Benzene-free low-hydroxyl acrylic resin as well as preparation method and application thereof
Through the preparation method of benzene-free low-hydroxyacrylic resin, acrylate monomers, alkenic acid and alkyl ester solvents, the problem of benzene-based solvents in the synthesis of acrylic paints was solved, and the benzene-free environmental protection and high color paint performance was achieved , reducing environmental pollution and construction difficulties.
Patent Information
- Application Number
- CN202411257964.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-09
- Publication Date
- 2024-11-22
AI Technical Summary
The existing acrylic coatings require the use of benzene solvents during the synthesis process, which cannot achieve true benzene-free environmental protection, and the synthesis temperature requirements of acrylic resins are difficult to meet the conditions of non-benzene solvents.
The preparation method of benzene-free low-hydroxyl acrylic resin is adopted, and acrylate monomers, alkenic acid, initiators and alkyl ester solvents are used. Through specific formula ratios and process steps, the use of benzene solvents is avoided and the acrylic resin is satisfied. synthesis temperature requirements.
It achieves a benzene-free environmental protection effect, reduces environmental pollution in production and construction, protects human health, and maintains good brightness and high color of acrylic resin, improving the construction convenience and storage stability of paint.
Smart Images

Figure HDA0005034655520000011 
Figure HDA0005034655520000012 
Figure HDA0005034655520000013
Abstract
Description
Technical Field
[0001] The invention relates to a benzene-free low-hydroxyl acrylic resin and a preparation method and application thereof, and relates to C09D, and in particular to the field of coating compositions. Background Art
[0002] With the development of society, people's environmental awareness is getting stronger and stronger. Acrylic paint has better color retention and gloss retention, good mechanical properties, excellent weather resistance, and is suitable for coating on the surface of metal components and instrument housings. However, acrylic paint needs to use benzene solvents for reflux and dilution during the synthesis process, which cannot meet the requirements of environmental protection. Since the synthesis temperature of acrylic resin is relatively high, the use of non-benzene solvents cannot meet the special requirements of the synthesis temperature of acrylic resin. Therefore, the use of benzene solvents can only be reduced, and true "benzene-free" environmental protection cannot be achieved. Therefore, it is crucial to develop an acrylic resin that does not use benzene solvents to achieve true environmentally friendly paint.
[0003] Chinese invention patent CN202111217723.3 discloses a double-modified self-crosslinking water-based acrylic emulsion and its preparation method. It adopts a process combining soap-free emulsion polymerization and core-shell emulsion polymerization, introduces self-crosslinking monomers, and double-modifies alkyd resin and silicone acrylic resin. It has the characteristics of quick drying, high gloss and high hardness, but styrene is required in the preparation process, which is not environmentally friendly. Chinese invention patent CN201510291446.9 discloses a phosphate-acrylic resin for silver powder paint and its preparation method. The acrylic resin is modified by phosphate acrylate, which greatly increases the encapsulation of the resin on the silver powder and increases the interlayer adhesion to UV. In the production process, propylene glycol methyl ether is used to dissolve phosphate acrylate, which can better enhance the performance of the paint, but styrene is also required in the preparation process, and the benzene-free requirement cannot be met. Summary of the invention
[0004] In order to improve the environmental performance of acrylic resin, avoid the introduction of benzene solvents, and maintain the good brightness and high chroma of acrylic resin, the first aspect of the present invention provides a benzene-free low-hydroxyl acrylic resin, and the raw materials for preparing the benzene-free low-hydroxyl acrylic resin include, by weight: 35-55 parts of acrylate monomers, 0-5 parts of alkene acid, 1-2 parts of initiator, and 45-55 parts of solvent.
[0005] As a preferred embodiment, the raw materials for preparing the benzene-free low-hydroxyl acrylic resin include, by weight: 40-50 parts of acrylic acid ester monomers, 0.1-1 parts of alkene acid, 1-1.5 parts of initiator, and 48-50 parts of solvent.
[0006] The raw materials for preparing the benzene-free low-hydroxyl acrylic resin include, by weight: 48.5 parts of acrylic ester monomers, 0.5 parts of alkene acid, 1 part of initiator, and 50 parts of solvent.
[0007] As a preferred embodiment, the acrylic ester monomers include hydroxy acrylic ester monomers, and the weight ratio of the hydroxy acrylic ester monomers to the non-hydroxy acrylic ester monomers is (5-10):(40-50).
