High-strength alkoxy-terminated 107 glue and preparation method thereof, and dealcoholized silicone rubber and preparation method thereof
By optimizing the preparation method of alkoxy-terminated 107 rubber and using silicon-aza-cyclopentane compounds, the problems of high viscosity, poor storage stability and free methanol formation of dealcoholized silicone rubber are solved, and high reaction activity is achieved. Strength and storage stability, suitable for high-precision applications.
Patent Information
- Application Number
- CN202411093422.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-09
AI Technical Summary
During the preparation and storage process of existing dehydrogenated silicone rubber, there are problems such as peak viscosity, poor storage stability, low reaction activity and strength, and the formation of free methanol, which is difficult to meet market demand.
Using high-strength alkoxy end capping 107 glue, the end-side vinyl silicone oil and silicone ethylene silicone oligomers are used as raw materials, combined with platinum catalyst and A-171 vinyl trimethoxy silane, optimized silicon hydrocarbon addition Reaction, increase the reactivity and strength, and use the silicon-aza-cyclopentane compound as a stabilizer to remove water and capture free alcohols, improving storage stability and adhesion properties.
It significantly improves the reaction activity and strength, extends the shelf life of the product, enhances market competitiveness, enhances the adhesion ability to the substrate, and ensures the long-term stability and environmental friendliness of the product.
Smart Images

Figure CN118994588A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of dealcoholized silicone rubber, and more specifically, to a high-strength alkoxy-terminated 107 rubber and a preparation method thereof, and a dealcoholized silicone rubber and a preparation method thereof. Background Art
[0002] In the current field of chemical materials, room temperature vulcanized silicone rubber (RTV silicone rubber) is an important polymer material. It is widely used in many industries such as construction, electronics, and automobiles due to its unique physical and chemical properties, such as good weather resistance, excellent insulation, and good adhesion to a variety of substrates. Among them, 107 glue (i.e. α, ω-dihydroxy polydimethylsiloxane) is the base rubber for most room temperature vulcanized silicone rubber. It occupies an important position due to its non-flammable, moderate price, and easy use.
[0003] Most of the existing 107 glues are deacidified, dealcoholized, and deketoxime types, among which the dealcoholized 107 glue has the advantages of neutral properties, cleanliness, non-toxicity, non-corrosiveness, low cost, and good bonding performance to materials such as glass and metal. The dealcoholized room temperature vulcanized silicone rubber prepared using the dealcoholized 107 glue is environmentally friendly due to the release of small molecules of methanol or ethanol, is non-corrosive to metals, and does not produce irritating odor. It is widely used in electronics, construction, automobiles and other industries; however, in the actual application of 107 glue and its derived room temperature vulcanized silicone rubber, especially in the preparation and use of dealcoholized silicone rubber, there are still a series of problems that need to be solved.
[0004] First, in the preparation process of traditional dealcoholized silicone rubber, titanate catalysts are often used to promote crosslinking reactions. However, such catalysts can easily cause the viscosity of the rubber to rise sharply, forming a viscosity peak, which not only increases the difficulty of production, but may also damage the production equipment. In addition, the use of titanate catalysts also makes the storage stability of the product poor, which is prone to premature curing or deterioration, affecting the performance of the product.
[0005] To solve the above problems, researchers have tried to treat 107 silicone rubber with alkoxy end-capping to improve its viscosity control and storage stability. However, the commercially available alkoxy end-capped 107 rubber is still insufficient in reactivity and strength and cannot fully meet market demand. Therefore, the development of an alkoxy end-capped 107 rubber that can effectively control the viscosity peak, improve storage stability, and have both high reactivity and strength has become a hot topic in current research.
[0006] On the other hand, during the storage of dealcoholized silicone rubber, the residual water in the rubber reacts with the crosslinking agent (such as methyltrimethoxysilane) to generate free methanol, which not only reduces the storage stability of silicone rubber and shortens its effective storage period (usually only 3-6 months), but also may cause potential harm to the environment and human health. Although some studies have tried to solve this problem by adding stabilizers (such as β-diketone compounds), these stabilizers cannot simultaneously remove water, capture free alcohol, and enhance the bonding performance to the contact substrate, which is a technical problem in the industry.
