by the present invention to achieve the above-mentioned purpose is: The present invention provides a CO2-cured prefabricated regenerated filter layer, comprising the following raw materials in parts by weight: 50 to 80 parts of recycled aggregate, 5 to 15 parts of recycled sand, 35 to 65 parts of binder, 10 to 30 parts of water, 0.05 to 2 parts of polycarboxylic acid water reducer, 0 to 0.05 parts of cellulose ether and 0 to 0.02 parts of sodium polyacrylate.
[0008] Furthermore, the particle size of the recycled aggregate is 5 to 15 mm, which is a coarse aggregate for crushing recycled building concrete; the particle size of the recycled sand is 0.3 to 0.5 mm, which is a fine aggregate for crushing recycled building concrete.
[0009] Furthermore, the binder is composed of the following raw materials in parts by weight: 20-30 parts of ordinary Portland cement and 15-35 parts of spinel carbon-fixing cementitious material.
[0010] Furthermore, the mass fractions of the mineral phase composition of the spinel carbon-fixing cementitious material are: 45-60% C2SF, 10-20% C2S, 5-15% C3S2, 5-12% C4AF and 6-10% CMS.
[0011] Furthermore, the raw materials required for the spinel carbon-fixing cementitious material system are conventional steel slag, ferrochrome slag, fluorite tailings and blast furnace slag; its oxide composition is: 40-58% CaO, 25-43% SiO2, 2-6% Fe2O3, 2-5% MgO and 2-4% Al2O3, and contains 10-13% CaF2; the C2S is composed of γ-C2S and β-C2S, among which the content of β-C2S is 50-65%.
[0012] Furthermore, the spinel carbon fixation system needs to be doped with 0.5-2.0% fluorine-sulfur composite mineralizer; the F / SO3 ratio of the fluorine-sulfur composite mineralizer is 0.100-0.691; most preferably, the F / SO3 ratio of the fluorine-sulfur composite mineralizer is 0.45.
[0013] The preparation method of the spinel carbon-fixing cementitious material used in the present invention is: 1) Grind steel slag, ferrochrome slag, fluorite tailings and blast furnace slag in a ball mill, pass through a 200-mesh sieve, and the sieve residue is less than 5% to obtain a mixed raw material; 2) Fully ball-milling and mixing the sieved mixed raw materials and the fluorine-sulfur composite mineralizer; 3) The ball-milled material is mixed evenly with anhydrous ethanol and pressed into a shape to obtain a raw material body; 4) drying the pressed green body and then calcining it at high temperature; 5) After calcination, air cool the mixture.
[0014] Furthermore, the ball milling speed is 250r / min, and the ball milling time is 2h; the water-solid ratio of the material to anhydrous ethanol is 0.15; the molding pressure of the raw material body is 20-50MPa; the high-temperature calcination is carried out at a heating rate of 10℃ / min, the temperature is increased to 1100-1250℃, and the calcination holding time is 6-8h.
[0015] The present invention also provides a method for preparing the above-mentioned CO2-cured prefabricated regenerated filter layer, comprising the following steps: (1) The absolutely dry recycled aggregate absorbs water to reach saturated surface dryness; weigh recycled aggregate, recycled sand and 60% water in proportion and add them into the mixer, stirring for 60s to 120s; (2) Add the binder and continue stirring for 60s to 180s; add the remaining 40% water, polycarboxylate water reducer, cellulose ether and sodium polyacrylate and stir for 60s to 180s; (3) Vibrate the stirred material to remove bubbles and make the interior dense, then perform CO2 curing and demold after curing.
[0016] Furthermore, the CO2 curing process is: at a relative humidity of 50±10%, CO2 curing is constant at 0.2-0.3MPa, and curing is performed for 10-24h.
[0017] The strength of the regenerated filter layer product made by the CO2 curing technology of the present invention increases rapidly, and the efficiency is better than steam curing. In addition, the mineralization effect of CO2 on concrete further optimizes the use of the filter layer. The filter layer has a large porosity, CO2 gas can easily penetrate, and the slurry surrounding the aggregate is thin, which can achieve full carbonization in a short time.