[0008] As a preferred embodiment, the weight ratio of the hydroxy acrylate monomer to the non-hydroxy acrylate monomer is (6-8): (40-45).
[0009] As a preferred embodiment, the weight ratio of the hydroxy acrylate monomer to the non-hydroxy acrylate monomer is 7.5:41.
[0010] As a preferred embodiment, the non-hydroxyl acrylate monomer is selected from one or a combination of butyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, n-butyl methacrylate, methyl acrylate, and isooctyl acrylate.
[0011] As a preferred embodiment, the non-hydroxyl acrylic acid ester monomer includes a combination of butyl acrylate, methyl methacrylate, isooctyl acrylate, and n-butyl methacrylate.
[0012] As a preferred embodiment, the weight ratio of butyl acrylate, methyl methacrylate, isooctyl acrylate and n-butyl methacrylate is (1-5):(10-50):(1-5):(1-5).
[0013] As a preferred embodiment, the weight ratio of butyl acrylate, methyl methacrylate, isooctyl acrylate and n-butyl methacrylate is (3-5):(20-40):(3-5):(3-5).
[0014] As a preferred embodiment, the weight ratio of butyl acrylate, methyl methacrylate, isooctyl acrylate and n-butyl methacrylate is 3.5:30:3.5:4.
[0015] As a preferred embodiment, the hydroxyacrylate monomer is selected from one or a combination of hydroxyethyl acrylate, hydroxypropyl acrylate, hydroxyacrylate, hydroxyethyl methacrylate, and hydroxypropyl methacrylate.
[0016] As a preferred embodiment, the hydroxy acrylate monomer is hydroxyethyl acrylate.
[0017] As a preferred embodiment, the solvent does not include a benzene-containing solvent. Preferably, the solvent is an alkyl ester solvent.
[0018] As a preferred embodiment, the alkyl ester solvent is selected from one or a combination of methyl formate, methyl acetate, ethyl acetate, methyl propionate, ethyl propionate and butyl propionate.
[0019] As a preferred embodiment, the alkyl ester solvent is butyl ester.
[0020] As a preferred embodiment, the alkene acid is a monounsaturated alkene acid, and the monounsaturated alkene acid is selected from one or a combination of acrylic acid and methacrylic acid.
[0021] As a preferred embodiment, the alkene acid is methacrylic acid.
[0022] As a preferred embodiment, the initiator is an organic peroxide initiator, and the organic peroxide initiator is selected from one or a combination of tert-butyl perbenzoate, tert-butyl peroxy-2-ethylhexyl acid ester, tert-butyl peroxyvalerate, diisopropyl peroxydicarbonate, and dicyclohexyl peroxydicarbonate.
[0023] As a preferred embodiment, the initiator is tert-butyl perbenzoate.
[0024] The second aspect of the present invention provides a method for preparing a benzene-free low-hydroxyl acrylic resin, comprising the following steps:
[0025] S1 takes 30%-70% of the solvent in the formula and adds it into the reaction kettle;
[0026] S2: mixing acrylate monomers, alkene acid, and 50% to 80% of a formula amount of an initiator to obtain a mixture;
[0027] S3 The reaction kettle is stirred and heated to 100-120°C, and the mixture of step S2 is added dropwise;
[0028] S4 was added dropwise for 3-5h, kept warm for 1-2h, and the remaining initiator was added dropwise;
[0029] S5 was added dropwise for 1-2 hours, and the temperature was kept at 2-3 hours, then the temperature was lowered to 80-90°C, and the remaining solvent was added and mixed with stirring;
[0030] S6 is cooled and filtered to obtain.
[0031] The third aspect of the present invention provides an application of a benzene-free, low-hydroxyl acrylic resin in metal exterior decorative paint.
[0032] As a preferred embodiment, the paint using the benzene-free low-hydroxy acrylic resin is prepared by using raw materials including, by weight percentage: 40% benzene-free low-hydroxy acrylic resin, 15% CAB (cellulose acetate butyrate), 5% silver powder, 20% EAC (ethyl acetate), 10% PM (propylene glycol methyl ether), and 10% IBA (isobutyl alcohol).
[0033] As a preferred embodiment, the method for preparing the paint using the benzene-free low-hydroxyl acrylic resin comprises the following steps: stirring and mixing the raw materials to obtain the paint.