[0007] In summary, there are problems in the preparation, storage and use of dealcoholized room temperature vulcanized silicone rubber in the prior art, and an innovative solution is urgently needed. Summary of the invention
[0008] In order to solve the above problems, the present application provides a high-strength alkoxy-terminated 107 rubber and a preparation method and a dealcoholized silicone rubber and a preparation method. The purpose is to optimize the alkoxy-terminated process of 107 silicone rubber and use a highly efficient multifunctional stabilizer to effectively solve the problems of viscosity peak, poor storage stability, low reactivity and strength, and free methanol generation, and provide more reliable technical support for the preparation and application of room temperature vulcanized silicone rubber.
[0009] In the first aspect, the present application provides a high-strength alkoxy-terminated 107 glue, which adopts the following technical solution: A high-strength alkoxy-terminated 107 glue comprising the following components: 100 parts by mass of end-side vinyl silicone oil; 3-10 parts by mass of silylene siloxane oligomer; 1-10ppm platinum catalyst; 0.06-0.25 parts by mass of A-171 vinyltrimethoxysilane; The ratio of the vinyl content of the end-side vinyl silicone oil to the hydrogen content of the silylethylenesiloxane oligomer is 1:(1-1.15); The ratio of the vinyl content of A-171 vinyltrimethoxysilane to the hydrogen content of silylethylenesiloxane oligomer is (1-1.25):1.
[0010] The structural formula of silylene siloxane oligomer is as follows: The structural formula of high-strength alkoxy-terminated 107 glue is as follows (n and m are integers, and m is not 0): Where m≠0 By adopting the above technical solution, alkoxy-terminated 107 rubber was prepared by hydrosilylation using end-side vinyl silicone oil and silylethylene siloxane oligomer as raw materials. This innovation not only greatly enhances the reaction activity, making the reaction process faster and more efficient, but also significantly improves the strength of the final product, meeting the strict requirements of high-performance materials for mechanical properties. In addition, this improvement also effectively solves the problem of poor storage stability faced by traditional dealcoholized silicone rubber during the preparation process, prolongs the shelf life of the product, reduces storage costs, and improves market competitiveness.
[0011] In terms of raw material selection, the present application abandons the use of traditional hydrogen-containing silanes (such as hydrogen-containing trimethoxysilane or hydrogen-containing methyldimethoxysilane) and instead adopts silylene siloxane oligomers, which are relatively non-toxic and harmless, have a high flash point (flash point greater than 60°C), good safety, good stability, and a mild and controllable reaction.
[0012] In order to further improve the storage stability, the present application makes the hydrogen content of silylethylene siloxane oligomer slightly higher than the vinyl content of the end-side vinyl silicone oil, and then introduces an excess of A-171 vinyl trimethoxy silane into the reaction system. This step not only ensures the thoroughness of the hydrosilylation reaction and avoids the adverse effects of unreacted hydrogen bonds on product quality, but also brings into play the dual role of A-171 vinyl trimethoxy silane as a stable dehydrating agent and cross-linking agent. A-171 can effectively remove moisture from the system and prevent colloid degradation or performance degradation caused by moisture; at the same time, its cross-linking effect enhances the cohesion and structural stability of the colloid, so that the alkoxy-terminated 107 glue can maintain excellent performance during storage and is not prone to aging or deterioration. This innovative design greatly improves the storage stability of the product and provides a more reliable and lasting user experience.
[0013] Preferably, the ratio of the vinyl content of the terminal vinyl silicone oil to the hydrogen content of the silylethylenesiloxane oligomer is 1:(1.05-1.1); The ratio of the vinyl content of A-171 vinyltrimethoxysilane to the hydrogen content of silylethylenesiloxane oligomer is (1.1-1.2):1.
[0014] By adopting the above technical scheme, the vinyl content of the end-side vinyl silicone oil and the hydrogen content of the silylene siloxane oligomer, the vinyl content of A-171 vinyl trimethoxysilane and the hydrogen content of the silylene siloxane oligomer are further optimized, so that the hydrosilylation reaction is complete, and the excess silylene siloxane oligomer is reacted with the excess A-171 vinyl trimethoxysilane. The excess A-171 vinyl trimethoxysilane with a further limited amount will not only not affect the 107 glue, but on the contrary, it has the dual role of stabilizing the dehydrating agent and the crosslinking agent, which is conducive to the subsequent preparation of dealcoholized silicone rubber.
[0015] Preferably, the viscosity of the end-side vinyl silicone oil is 500mPa.s-80000mPa.s.
[0016] In the second aspect, the present application provides a method for preparing high-strength alkoxy-terminated 107 glue, using the following technical solution: A method for preparing high-strength alkoxy-terminated 107 glue comprises the following steps: Step 1: Mix terminal vinyl silicone oil, silylene siloxane oligomer and platinum catalyst, and react at 50-100° C. for 120-360 minutes to obtain a first reactant; Step 2: react the first reactant with A-171 vinyltrimethoxysilane at 50-100° C. for 60-120 min to obtain high-strength alkoxy-terminated 107 glue.
