Toughened ceramic and preparation method thereof
The glass phase is generated by loading silicon carbide whiskers and sodium nitride with silicon micropowder, which solves the problem of poor cracking and toughening effects of ceramic materials during firing, and achieves uniform toughening and high-temperature stability of ceramic materials Sex improvement.
Patent Information
- Application Number
- CN202310552892.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-17
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2043-05-17
AI Technical Summary
Ceramic materials are prone to cracking during firing. In the existing reinforcement and toughening methods, whiskers are prone to agglomeration, resulting in uneven distribution and poor toughening effect.
Silicon micropowder is used to load silicon carbide whiskers, and the adsorption capacity of silicon micropowder is improved through hydrochloric acid treatment, reducing whisker agglomeration, combining sodium nitride and phosphorus tailings to generate glass phases, enhancing the toughness and creep resistance of ceramics.
It achieves uniform toughening of ceramic materials, reduces cracking, improves bending strength and high temperature stability, and enhances the overall performance of ceramics.
Smart Images

Figure BDA0004231952700000041 
Figure BDA0004231952700000042 
Figure BDA0004231952700000051
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of ceramics, and more specifically, to a toughened ceramic and a preparation method thereof. Background Art
[0002] Ceramics are mostly used as structural materials, and have the characteristics of high melting point, high hardness and high wear resistance. However, ceramics are also very brittle, which leads to cracking during the firing process. The use of ceramic strengthening and toughening methods can reduce the cracking of ceramics and improve their brittleness problem.
[0003] At present, the existing ceramic strengthening and toughening methods are to greatly improve the mechanical properties of ceramic materials through phase change, fiber or whisker reinforcement, ultrafine powder, dispersion strengthening particles and other physical and chemical methods to obtain ceramics with uniform structure and strong performance.
[0004] With respect to the above-mentioned related technologies, the inventors believe that when adding whiskers to ceramic clay to toughen ceramics, the whiskers are prone to agglomeration, resulting in uneven distribution in the ceramic clay, leading to poor toughening effect. Summary of the invention
[0005] In order to improve the toughening effect of toughened ceramics, the present application provides a toughened ceramic and a preparation method thereof.
[0006] In a first aspect, the present application provides a toughened ceramic, using the following technical solution: A toughened ceramic comprises a ceramic body and a glaze layer, wherein the ceramic body comprises the following raw materials in parts by weight: Ceramic clay: 1-3 parts of wollastonite, 5-10 parts of porcelain powder, 13-17 parts of feldspar, 10-15 parts of ball clay, 5-8 parts of dolomite, 100-120 parts of Zhangcun soil; Silicon powder loaded with 50-60 parts of silicon carbide whiskers, 150-200 parts of water.
[0007] By adopting the above technical solution, silicon carbide whiskers loaded with silicon powder are added to the ceramic body as a toughening component to improve the toughness of the ceramic body. Silicon carbide has a high silicon content, and a continuous and dense glass phase with a certain fluidity can be generated during the firing process of the ceramic system to fill and bond cracks, thereby reducing the occurrence of ceramic cracking. Silicon micropowder has good adsorption capacity, which is conducive to loading silicon carbide whiskers on silicon micropowder. On the one hand, it can reduce the problem of mutual entanglement and agglomeration of silicon carbide whiskers, so that silicon carbide whiskers can be evenly dispersed in the ceramic mud; on the other hand, during the high-temperature firing process, the presence of silicon micropowder can reduce the damage to silicon carbide whiskers caused by firing and enhance the interface bonding between silicon carbide whiskers and the ceramic matrix.
[0008] Preferably, the silicon micropowder loaded silicon carbide whiskers comprises the following preparation steps: A1. Immerse the silicon micropowder in a 2-4 mol / L hydrochloric acid solution for 1-2 hours, wherein the weight ratio of the silicon micropowder to the hydrochloric acid solution is 1:(1-2); A2. Add silicon carbide whiskers and disperse them ultrasonically for 10-15 minutes. The mass ratio of silicon carbide whiskers to silicon micropowder is (1-1.5):1 to obtain silicon micropowder-loaded silicon carbide whiskers.