[0034] Compared with the prior art, the present invention has the following beneficial effects:
[0035] (1) The benzene-free low-hydroxyl acrylic resin of the present invention uses butyl ester solvent instead of benzene solvent to meet the processing requirements of acrylic resin reflux, achieve a true benzene-free environmental protection effect, greatly reduce environmental pollution in production and construction, and protect human health.
[0036] (2) The benzene-free, low-hydroxyl acrylic resin of the present invention needs to be introduced into CAB (cellulose acetate butyrate) when applied to paint. The benzene-free, low-hydroxyl acrylic resin of the present invention has little effect on color after adding CAB, the overall color value is not seriously reduced, and the sensitivity to CAB is low.
[0037] (3) The benzene-free low-hydroxyl acrylic resin of the present invention is applied to paint. After construction, the difference between wet and dry boards is small, the color formula is easy to control, the storage stability is excellent, the selection range of auxiliary agents such as dispersants is wide, and the formula selectivity is large.
[0038] (4) The benzene-free low-hydroxyl acrylic resin of the present invention is applied to paint, and the gloss of the paint is relatively matte, the color after varnishing is higher, the glossiness is more excellent, and it is easier to distinguish whether the surface is dry during the construction process, and it is easy to judge whether the lower layer construction can be carried out, and the construction is convenient.
[0039] (5) The benzene-free low-hydroxyl acrylic resin of the present invention, when used in paint, has both the wettability of color pigments and the arrangement and solvent resistance of silver powder, and has high comprehensive performance and excellent storage stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1 The effect pictures of the prepared paint after application, left picture: competitor's product; right picture: paint of application example 1;
[0041] Figure 2 The effect diagram of the prepared paint after applying the cover oil, left picture: competitor product; right picture: application example 1;
[0042] Figure 3The effect diagram of the prepared paint after application, left: competitor's product; right: paint of application example 2;
[0043] Figure 4 The effect diagram of the prepared paint after applying the cover oil, left picture: competitor product; right picture: application example 2;
[0044] Figure 5 The effect pictures of the prepared paint after application, left picture: competitor's product; right picture: paint of application example 3;
[0045] Figure 6 The effect diagram of the prepared paint after applying the cover oil, left picture: competitor product; right picture: application example 3;
[0046] Figure 7 The effect diagram of the prepared paint after application, left: competitor product; right: paint of application example 4;
[0047] Figure 8 The effect pictures of the prepared paint after applying the cover oil, left picture: competitor's product; right picture: application example 4. DETAILED DESCRIPTION
[0048] Example 1
[0049] A benzene-free low-hydroxyl acrylic resin. The raw materials for preparing the benzene-free low-hydroxyl acrylic resin include, by weight, 48.5 parts of acrylate monomers, 0.5 parts of alkene acid, 1 part of initiator, and 50 parts of solvent.
[0050] The weight ratio of the hydroxy acrylate monomer to the non-hydroxy acrylate monomer is 7.5:41.
[0051] The non-hydroxyl acrylic acid ester monomer includes a combination of butyl acrylate, methyl methacrylate, isooctyl acrylate, and n-butyl methacrylate, with a weight ratio of 3.5:30:3.5:4.
[0052] The hydroxy acrylate monomer is hydroxyethyl acrylate.
[0053] The solvent is butyl ester, the alkene acid is methacrylic acid, and the initiator is tert-butyl peroxybenzoate.
[0054] A method for preparing a benzene-free low-hydroxyl acrylic resin comprises the following steps:
[0055] S1 takes 50% of the solvent in the formula and adds it into the reactor;
[0056] S2: mixing acrylate monomer, alkene acid and 65% of the formula amount of initiator to obtain a mixture;
[0057] S3 The reaction kettle is stirred and heated to 120°C, and the mixture of step S2 is added dropwise;
[0058] S4 was added dropwise for 4 hours, and then kept warm for 2 hours, and the remaining initiator was added dropwise;
[0059] S5 was added dropwise for 1 hour, and the temperature was kept for 2 hours, then the temperature was lowered to 80°C, and the remaining solvent was added and mixed and stirred for 30 minutes;
[0060] S6 is cooled to 25°C and filtered to obtain.