[0017] Preferably, the reaction temperature of step 1 and step 2 is 60°C.
[0018] In a third aspect, the present application provides a dealcoholized silicone rubber.
[0019] A dealcoholized silicone rubber comprises the following components in parts by mass: 60-70 parts of high-strength alkoxy-terminated 107 rubber, 1-6 parts of silicon-aza-cyclopentane compound, 10-15 parts of hydrophobic fumed silica, 1-3 parts of a crosslinking agent, 0.1-0.5 parts of a coupling agent, 0.1-0.5 parts of a catalyst, and 5-10 parts of dimethyl silicone oil.
[0020] Preferably, the crosslinking agent includes a mixture of one or more of methyltrimethoxysilane and cyanoethyltrimethoxysilane.
[0021] Preferably, the coupling agent is glycidyloxypropyltrimethoxysilane (KH560).
[0022] Preferably, the catalyst is an organic titanium catalyst or an organic tin catalyst.
[0023] Preferably, the catalyst is an organic tin catalyst, more preferably dibutyltin dineodecanoate.
[0024] Dealcoholized silicone rubber is also known as dealcoholized component room temperature curing silicone rubber.
[0025] The synergistic effect of silicon-aza-cyclopentane compounds and high-strength alkoxy-terminated 107 glue makes the silicone rubber sealant show excellent storage stability, and it can still maintain good performance without attenuation even after long-term storage. At the same time, its bonding ability to various substrates is significantly improved, especially suitable for high-precision and high-demand application fields such as electronics, ensuring reliable connection of products in different environments.
[0026] For precision manufacturing industries such as electronics, the dealcohol-type component room temperature curing silicone rubber of the present invention has stronger bonding ability and less glue consumption, which directly reduces production costs and improves production efficiency. At the same time, the excellent comprehensive performance also reduces the frequency of later maintenance and replacement, further improving the overall economic benefits.
[0027] Moreover, the synergistic effect of silicon-aza-cyclopentane compounds and high-strength alkoxy-terminated 107 rubber can effectively remove water and capture free alcohols, significantly enhancing the resistance of dealcoholization-type room-temperature-curing silicone rubber to environmental factors, ensuring the excellent performance and long-term stability of the final product.
[0028] Preferably, the silicon-aza-cyclopentane compound is prepared by reacting hexamethyldisilazane with an aminoalkyldialkoxysilyl-terminated diorganosiloxane oligomer (amino-functionalized diorganosiloxane oligomer) at both ends of the molecular chain. The synthesis route is as follows: By adopting the above technical scheme, the present invention uses hexamethyldisilazane and an amino-functionalized diorganosiloxane oligomer of a specific structure to generate 1-silicon-azacyclopentylsiloxane oligomers at both ends of the molecular chain and the condensation product, namely, silicon-aza-cyclopentane compound, through the above synthesis path. The 1-silicon-azacyclopentylsiloxane oligomers at both ends of the molecular chain are a highly efficient stabilizer with the dual effects of strong alcohol removal and viscosity enhancement, which effectively solves the problem of free alcohol that is easily generated during the curing process of traditional dealcoholized silicone rubber, and at the same time significantly enhances the adhesion between the sealant and the substrate, ensuring the durability and reliability of the sealing effect.
[0029] The additive not only effectively removes free alcohol produced during the curing process, but also effectively captures and removes trace moisture in the system, further improving the purity and curing quality of the silicone rubber sealant. This feature is crucial to improving the electrical insulation performance and long-term durability of the product.
[0030] Preferably, the synthesis of the silicon-aza-cyclopentane compound comprises the following steps: Step a: α,ω dihydroxy polydimethylsiloxane and aminopropyltrimethoxysilane are mixed in a mass ratio of (1.3-1.6):1, a small amount of formic acid aqueous solution is added dropwise, and the mixture is reacted at 55-65° C. for 0.5-1.5 h to obtain an amino-functionalized diorganosiloxane oligomer; Step b: Mix the amino-functionalized diorganosiloxane oligomer, hexamethyldisilazane and trimethylchlorosilane, and react at 95-105° C. for 7-9 hours to obtain a silicon-aza-cyclopentane compound.
[0031] In a fourth aspect, the present application provides a method for preparing dealcoholized silicone rubber.