[0009] By adopting the above technical solution, after the silicon micropowder is acidified with hydrochloric acid, the specific surface area of the silicon micropowder can be increased, the adsorption capacity of the silicon micropowder to the silicon carbide whiskers can be enhanced, and the silicon carbide whiskers can be stably loaded on the silicon micropowder.
[0010] Preferably, the particle size of the silicon carbide whiskers loaded with silicon powder is 10-30 microns.
[0011] By adopting the above technical solution, when the particle size of silicon carbide whiskers loaded with silicon micropowder is in the range of 10-30 microns, it can be better dispersed in the ceramic mud, and can fully exert the toughening effect during the firing process to reduce the cracking of the ceramic.
[0012] Preferably, 2-5 parts of a surfactant are also added to the raw material, and the surfactant is ethoxylated sodium alkyl sulfate.
[0013] By adopting the above technical solution, ethoxylated alkyl sodium sulfate is used as a surfactant, which is easily soluble in water, can reduce the friction between ceramic mud materials, make the ceramic mud particles have good fluidity, and enhance the dispersion effect of the toughening component.
[0014] Preferably, 30-50 parts of sodium nitride are also added to the raw materials of the ceramic body.
[0015] By adopting the above technical scheme, sodium nitride is mixed into the ceramic slurry. When sodium nitride is mixed with the water in the ceramic slurry, a large amount of heat is released. The heat generated by the reaction of sodium nitride with water helps to improve the bonding degree between the silicon micropowder-loaded silicon carbide whiskers and the ceramic mud. In addition, the reaction of sodium nitride with water will produce sodium hydroxide. Sodium hydroxide cannot play a toughening effect, but can promote the toughening effect of the toughening substance. This is because sodium hydroxide is sintered together with silicon micropowder, which can break the silicon-oxygen bonds in the silicon micropowder, thereby releasing silicon dioxide, increasing the viscosity of the glass phase in the ceramic system, thereby increasing the creep resistance of the silicon carbide whiskers, and further improving the toughening effect of the ceramic.
[0016] In addition, since the surface of the silicon micropowder is treated with hydrochloric acid, during the preparation of the ceramic slurry, the hydrochloric acid remaining on the surface of the silicon micropowder can react with part of the sodium nitride to produce sodium chloride. Sodium chloride, as an electrolyte, can increase the viscosity of the ethoxylated alkyl sodium sulfate solution, so that the ceramic slurry can be quickly formed during the forming process, and it is not easy to cause the slurry viscosity to decrease due to the increase in temperature, resulting in poor forming effect.
[0017] Preferably, 20-30 parts of phosphate tailings are also added to the ceramic mud.
[0018] By adopting the above technical scheme, the phosphate tailings contain relatively high levels of silicon dioxide and calcium oxide. The sodium hydroxide generated by the reaction of sodium nitride and water provides an alkaline environment, which can also promote the release of silicon dioxide in the phosphate tailings. During the high-temperature firing process, the phosphate tailings react with calcium oxide and other oxides in the ceramic mud to form a glass phase, which further increases the viscosity of the glass phase, improves the high-temperature creep resistance of the silicon carbide whiskers, and thereby enhances its toughening effect.
[0019] In a second aspect, the present application provides a method for preparing toughened ceramics, using the following technical solution: A method for preparing toughened ceramics comprises the following steps: S1, mixing ceramic mud, silicon carbide whiskers loaded with silicon powder, surfactant and water by ball milling to obtain slurry; S2, injecting the slurry into a gypsum mold to obtain a ceramic green body by slip injection molding; S3, sintering the ceramic green body to obtain a ceramic green body, glazing the ceramic green body and firing it again to obtain a toughened ceramic.