[0061] Application Example 1
[0062] The invention discloses an application of a benzene-free low-hydroxy acrylic resin, which is applied to paint. The raw materials for preparing the resin include, by weight percentage, 40% of the benzene-free low-hydroxy acrylic resin of Example 1, 15% of CAB (cellulose acetate butyrate), 5% of silver powder, 10% of EAC (ethyl acetate), 10% of PM (propylene glycol methyl ether), 10% of red color paste, and 10% of IBA (isobutyl alcohol).
[0063] The method for preparing the paint using the benzene-free low-hydroxy acrylic resin comprises the following steps: stirring and mixing the raw materials to obtain the paint.
[0064] Application Example 2
[0065] The invention discloses an application of a benzene-free low-hydroxy acrylic resin, which is applied to paint. The raw materials for preparing the resin include, by weight percentage, 40% of the benzene-free low-hydroxy acrylic resin of Example 1, 15% of CAB (cellulose acetate butyrate), 5% of silver powder, 10% of EAC (ethyl acetate), 10% of PM (propylene glycol methyl ether), 10% of yellow color paste, and 10% of IBA (isobutyl alcohol).
[0066] The method for preparing the paint using the benzene-free low-hydroxy acrylic resin comprises the following steps: stirring and mixing the raw materials to obtain the paint.
[0067] Application Example 3
[0068] The invention discloses an application of a benzene-free low-hydroxy acrylic resin, which is applied to paint. The raw materials for preparing the resin include, by weight percentage, 40% of the benzene-free low-hydroxy acrylic resin of Example 1, 15% of CAB (cellulose acetate butyrate), 5% of silver powder, 10% of EAC (ethyl acetate), 10% of PM (propylene glycol methyl ether), 10% of blue color paste, and 10% of IBA (isobutyl alcohol).
[0069] The method for preparing the paint using the benzene-free low-hydroxy acrylic resin comprises the following steps: stirring and mixing the raw materials to obtain the paint.
[0070] Application Example 4
[0071] The invention discloses an application of a benzene-free low-hydroxy acrylic resin, which is applied to paint. The raw materials for preparing the resin include, by weight percentage: 40% of the benzene-free low-hydroxy acrylic resin of Example 1, 15% of CAB (cellulose acetate butyrate), 5% of silver powder, 10% of EAC (ethyl acetate), 10% of PM (propylene glycol methyl ether), 10% of green color paste, and 10% of IBA (isobutyl alcohol).
[0072] The method for preparing the paint using the benzene-free low-hydroxy acrylic resin comprises the following steps: stirring and mixing the raw materials to obtain the paint.
[0073] Performance Testing
[0074] 1. The content of benzene series of the acrylic resin prepared in Example 1 was tested in accordance with GB / T23990-2009, using gas chromatography with a detection limit of 50 mg / kg.
[0075] The total amount of benzene series (total amount of benzene, toluene, ethylbenzene and xylene) in the acrylic resin prepared in Example 1 was not detected (or was below the detection limit).
[0076] 2. After the paint of Application Example 1-4 is dry, it is covered with oil. The raw materials for preparing the paint covering water include, by weight percentage: EAC (ethyl acetate) 48%, BAC (n-butyl acetate) 2%, IPA (isopropyl alcohol) 3%, IBA (isobutyl alcohol) 28%, BCS (ethylene glycol monobutyl ether) 12%, DAA (diacetone alcohol) 2%, and MIBA (methyl isobutyl ketone) 5%.
[0077] The preparation method of paint opening water comprises the following steps: stirring and mixing the raw materials to obtain the paint opening water.
[0078] The mass ratio of the paint of Application Examples 1-4 to the paint opening water is 1:1.
[0079] The raw materials for preparing the varnish include, by weight percentage, 20% of 604 epoxy resin, 20% of hexafunctional polyurethane resin (purchased from Santong, model 8396), 10% of difunctional polyurethane resin (purchased from Santong, model 8172), 10% of solvent-based trifunctional polyurethane resin (purchased from Santong, model PSt03), 10% of TM (trimethylolpropane triacrylate), 3.5% of 184 photoinitiator, 0.5% of TPO photoinitiator, 0.3% of leveling agent (BYK 306), 0.2% of leveling agent (BYK 333), 17% of EAC (ethyl acetate), and 8.5% of BAC (n-butyl acetate). The raw materials are mixed to obtain the varnish.