[0032] A method for preparing dealcoholized silicone rubber comprises the following steps: Step A: high-strength alkoxy-terminated 107 glue and dimethyl silicone oil are stirred and mixed at 30-50° C. and vacuum (-0.085-0.095 MPa) for 5-10 minutes to obtain a first mixture; Step B: mixing the first mixture with the crosslinking agent, the coupling agent and the silicon-aza-cyclopentane compound under vacuum (-0.035-0.055 MPa) for 5-10 minutes to obtain a second mixture; Step C: vacuum-dispersing the second mixture and hydrophobic fumed silica for 15-30 minutes at high speed, and then dispersing them at high speed for 5-10 minutes while evacuating (-0.085-0.095 MPa) to obtain a third mixture; Step D: Mix the third mixture with the catalyst under vacuum (-0.085-0.095 MPa) for 5-10 min to obtain dealcoholized silicone rubber.
[0033] In summary, this application has the following beneficial effects: 1. Using end-vinyl silicone oil and silylethylene siloxane oligomer as raw materials, alkoxy-terminated 107 glue is prepared by hydrosilylation. The content of end-capped 107 alkoxy groups can be adjusted according to needs, thereby adjusting the reaction activity, and then adjusting the curing operation time and strength of the alcohol-type glue.
[0034] 2. During the preparation process, after the end-side vinyl silicone oil and silylethylenesiloxane oligomer have completed their reaction, add an excess of A-171 vinyltrimethoxysilane to continue the reaction to ensure that the hydrogen bond reaction of the system is complete. At the same time, A-171 is also a stable dehydrating agent and cross-linking agent to improve the storage stability of alkoxy-terminated 107 glue.
[0035] 3. Silicone ethylene siloxane oligomer is used as the raw material. Compared with hydrogen-containing silane (hydrogen-containing trimethoxysilane or hydrogen-containing methyldimethoxysilane), silicone ethylene siloxane oligomer is non-toxic and harmless, has a high flash point (flash point greater than 60°C), good safety, good stability, and a mild and controllable reaction.
[0036] 4. The silicon-aza-cyclopentane compound (1-silicon-azacyclopentylsiloxane oligomers at both ends of the molecular chain and condensation products) obtained by the reaction of hexamethyldisilazane with amino-functionalized diorganosiloxane oligomers (diorganosiloxane oligomers terminated with aminoalkyldialkoxysilyl groups at both ends of the molecular chain) is a highly efficient stabilizer, which is used to prepare dealcoholization-type component room temperature curing silicone rubber sealant. In addition to the effects of removing water and capturing free alcohol, it also achieves the effect of viscosity increase, so that the formulated sealant has good storage stability and excellent bonding properties to the contact substrate. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1It is the structural formula of silylene siloxane oligomer.
[0038] Figure 2 It is the structural formula of high-strength alkoxy-terminated 107 glue.
[0039] Figure 3 This is a schematic diagram of the reaction process of step b. DETAILED DESCRIPTION
[0040] The present application is further described in detail below with reference to the accompanying drawings and embodiments.
[0041] The raw materials used in the following examples and comparative examples are all commercially available products.
[0042] The viscosity of the end-side vinyl silicone oil is 500mPa.s to 80000mPa.s. Example
[0043] Example 1 A high-strength alkoxy-terminated 107 glue comprises 100 parts by weight of 19560cs of end-side vinyl silicone oil with a vinyl content of 0.442%; 5 parts by weight of silylene siloxane oligomer with a hydrogen content of 0.36%; 5ppm (content of the total material) of platinum catalyst; and 0.118 parts by weight of A-171 vinyl trimethoxy silane.
[0044] The ratio of the vinyl content of the terminal vinyl silicone oil to the hydrogen content of the silylethylenesiloxane oligomer is 1:1.1.
[0045] The ratio of the vinyl content of A-171 vinyl trimethoxysilane to the hydrogen content of silylene siloxane oligomer is 1.2:1.
[0046] The platinum catalyst is a Custer catalyst.
[0047] Structural formula reference of silylethylene siloxane oligomer Figure 1 .
[0048] The present application also provides a method for preparing high-strength alkoxy-terminated 107 glue, comprising the following steps: Step 1: Mix the end-side vinyl silicone oil and the silylene siloxane oligomer, then add the platinum catalyst, and react at 60° C. for 240 minutes to obtain the first reactant.
[0049] Step 2: Add A-171 vinyl trimethoxysilane to the first reactant and react at 60°C for 90 minutes. After the reaction is completed, cool down to obtain high-strength alkoxy-terminated 107 glue.