[0018] The present invention utilizes CO2 to maintain the prefabricated regenerated filter layer, thereby solving the problems of low compressive strength and slow strength growth of the filter layer, and providing an efficient and environmentally friendly method for producing the filter layer. At the same time, the binder used in preparing the regenerated filter layer is fired from industrial solid waste, which not only consumes part of the construction waste and absorbs CO2 in the industrial tail gas, but also the reaction products are mainly carbonates and silica gel, which can improve the strength. Since the aggregate itself is a recycled aggregate with certain hydration and carbonization properties, the strength of the filter layer is greatly improved under the dual effects. The present invention provides an effective technical approach to solving industrial solid waste and reducing CO2 in the atmosphere.
[0019] The beneficial effects of the present invention are: 1. The filter layer prepared by the present invention has a high porosity. As an important building material for sponge city construction, it can play an important role in controlling storm runoff, strengthening water resource utilization, and reducing road surface waterlogging. The present invention uses CO2 to maintain the prefabricated regenerated filter layer. The high porosity of the filter layer is reasonably utilized in that CO2 can easily enter between aggregates, improve the carbonization efficiency, and enable the filter layer to reach a higher degree of carbonization in a shorter period of time. The strength is rapidly improved, and the production efficiency is greatly improved. At the same time, compared with traditional steam maintenance, the use of CO2 for the maintenance of the prefabricated regenerated filter layer consumes a large amount of CO2, reduces the energy consumption in the preparation process of the filter layer, and provides an effective way to reduce industrial tail gas.
[0020] 2. The present invention uses blast furnace slag and ferrochrome slag as main raw materials, and the carbon-fixing cementitious material composed of spinel C2SF, C2S, C3S2 and CMS is prepared. The reaction products are calcium carbonate, magnesium carbonate and silica gel under CO2 curing, so that the slurry is well wrapped on the aggregate surface, further improving the strength of the inverted filter layer; the wear resistance is poor, which is conducive to enhancing the wear resistance of the inverted filter layer; The performance of the recycled aggregate itself is not outstanding, but the present invention improves its performance during the CO2 curing process, allowing it to continue to carbonize, thereby achieving the effect of directly strengthening the recycled aggregate. The present invention can consume a large amount of industrial solid waste and effectively solve the problem of large accumulation of construction waste.
[0021] 3. The present invention adopts a combination of polycarboxylic acid water-reducing agent, cellulose ether and sodium polyacrylate to effectively improve the viscosity of concrete, so that the slurry has good fluidity and can be well hung on the surface of recycled aggregate, avoiding the problem of slurry sinking and clogging during construction; the inverted filter layer provided by the present invention, under the synergistic effect of various raw materials, can obtain high-strength and high-durability recycled inverted filter layer concrete products, which is an environmentally friendly and sustainable building material. DETAILED DESCRIPTION
[0022] The technical solution of the present invention is further explained and illustrated by means of specific embodiments below.
[0023] The present invention utilizes a CO2-cured prefabricated regenerated filter layer prepared from blast furnace slag, ferrochrome slag and recycled aggregate, wherein the regenerated filter layer is composed of the following parts by weight: 50 to 80 parts of recycled aggregate, 5 to 15 parts of regenerated sand, 35 to 65 parts of binder, 10 to 30 parts of water, 0.05 to 2 parts of polycarboxylic acid water reducer, 0 to 0.05 parts of cellulose ether and 0 to 0.02 parts of sodium polyacrylate.
[0024] The binder is composed of the following parts by weight: 20-30 parts of ordinary Portland cement and 15-35 parts of spinel carbon-fixing cementitious material.
[0025] The particle size of the recycled aggregate is between 5 and 15 mm, and it is the coarse aggregate of crushed building recycled concrete; The particle size of the regenerated sand is between 0.3 and 0.5 mm, and it is fine aggregate for crushing construction recycled concrete.
[0026] In the CO2-cured prefabricated filter layer, the spinel is calcium-silicon-fluoride spinel, which is a carbon-fixing cementitious material. The oxide composition of the spinel carbon-fixing cementitious material is: 40-58% CaO, 25-43% SiO2, 2-6% Fe2O3, 2-5% MgO and 2-4% Al2O3, and contains 10-13% CaF2.
[0027] The raw materials required for the spinel carbon-fixing cementitious material system are conventional steel slag, ferrochrome slag, fluorite tailings and blast furnace slag; its oxide composition is: 40-58% CaO, 25-43% SiO2, 2-6% Fe2O3, 2-5% MgO and 2-4% Al2O3, and contains 10-13% CaF2.