[0080] The raw materials for preparing the polishing and oiling water include, by weight percentage: 55% EAC (ethyl acetate), 10% BAC (n-butyl acetate), 15% IPA (isopropyl alcohol), 15% IBA (isobutyl alcohol), and 5% BCS (ethylene glycol monobutyl ether). The raw materials are mixed to obtain the polishing and oiling water.
[0081] The mass ratio of varnish to topcoat water is 1:0.5.
[0082] The construction process is as follows:
[0083] Clean the board surface, then spray the paint and paint opener of the application example, bake at 60℃ for 5min, then spray varnish and topcoat opener, UV cure, curing energy is 550mj / cm 2 , the curing time is 3s.
[0084] The effect of spraying varnish and varnish before opening oil and water is shown in Figure 1 , 3, 5, 7; the effect of spraying varnish and varnishing after opening oil water is shown in Figure 2 , 4, 6, 8.
[0085] It can be seen from the figure that the prepared paint has low gloss, and the color saturation is higher after being covered with varnish, and the glossiness of the varnish is better. At the same time, during the construction process, it is easier to distinguish whether the surface is dry and whether the next layer of spraying can be continued. It is easy to construct in actual application.
Claims
1. A benzene-free low-hydroxyl acrylic resin, characterized in that: The raw materials for preparing the benzene-free low-hydroxyl acrylic resin include, by weight: 35-55 parts of acrylic ester monomers, 0-5 parts of alkene acid, 1-2 parts of initiator, and 45-55 parts of solvent.
2. The benzene-free low-hydroxyl acrylic resin according to claim 1, characterized in that: The acrylic ester monomers include hydroxy acrylic ester monomers, and the weight ratio of the hydroxy acrylic ester monomers to the non-hydroxy acrylic ester monomers is (5-10):(40-50).
3. The benzene-free low-hydroxyl acrylic resin according to claim 2, characterized in that: The non-hydroxyl acrylic acid ester monomer is selected from one or a combination of butyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, n-butyl methacrylate, methyl acrylate, and isooctyl acrylate.
4. The benzene-free low-hydroxyl acrylic resin according to claim 2, characterized in that: The hydroxy acrylate monomer is selected from one or a combination of hydroxyethyl acrylate, hydroxypropyl acrylate, hydroxyacrylate, hydroxyethyl methacrylate, and hydroxypropyl methacrylate.
5. The benzene-free low-hydroxyl acrylic resin according to claim 1, characterized in that: The solvent does not include a benzene-containing solvent. Preferably, the solvent is an alkyl ester solvent.
6. The benzene-free low-hydroxyl acrylic resin according to claim 5, characterized in that: The alkyl ester solvent is selected from one or a combination of methyl formate, methyl acetate, ethyl acetate, methyl propionate, ethyl propionate and butyl propionate.
7. The benzene-free low-hydroxyl acrylic resin according to claim 1, characterized in that: The alkene acid is a monounsaturated alkene acid, and the monounsaturated alkene acid is selected from one or a combination of acrylic acid and methacrylic acid.
8. The benzene-free low-hydroxyl acrylic resin according to claim 1, characterized in that: The initiator is an organic peroxide initiator, and the organic peroxide initiator is selected from one or a combination of tert-butyl perbenzoate, tert-butyl peroxy-2-ethylhexyl acid ester, tert-butyl peroxy-t-valerate, diisopropyl peroxydicarbonate, and dicyclohexyl peroxydicarbonate.
9. A method for preparing the benzene-free low-hydroxyl acrylic resin according to any one of claims 1 to 8, characterized in that: The following steps are involved: S1 takes 30%-70% of the solvent in the formula and adds it into the reaction kettle; S2: mixing acrylate monomers, alkene acid, and 50% to 80% of a formula amount of an initiator to obtain a mixture; S3 The reaction kettle is stirred and heated to 100-120°C, and the mixture of step S2 is added dropwise; After S4 is added dropwise, keep warm for 1-2 hours and add the remaining initiator dropwise; After the addition of S5 is completed, keep warm for 2-3 hours, add the remaining solvent and mix with stirring; S6 is cooled and filtered to obtain.
10. An application of the benzene-free, low-hydroxyl acrylic resin according to any one of claims 1 to 8, characterized in that: Used in metal exterior decorative paint.