[0020] By adopting the above technical solution, silicon micropowder loaded with silicon carbide whiskers as toughening components are added to ceramic mud, which can reduce the problem of simple silicon carbide whiskers being easy to agglomerate and poorly dispersed. In addition, the presence of silicon micropowder can protect the silicon carbide whiskers from being easily damaged during the firing process, thereby improving the toughening effect.
[0021] Preferably, when sodium nitride is further added to the raw material of the ceramic body, the preparation method thereof comprises the following steps: S1, mixing ceramic mud, silicon micropowder loaded silicon carbide whiskers, surfactant and water by ball milling, and then adding sodium nitride and mixing to obtain mud; S2, injecting the slurry into a gypsum mold to obtain a ceramic green body by slip injection molding; S3, drying, glazing and firing the ceramic green body to obtain toughened ceramic.
[0022] By adopting the above technical solution, sodium nitride is mixed before grouting molding, and a part of the sodium nitride reacts with water to generate a large amount of heat, so that the ceramic mud can have a certain molding temperature without additional heating during the grouting molding process, which helps to shorten the molding time; and the generation of heat also provides reaction conditions for the other part of the sodium nitride to react with hydrochloric acid. Sodium nitride reacts with the hydrochloric acid remaining on the silicon micropowder to generate sodium chloride. Sodium chloride can increase the viscosity of the surfactant, which is beneficial to the molding of ceramics and makes the ceramics less likely to crack during the grouting molding process.
[0023] In summary, this application has the following beneficial effects: 1. Since the present application uses silicon micropowder to load silicon carbide whiskers, on the one hand, it can reduce the problem of mutual entanglement and agglomeration of silicon carbide whiskers, so that the silicon carbide whiskers can be evenly dispersed in the ceramic mud; on the other hand, during the high-temperature firing process, the presence of silicon micropowder can reduce the damage to the silicon carbide whiskers caused by firing and enhance the interface bonding between the silicon carbide whiskers and the ceramic matrix.
[0024] 2. In the present application, sodium nitride is preferably used. Sodium nitride is mixed into the ceramic slurry. Sodium nitride reacts with water to produce sodium hydroxide. Sodium hydroxide cannot play a toughening effect, but can promote the toughening effect of the toughening substance. This is because sodium hydroxide is sintered together with silicon micropowder, which can break the silicon-oxygen bonds in the silicon micropowder, thereby releasing silicon dioxide, increasing the viscosity of the glass phase in the ceramic system, thereby increasing the creep resistance of the silicon carbide whiskers, and further improving the toughening effect of the ceramic.
[0025] 3. The method of the present application comprises the following steps: firstly, ceramic mud, silicon micropowder loaded with silicon carbide whiskers, surfactant and water are ball-milled and mixed, and then sodium nitride is added and mixed to obtain mud; the mud is then injected into a gypsum mold, and a ceramic green body is obtained by slip injection molding; finally, the ceramic green body is subjected to high-temperature sintering, glazing and re-firing to obtain a toughened ceramic, which is beneficial to the molding of the ceramic and makes the ceramic less likely to crack during the slip injection molding process. DETAILED DESCRIPTION
[0026] Source of raw materials: The raw materials of the examples and comparative examples of the present application can all be obtained commercially.
[0027] The chemical composition of phosphate tailings is as follows: The chemical composition of raw materials such as ceramic clay and glaze is as follows: Example
[0028] Examples 1A-1C A toughened ceramic comprises a ceramic body and a glaze layer, wherein the ceramic body comprises the following raw materials: Ceramic mud: wollastonite 1-3kg, porcelain powder 5-10kg, feldspar 13-17kg, ball clay 10-15kg, dolomite 5-8kg, Zhangcun soil 100-120kg; Silicon powder loaded with 50-60kg of silicon carbide whiskers, with a particle size of 20 microns; 150-200kg of water.