[0050] Structural formula reference of high strength alkoxy terminated 107 glue Figure 2 .
[0051] This embodiment also provides a dealcoholized silicone rubber, including the following components: 65.4kg high-strength alkoxy-terminated 107 glue, 4kg silicon-aza-cyclopentane compound, 8.5kg dimethyl silicone oil, 13kg hydrophobic fumed silica, 0.7kg cyanoethyl trimethoxysilane, 1kg methyl trimethoxysilane, 0.25kg glycidyl ether oxide propyl trimethoxysilane (KH560), and 0.24kg dibutyl tin dineodecanoate.
[0052] The hydrophobic fumed silica of the present embodiment was purchased from Yichang Huifu, model number HB-620.
[0053] The synthesis of silicon-aza-cyclopentane compounds comprises the following steps: Step a: Mix 40 g of α, ω dihydroxy polydimethylsiloxane and 27 g of aminopropyltrimethoxysilane, add a small amount (2 drops) of 80% by mass formic acid aqueous solution, and stir the mixture at 60° C. for 1 h.
[0054] Then, under a reduced pressure of 2.66 kPa, unreacted components of the reaction species and methanol were distilled off at 120° C. to obtain a colorless transparent liquid, namely, an amino-functionalized diorganosiloxane oligomer.
[0055] Step b: Mix the amino-functionalized diorganosiloxane oligomer, hexamethyldisilazane and trimethylchlorosilane and slowly raise the temperature to 100°C. When the temperature is reached, trimethylmethoxysilane is distilled out, accompanied by a considerable amount of NH3. Continue to maintain the temperature and stir the reaction for 8 hours.
[0056] Then, the volatile components were distilled at 100° C. and 2.66 kPa under reduced pressure to obtain a light yellow liquid, namely, a silicon-aza-cyclopentane compound.
[0057] The reaction process of step b is shown in Figure 3 .
[0058] The preparation method of dealcoholized silicone rubber comprises the following steps: Step A: High-strength alkoxy-terminated 107 glue and dimethyl silicone oil were stirred and mixed at 40° C. under vacuum (-0.09 MPa) for 8 minutes to obtain a first mixture.
[0059] Step B: The first mixture is mixed with a crosslinking agent, a coupling agent and a silicon-aza-cyclopentane compound under vacuum (-0.045 MPa) for 8 minutes to obtain a second mixture.
[0060] Step C: The second mixture and the hydrophobic fumed silica are dispersed at high speed in vacuum for 20 minutes, and then dispersed at high speed for 8 minutes while evacuating the vacuum (-0.09 MPa) to obtain a third mixture.
[0061] Step D: The third mixture and the catalyst were mixed under vacuum (-0.09 MPa) for 8 min to obtain dealcoholized silicone rubber.
[0062] Example 2 A high-strength alkoxy-terminated 107 glue, which is different from Example 1 in that it includes 100 parts by mass of 9820cs end-side vinyl silicone oil with a vinyl content of 0.278%, 3 parts by mass of silylethylene siloxane oligomer with a hydrogen content of 0.36%, 1 ppm (total material content) of platinum catalyst, and 0.065 parts by mass of A-171 vinyl trimethoxy silane.
[0063] The ratio of the vinyl content of the terminal vinyl silicone oil to the hydrogen content of the silylethylenesiloxane oligomer is 1:1.05.
[0064] The ratio of the vinyl content of A-171 vinyl trimethoxysilane to the hydrogen content of silylethylene siloxane oligomer is 1.1:1.
[0065] A method for preparing high-strength alkoxy-terminated 107 glue, which is different from Example 1 in that it comprises the following steps: Step 1: Mix the end-vinyl silicone oil and the silylethylenesiloxane oligomer, then add the platinum catalyst, and react at 50° C. for 360 minutes to obtain the first reactant.
[0066] Step 2: Add A-171 vinyl trimethoxysilane to the first reactant and react at 50°C for 120 minutes. After the reaction is completed, cool down to obtain high-strength alkoxy-terminated 107 glue.
[0067] A dealcoholized silicone rubber, which is different from Example 1 in that: The dealcoholized silicone rubber includes the following components: 60kg high-strength alkoxy-terminated 107 rubber, 1kg silicon-aza-cyclopentane compound, 5kg dimethyl silicone oil, 10kg hydrophobic fumed silica, 0.4kg cyanoethyl trimethoxy silane, 0.6kg methyl trimethoxy silane, 0.1kg glycidyl ether oxide propyl trimethoxy silane (KH560), and 0.1kg dibutyl tin dineodecanoate.