[0028] The C2S consists of γ-C2S and β-C2S, wherein the content of β-C2S is 50-65%.
[0029] In the following embodiments, the mineral phase composition mass fraction of the spinel carbon-fixing cementitious material used is: 55% C2SF (fluorine-containing spinel), 15% C2S, 10% C3S2, 5% C4AF and 10% CMS; it is prepared according to the mass ratio of steel slag, ferrochrome slag, fluorite tailings and blast furnace slag of 2:1:1:1.
[0030] Example 1 The preparation of the prefabricated regenerated filter layer cured by CO2 is composed of the following components by weight: Table 1 Composition by weight of Example 1 The preparation method comprises the following steps: 1) The absolutely dry recycled aggregate absorbs water to reach saturated surface dryness; weigh the recycled aggregate, recycled sand and 60% water in proportion and add them into the mixer, stirring for 30 seconds; 2) Add the binder and continue stirring for 150 seconds; add the remaining 40% water, polycarboxylate water reducer, cellulose ether and sodium polyacrylate and stir for 120 seconds; 3) Pour the mixed material into the mold, place it on a vibration table, vibrate out the bubbles to make the inside dense, then put it into a curing room or curing box and pass CO2 to keep the environment in the curing room or curing box at a relative humidity of 60% and a constant CO2 of 0.3MPa. Curing for 12 hours; demoulding can be completed after curing.
[0031] Example 2 The preparation of the prefabricated regenerated filter layer cured by CO2 is composed of the following components by weight: Table 2 Composition of Example 2 by weight The preparation method comprises the following steps: 1) The absolutely dry recycled aggregate absorbs water to reach saturated surface dryness; weigh the recycled aggregate, recycled sand and 60% water in proportion and add them into the mixer, stir for 60 seconds; add the binder and continue stirring for 120 seconds; 2) Add the remaining 40% water, polycarboxylate water reducer, cellulose ether and sodium polyacrylate, and stir for 60 seconds; 3) Pour the mixed material into the mold, place it on a vibration table, vibrate out the bubbles to make the inside dense, then put it into a curing room or curing box and pass CO2 to keep the environment in the curing room or curing box at a relative humidity of 50% at all times, and the CO2 curing is constant at 0.3MPa for 12 hours; demold after the curing is completed.
[0032] Example 3 The preparation of the prefabricated regenerated filter layer cured by CO2 is composed of the following components by weight: Table 3 Composition of Example 3 by weight The preparation method comprises the following steps: 1) The absolutely dry recycled aggregate absorbs water to reach saturated surface dryness; weigh the recycled aggregate, recycled sand and 60% water in proportion and add them into the mixer, stirring for 60 seconds; 2) Add the binder and continue stirring for 120 seconds; add the remaining 40% water, polycarboxylate water reducer, cellulose ether and sodium polyacrylate and stir for 120 seconds; 3) Pour the mixed material into the mold, place it on a vibration table, vibrate out the bubbles to make the inside dense, then put it into a curing room or curing box and pass CO2 to keep the environment in the curing room or curing box at a relative humidity of 50% at all times, CO2 curing at a constant 0.3MPa, and curing for 12 hours; demoulding can be completed after curing.
[0033] Effect Example The test was carried out with reference to GB / T50080-2016 "Standard for Test Methods of Ordinary Concrete Mixture Performance", GB / T50081 "Standard for Test Methods of Physical and Mechanical Properties of Concrete", GB / T50082 "Test Methods for Long-term Performance and Durability of Ordinary Concrete" and JC / T2550-2020 "Standard for Permeable Concrete". The effects of the samples prepared in the embodiment are shown in Table 4, which shows that the inverted filter layer prepared by the present invention has high strength, good wear resistance and good water permeability.
[0034] Table 4 The present invention adopts CO2 for curing during the preparation process. Compared with the traditional high-temperature and high-pressure energy-consuming curing method, it not only reduces the energy consumption and production cost during the curing process, but also accelerates the strength growth of the filter layer, saves preparation time, and improves production efficiency. The binder used in the preparation process of the present invention belongs to a carbon-fixing cementitious material. The preparation process uses a large amount of steel slag, ferrochrome slag, fluorite tailings and blast furnace slag, effectively utilizes industrial solid waste, and utilizes CO2 in industrial tail gas, which is an environmentally friendly and efficient building material.