[0029] The method for preparing silicon carbide whiskers loaded with silicon powder comprises the following steps: A1. Soak the silicon micropowder in 3 mol / L hydrochloric acid solution for 1.5 h, with the weight ratio of silicon micropowder to hydrochloric acid solution being 1:1.5; A2, adding silicon carbide whiskers, ultrasonically dispersing for 15 minutes, the mass ratio of silicon carbide whiskers to silicon micropowder is 1:1, and silicon micropowder-loaded silicon carbide whiskers are obtained; A method for preparing toughened ceramics comprises the following steps: S1, mixing ceramic mud, silicon carbide whiskers loaded with silicon powder, surfactant and water after ball milling for 12 hours to obtain mud; S2, injecting the slurry into a gypsum mold to obtain a ceramic green body by slip injection molding; S3. Dry the ceramic green body for 12 hours, apply glaze after drying, the thickness of the glaze layer is 3 mm, and then fire the green body at a temperature of 1300° C. for 18 hours to finally obtain toughened ceramics.
[0030] The ceramic glaze is prepared by mixing 22 kg of solvent powder, 22 kg of feldspar, 7 kg of wollastonite, 8 kg of calcite, 3 kg of dolomite, 3 kg of burnt zinc oxide, 2 kg of burnt aluminum oxide, 1 kg of frit and 35 kg of water.
[0031] The amounts of raw materials used for the ceramic bodies of Examples 1A-1C are shown in Table 1.
[0032] Table 1 Amount of raw materials used for ceramic bodies of Examples 1A-1C (unit: kg) Examples 2A-2D A toughened ceramic, which is different from Example 1B in that the particle sizes of silicon carbide whiskers loaded by silicon micropowder are different.
[0033] The particle size of the silicon carbide whiskers loaded with silicon powder in Example 2A is 10 μm; The particle size of the silicon carbide whiskers loaded with silicon powder in Example 2B is 30 μm; The particle size of the silicon carbide whiskers loaded with silicon powder in Example 2C is 5 μm; The particle size of the silicon carbide whiskers loaded with silicon powder in Example 2D is 50 μm; Examples 3A-3C A toughened ceramic, which is different from Example 1B in that 2-5 kg of a surfactant is also added to the raw material of the ceramic body, and the surfactant is ethoxylated sodium alkyl sulfate; Wherein, the amount of surfactant used in Example 3A is 2 kg; The amount of surfactant used in Example 3B is 3.5 kg; The amount of surfactant used in Example 3C is 5 kg.
[0034] Examples 4A-4C A toughened ceramic, which is different from Example 3A in that 30-50 kg of sodium nitride is also added to the raw material of the ceramic body. When sodium nitride is also added to the raw material, the preparation method thereof comprises the following steps: S1, mixing ceramic mud, silicon carbide whiskers loaded with silicon powder, surfactant and water by ball milling, and then adding sodium nitride to obtain slurry; S2, injecting the slurry into a gypsum mold to obtain a ceramic green body by slip injection molding; S3. Dry the ceramic green body for 12 hours, apply glaze after drying, the thickness of the glaze layer is 3 mm, and then fire the green body at a temperature of 1300° C. for 18 hours to finally obtain toughened ceramics.
[0035] Wherein, the amount of sodium nitride used in Example 4A is 30 kg; The amount of sodium nitride used in Example 4B is 40 kg; The amount of sodium nitride used in Example 4C is 50 kg.
[0036] Examples 5A-5C A toughened ceramic, which is different from Example 4A in that 20-30 kg of phosphorus tailings are also added to the ceramic mud.
[0037] Wherein, the amount of phosphate tailings used in Example 5A is 20 kg; The amount of phosphate tailings used in Example 5B is 25 kg; The amount of phosphate tailings used in Example 5C is 30 kg.
[0038] Example 6 A toughened ceramic, which differs from Example 4B in that an equal amount of aluminum nitride is used to replace sodium nitride.
[0039] Example 7 A toughened ceramic, which is different from Example 4B in that sodium nitride is directly added to the ceramic mud for mixing.
[0040] Comparative Example Comparative Example 1 A toughened ceramic, which is different from Example 1B in that the amount of silicon carbide whiskers loaded with silicon powder is 0 kg.