[0068] The synthesis of silicon-aza-cyclopentane compounds comprises the following steps: Step a: Mix 35.1 g of α, ω dihydroxy polydimethylsiloxane and 27 g of aminopropyltrimethoxysilane, add a small amount (2 drops) of 80% by mass formic acid aqueous solution, and stir the mixture at 55° C. for 1.5 h.
[0069] Then, under a reduced pressure of 2.66 kPa, unreacted components of the reaction species and methanol were distilled off at 120° C. to obtain a colorless transparent liquid, namely, an amino-functionalized diorganosiloxane oligomer.
[0070] Step b: Mix the amino-functionalized diorganosiloxane oligomer, hexamethyldisilazane and trimethylchlorosilane and slowly raise the temperature to 95°C. When the temperature is reached, trimethylmethoxysilane is distilled out, accompanied by a considerable amount of NH3. Continue to maintain the temperature and stir the reaction for 9 hours.
[0071] Then, the volatile components were distilled at 100° C. and 2.66 kPa under reduced pressure to obtain a light yellow liquid, namely, a silicon-aza-cyclopentane compound.
[0072] The method for preparing the dealcoholized silicone rubber is different from that of Example 1 in that it comprises the following steps: Step A: High-strength alkoxy-terminated 107 glue and dimethyl silicone oil were stirred and mixed at 30° C. under vacuum (-0.095 MPa) for 10 min to obtain a first mixture.
[0073] Step B: The first mixture is mixed with a crosslinking agent, a coupling agent and a silicon-aza-cyclopentane compound under vacuum (-0.055 MPa) for 5 minutes to obtain a second mixture.
[0074] Step C: The second mixture and the hydrophobic fumed silica are dispersed at high speed in vacuum for 20 minutes, and then dispersed at high speed for 5 minutes while evacuating the vacuum (-0.095 MPa) to obtain a third mixture.
[0075] Step D: The third mixture and the catalyst were mixed under vacuum (-0.095 MPa) for 5 min to obtain dealcoholized silicone rubber.
[0076] Example 3 A high-strength alkoxy-terminated 107 glue, which is different from Example 1 in that it includes 100 parts by mass of 1430cs end-side vinyl silicone oil with a vinyl content of 0.845%, 10 parts by mass of silylethylene siloxane oligomer with a hydrogen content of 0.36%, 10 ppm (total material content) of platinum catalyst, and 0.247 parts by mass of A-171 vinyl trimethoxy silane.
[0077] The ratio of the vinyl content of the terminal vinyl silicone oil to the hydrogen content of the silylethylenesiloxane oligomer is 1:1.15.
[0078] The ratio of the vinyl content of A-171 vinyl trimethoxysilane to the hydrogen content of silylene siloxane oligomer is 1.25:1.
[0079] A method for preparing high-strength alkoxy-terminated 107 glue, which is different from Example 1 in that it comprises the following steps: Step 1: Mix the end-vinyl silicone oil and silylethylenesiloxane oligomer, then add a platinum catalyst, and react at 100° C. for 120 minutes to obtain a first reactant.
[0080] Step 2: Add A-171 vinyl trimethoxysilane to the first reactant and react at 100°C for 60 minutes. After the reaction is completed, cool down to obtain high-strength alkoxy-terminated 107 glue.
[0081] A dealcoholized silicone rubber, which is different from Example 1 in that: The dealcoholized silicone rubber includes the following components: 70kg high-strength alkoxy-terminated 107 glue, 6kg silicon-aza-cyclopentane compound, 10kg dimethyl silicone oil, 15kg hydrophobic fumed silica, 1.2kg cyanoethyl trimethoxy silane, 1.8kg methyl trimethoxy silane, 0.5kg glycidyl ether oxide propyl trimethoxy silane (KH560), and 0.5kg dibutyl tin dineodecanoate.
[0082] The synthesis of silicon-aza-cyclopentane compounds comprises the following steps: Step a: Mix 43.2 g of α,ω dihydroxy polydimethylsiloxane and 27 g of aminopropyltrimethoxysilane, add a small amount (2 drops) of 80% by mass formic acid aqueous solution, and stir the mixture at 65° C. for 0.5 h.
[0083] Then, under a reduced pressure of 2.66 kPa, unreacted components of the reaction species and methanol were distilled off at 120° C. to obtain a colorless transparent liquid, namely, an amino-functionalized diorganosiloxane oligomer.