Claims
1. A CO2-cured prefabricated regenerated filter layer, characterized in that: The invention comprises the following raw materials in parts by weight: 50 to 80 parts of recycled aggregate, 5 to 15 parts of recycled sand, 35 to 65 parts of binder, 10 to 30 parts of water, 0.05 to 2 parts of polycarboxylic acid water reducing agent, 0 to 0.05 parts of cellulose ether and 0 to 0.02 parts of sodium polyacrylate.
2. The CO2-cured prefabricated regenerated filter layer according to claim 1, characterized in that: The particle size of the recycled aggregate is 5-15 mm, which is the coarse aggregate for crushing recycled concrete for construction; the particle size of the recycled sand is 0.3-0.5 mm, which is the fine aggregate for crushing recycled concrete for construction.
3. The CO2-cured prefabricated regenerated filter layer according to claim 1 or 2, characterized in that: The binder is composed of the following raw materials in parts by weight: 20-30 parts of ordinary Portland cement and 15-35 parts of spinel carbon-fixing cementitious material.
4. The CO2-cured prefabricated regenerated filter layer according to claim 3, characterized in that: The mass fractions of the mineral phase composition of the spinel carbon-fixing cementitious material are: 45-60% C2SF, 10-20% C2S, 5-15% C3S2, 5-12% C4AF and 6-10% CMS.
5. The CO2-cured prefabricated regenerated filter layer according to claim 4, characterized in that: The raw materials required for the spinel carbon-fixing cementitious material system are conventional steel slag, ferrochrome slag, fluorite tailings and blast furnace slag; its oxide composition is: 40-58% CaO, 25-43% SiO2, 2-6% Fe2O3, 2-5% MgO and 2-4% Al2O3, and contains 10-13% CaF2; the C2S is composed of γ-C2S and β-C2S, among which the content of β-C2S is 50-65%.
6. The CO2-cured prefabricated regenerated filter layer according to claim 5, characterized in that: The spinel carbon fixation system needs to be doped with 0.5-2.0% fluorine-sulfur composite mineralizer; the F / SO3 ratio of the fluorine-sulfur composite mineralizer is 0.100-0.691; most preferably, the F / SO3 ratio of the fluorine-sulfur composite mineralizer is 0.
45.
7. The CO2-cured prefabricated regenerated filter layer according to any one of claims 3 to 6, characterized in that: The preparation method of the spinel carbon-fixing cementitious material is as follows: 1) Grind steel slag, ferrochrome slag, fluorite tailings and blast furnace slag in a ball mill, pass through a 200-mesh sieve, and the sieve residue is less than 5% to obtain a mixed raw material; 2) Fully ball-milling and mixing the sieved mixed raw materials and the fluorine-sulfur composite mineralizer; 3) The ball-milled material is mixed evenly with anhydrous ethanol and pressed into a shape to obtain a raw material body; 4) drying the pressed green body and then calcining it at high temperature; 5) After calcination, air cool the mixture.
8. The CO2-cured prefabricated regenerated filter layer according to claim 7, characterized in that: The ball mill has a rotation speed of 250 r / min and a ball milling time of 2 h; the water-solid ratio of the material to anhydrous ethanol is 0.15; the molding pressure of the raw material body is 20-50 MPa; the high-temperature calcination is carried out at a heating rate of 10 °C / min, the temperature is increased to 1100-1250 °C, and the calcination holding time is 6-8 h.
9. A method for preparing a CO2-cured prefabricated regenerated filter layer as claimed in any one of claims 1 to 8, characterized in that: The following steps are involved: (1) The absolutely dry recycled aggregate absorbs water to reach saturated surface dryness; weigh recycled aggregate, recycled sand and 60% water in proportion and add them into the mixer, stirring for 60s to 120s; (2) Add the binder and continue stirring for 60s to 180s; add the remaining 40% water, polycarboxylate water reducer, cellulose ether and sodium polyacrylate and stir for 60s to 180s; (3) Vibrate the stirred material to remove bubbles and make the interior dense, then perform CO2 curing and demold after curing.
10. The preparation method according to claim 9, characterized in that: The CO2 curing process is: at a relative humidity of 50±10%, CO2 curing is constant at 0.2-0.3MPa, and curing is performed for 10-24h.