[0041] Comparative Example 2 A toughened ceramic, which is different from Example 1B in that the silicon carbide whiskers loaded on silicon powder are replaced by an equal amount of silicon carbide whiskers.
[0042] Performance testing The tests include: 1. Bending strength test The test was carried out according to the method specified in GB / T 4741-1999 “Test method for flexural strength of ceramic materials”.
[0043] The test results are shown in Table 2. Table 2 Test results of Examples 1-7 and Comparative Examples 1-2 It can be seen from the combination of Examples 1A-1C and Comparative Examples 1-2 and Table 2 that the toughened ceramics of Examples 1A-1C have better bending strength, indicating that the present application loads the silicon carbide whiskers on silicon micropowder. On the one hand, it can reduce the problem of mutual entanglement and agglomeration of silicon carbide whiskers, so that the silicon carbide whiskers can be evenly dispersed in the ceramic mud; on the other hand, during the high-temperature firing process, the presence of silicon micropowder can reduce the damage to the silicon carbide whiskers caused by firing, and enhance the interface bonding between the silicon carbide whiskers and the ceramic matrix.
[0044] Combining Example 1B and Example 2A-2D and Table 2, it can be seen that the flexural strength of Example 1B and Example 2A-2B is better than that of Example 2C-2D, indicating that when the particle size of the silicon micropowder loaded with silicon carbide whiskers in the present application is in the range of 10-30 microns, it can be better dispersed in the ceramic mud, and the toughening effect can be fully exerted during the firing process to reduce the cracking of the ceramic.
[0045] Combining Examples 3A-3C and Example 1B and Table 2, it can be seen that Examples 3A-3C are better than Example 1B, indicating that the addition of ethoxylated alkyl sodium sulfate as a surfactant in the present application can reduce the friction between ceramic mud materials, make the ceramic mud particles have good fluidity, and enhance the dispersion effect of the toughening component.
[0046] Combining Example 3A, Example 4A-4C, and Example 6 and Table 2, it can be seen that Example 4A-4C are better than Example 3A, indicating that in the present application, sodium nitride is mixed into the ceramic slurry. When sodium nitride is mixed with the water in the ceramic slurry, a large amount of heat will be released. The heat generated by the reaction of sodium nitride with water helps to improve the degree of bonding between the silicon micropowder-loaded silicon carbide whiskers and the ceramic mud material, and the reaction of sodium nitride with water will produce sodium hydroxide. Sodium hydroxide cannot have a toughening effect, but can promote the toughening effect of the toughening substance. This is because sodium hydroxide is sintered together with silicon micropowder, which can break the silicon-oxygen bonds in the silicon micropowder, thereby releasing silicon dioxide, thereby increasing the viscosity of the glass phase in the ceramic system, thereby increasing the creep resistance of the silicon carbide whiskers, and further improving the toughening effect of the ceramic.
[0047] In addition, since the surface of the silicon micropowder is treated with hydrochloric acid, during the preparation of the ceramic slurry, the hydrochloric acid remaining on the surface of the silicon micropowder can react with part of the sodium nitride to produce sodium chloride. Sodium chloride, as an electrolyte, can increase the viscosity of the ethoxylated alkyl sodium sulfate solution, so that the ceramic slurry can be quickly formed during the forming process, and it is not easy to cause the slurry viscosity to decrease due to the increase in temperature, resulting in poor forming effect.
[0048] Combining Example 4A and Examples 5A-5C and Table 2, it can be seen that Examples 5A-5C are better than Example 4A, indicating that the phosphate tailings added in the present application contain higher levels of silicon dioxide and calcium oxide. The sodium hydroxide generated by the reaction of sodium nitride and water provides an alkaline environment, which can also promote the release of silicon dioxide in the phosphate tailings. During the high-temperature sintering process, the phosphate tailings react with calcium oxide and other oxides in the ceramic mud to form a glass phase, further increasing the viscosity of the glass phase, improving the high-temperature creep resistance of the silicon carbide whiskers, and thereby enhancing its toughening effect.