[0084] Step b: Mix the amino-functionalized diorganosiloxane oligomer, hexamethyldisilazane and trimethylchlorosilane and slowly raise the temperature to 105°C. When the temperature is reached, trimethylmethoxysilane is distilled out, accompanied by a considerable amount of NH3. Continue to maintain the temperature and stir the reaction for 7 hours.
[0085] Then, the volatile components were distilled at 100° C. and 2.66 kPa under reduced pressure to obtain a light yellow liquid, namely, a silicon-aza-cyclopentane compound.
[0086] The method for preparing the dealcoholized silicone rubber is different from that of Example 1 in that it comprises the following steps: Step A: High-strength alkoxy-terminated 107 glue and dimethyl silicone oil were stirred and mixed at 50° C. under vacuum (-0.085 MPa) for 5 minutes to obtain a first mixture.
[0087] Step B: The first mixture is mixed with a crosslinking agent, a coupling agent and a silicon-aza-cyclopentane compound under vacuum (-0.035 MPa) for 10 min to obtain a second mixture.
[0088] Step C: The second mixture and the hydrophobic fumed silica are dispersed at high speed in vacuum for 20 minutes, and then dispersed at high speed for 10 minutes while evacuating the vacuum (-0.085 MPa) to obtain a third mixture.
[0089] Step D: The third mixture and the catalyst were mixed under vacuum (-0.085 MPa) for 10 min to obtain dealcoholized silicone rubber.
[0090] Comparative Example Comparative Example 1 A high-strength alkoxy-terminated 107 glue, which is different from Example 1 in that the ratio of the vinyl content of the end-side vinyl silicone oil to the hydrogen content of the silylethylene siloxane oligomer is 1:0.5.
[0091] That is, 100 parts by mass of 19560cs of terminal vinyl silicone oil, with a vinyl content of 0.442%; and 2.27 parts by mass of silylethylenesiloxane oligomer, with a hydrogen content of 0.36%.
[0092] The high-strength alkoxy-terminated 107 rubber is used in the preparation of dealcoholized silicone rubber.
[0093] In addition, the preparation method of high-strength alkoxy-terminated 107 rubber, the raw material composition of dealcoholized silicone rubber, and the preparation method of dealcoholized silicone rubber are the same as those in Example 1 and are not described in detail here.
[0094] Comparative Example 2 A high-strength alkoxy-terminated 107 glue, which is different from Example 1 in that the ratio of the vinyl content of the end-side vinyl silicone oil to the hydrogen content of the silylethylene siloxane oligomer is 1:2.
[0095] That is, 100 parts by mass of 19560 cs of terminal vinyl silicone oil, with a vinyl content of 0.442%; and 9.09 parts by mass of silylethylene siloxane oligomer, with a hydrogen content of 0.36%.
[0096] The high-strength alkoxy-terminated 107 rubber is used in the preparation of dealcoholized silicone rubber.
[0097] In addition, the preparation method of high-strength alkoxy-terminated 107 rubber, the raw material composition of dealcoholized silicone rubber, and the preparation method of dealcoholized silicone rubber are the same as those in Example 1 and are not described in detail here.
[0098] Comparative Example 3 A dealcoholized silicone rubber, which is different from Example 1 in that the high-strength alkoxy-terminated 107 rubber is replaced by 20000cs commercially available terminated 107 rubber (addition type).
[0099] In addition, the raw material composition of the dealcoholized silicone rubber and the preparation method of the dealcoholized silicone rubber are the same as those in Example 1, which will not be described in detail here.
[0100] Comparative Example 4 A dealcoholized silicone rubber is different from Example 1 in that the silicon-aza-cyclopentane compound is replaced by acetylacetone.
[0101] In addition, the raw material composition of the dealcoholized silicone rubber and the preparation method of the dealcoholized silicone rubber are the same as those in Example 1, which will not be described in detail here.
[0102] Comparative Example 5 A dealcoholized silicone rubber, which is different from Example 1 in that the high-strength alkoxy-terminated 107 rubber is replaced by 20000cs commercially available end-capped 107 rubber (addition type), and the silicon-aza-cyclopentane compound is replaced by acetylacetone.
[0103] In addition, the raw material composition of the dealcoholized silicone rubber and the preparation method of the dealcoholized silicone rubber are the same as those in Example 1, which will not be described in detail here.