[0049] Combining Example 4B and Example 7 and Table 2, it can be seen that Example 4B is better than Example 7, indicating that the sodium nitride of the present application is mixed separately before the grouting molding, so that a part of the sodium nitride reacts with water to generate a large amount of heat, so that the ceramic mud does not need additional heating during the grouting molding process, and can have a certain molding temperature, which helps to shorten the molding time; and the generation of heat also provides reaction conditions for the other part of the sodium nitride to react with hydrochloric acid. Sodium nitride reacts with the hydrochloric acid remaining on the silicon micropowder to generate sodium chloride. Sodium chloride can increase the viscosity of the surfactant, which is beneficial to the molding of the ceramic, making it less likely for the ceramic to crack during the grouting molding process.
[0050] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A toughened ceramic, It is characterized in that It comprises a ceramic body and a glaze layer, wherein the ceramic body comprises the following raw materials in parts by weight: Ceramic clay: 1-3 parts of wollastonite, 5-10 parts of porcelain powder, 13-17 parts of feldspar, 10-15 parts of ball clay, 5-8 parts of dolomite, 100-120 parts of Zhangcun soil; Silicon powder loaded with 50-60 parts of silicon carbide whiskers, 150-200 parts of water.
2. A toughened ceramic according to claim 1, Features: The silicon micropowder loaded silicon carbide whiskers comprises the following preparation steps: A1. Soak the silicon micropowder in a 2-4 mol / L hydrochloric acid solution for 1-2 hours, wherein the weight ratio of the silicon micropowder to the hydrochloric acid solution is 1:(1-2); A2. Add silicon carbide whiskers and disperse them ultrasonically for 10-15 minutes. The mass ratio of silicon carbide whiskers to silicon micropowder is (1-1.5):1 to obtain silicon micropowder-loaded silicon carbide whiskers.
3. A toughened ceramic according to claim 1, Features: The particle size of the silicon carbide whiskers loaded with silicon micropowder is 10-30 microns.
4. A toughened ceramic according to claim 2, Features: 2-5 parts of a surfactant are also added into the raw materials, and the surfactant is ethoxylated sodium alkyl sulfate.
5. A toughened ceramic according to claim 1, Features: 30-50 parts of sodium nitride are also added into the raw materials of the ceramic green body.
6. A toughened ceramic according to claim 1, Features: 20-30 parts of phosphorus tailings are also added into the ceramic mud.
7. A method for preparing a toughened ceramic according to any one of claims 1 to 6, It is characterized in that The following steps are involved: S1, mixing ceramic mud, silicon carbide whiskers loaded with silicon powder, surfactant and water by ball milling to obtain slurry; S2, injecting the slurry into a gypsum mold to obtain a ceramic green body by slip injection molding; S3, sintering the ceramic green body to obtain a ceramic green body, glazing the ceramic green body and firing it again to obtain a toughened ceramic.
8. A method for preparing toughened ceramics according to claim 7, Features: When sodium nitride is also added to the raw materials of the ceramic body, the preparation method comprises the following steps: S1, mixing ceramic mud, silicon carbide whiskers loaded with silicon powder, surfactant and water by ball milling, and then adding sodium nitride to obtain slurry; S2, injecting the slurry into a gypsum mold to obtain a ceramic green body by slip injection molding; S3, drying, glazing and firing the ceramic green body to obtain toughened ceramic.
Citation Information
Patent Citations
Preparation method of mud for sanitary porcelain large-piece products
CN103113082A
Coating and drilling method of ceramic substrate, coating sol and coating device
CN104014940A
Method for preparing ceramic-base composite material reinforced and toughened by silicon carbide whiskers
CN107778019A
High-strength ceramic biscuit and preparation process thereof
CN112573895A
Low-shrinkage FFC slurry ceramic biscuit and preparation process thereof
CN112624733A