[0104] Performance testing 1. Adhesion strength: With reference to GB / T 2791-1995 "Adhesive T peel strength test method - Flexible material to flexible material", the dealcoholized silicone rubbers of Examples 1-3 and Comparative Examples 1-5 were tested, and the results are recorded in Table 1.
[0105] Table 1 2. Storage stability: The detection objects are the dealcoholized silicone rubbers of Examples 1-3 and Comparative Examples 1-5.
[0106] The dealcoholized silicone rubber was tested with reference to GB / T 528-2009 “Determination of tensile stress-strain properties of vulcanized rubber or thermoplastic rubber”, and the tensile strength and elongation were recorded in Table 2.
[0107] The smaller the difference between the tensile strength and elongation of the dealcoholized silicone rubber measured at 70°C for 7d and 14d and the initially measured dealcoholized silicone rubber data, the higher the storage stability.
[0108] Table 2 According to the test data in Table 2, after the dealcoholized silicone rubber of Examples 1-3 was stored at 70° C. for 7 days and 14 days, the data was very close to the initial data, indicating that it has excellent storage stability.
[0109] Examples 1-3 show higher tensile strength than Comparative Examples 1, 3, and 5; although the dealcoholized silicone rubber of Comparative Examples 2 and 4 show higher tensile strength than Example 1 in the initial stage, the performance decreases rapidly after being stored at 70°C for 7d and 14d, and is not as stable as Example 1.
[0110] Regarding Comparative Example 2, the amount of silylene siloxane oligomer is excessive, so that the generated high-strength alkoxy-terminated 107 rubber has a large number of short-chain structures, low viscosity and excessive activity, which directly leads to poor storage stability of the prepared dealcoholized silicone rubber.
[0111] After being stored at 70°C for 7d and 14d, the dealcoholized silicone rubbers of Comparative Examples 1 and 3 have similar data to those measured initially, but their tensile strength in the initial state is not high, and their bonding strength with various substrates is not high, which makes it difficult to meet actual production needs.
[0112] Regarding Comparative Example 1, the performance of the high-strength alkoxy-terminated 107 rubber was affected because the end-vinyl silicone oil did not react sufficiently with the silylethylenesiloxane oligomer, resulting in low mechanical properties and bonding strength of the prepared dealcoholized silicone rubber.
[0113] According to Table 2, the strength and storage stability of the dealcoholized silicone rubber of Comparative Examples 4 and 5 are significantly different from those of Example 1. This indicates that the use of silicon-aza-cyclopentane compounds can indeed play a good role in removing water, capturing free alcohol, and enhancing the bonding performance to the contact substrate, and has a good matching effect with the high-strength alkoxy-terminated 107 glue.
[0114] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. High strength alkoxy terminated 107 glue, It is characterized in that Includes the following components: 100 parts by mass of end-side vinyl silicone oil; 3-10 parts by mass of silylene siloxane oligomer; 1-10ppm platinum catalyst; 06-0.25 parts by mass of A-171 vinyltrimethoxysilane; The ratio of the vinyl content of the end-side vinyl silicone oil to the hydrogen content of the silylethylenesiloxane oligomer is 1:(1-1.15); The ratio of the vinyl content of A-171 vinyltrimethoxysilane to the hydrogen content of silylethylenesiloxane oligomer is (1-1.25):
1.
2. The high-strength alkoxy-terminated 107 glue according to claim 1, Features: The ratio of the vinyl content of the terminal vinyl silicone oil to the hydrogen content of the silylethylenesiloxane oligomer is 1:(1.05-1.1); The ratio of the vinyl content of A-171 vinyltrimethoxysilane to the hydrogen content of silylethylenesiloxane oligomer is (1.1-1.2):
1.
3. The high-strength alkoxy-terminated 107 glue according to claim 1, Features: The viscosity of the end-side vinyl silicone oil is 500mPa.s-80000mPa.s.
4. A method for preparing the high-strength alkoxy-terminated 107 glue according to any one of claims 1 to 3, It is characterized in that The following steps are involved: Step 1: Mix terminal vinyl silicone oil, silylene siloxane oligomer and platinum catalyst, and react at 50-100° C. for 120-360 minutes to obtain a first reactant; Step 2: react the first reactant with A-171 vinyltrimethoxysilane at 50-100° C. for 60-120 min to obtain high-strength alkoxy-terminated 107 glue.
5. The method for preparing the high-strength alkoxy-terminated 107 glue according to claim 4, Features: The reaction temperature of step 1 and step 2 is 60°C. 6.De-alcoholized silicone rubber, It is characterized in that According to the mass parts, it includes the following components: 60-70 parts of high-strength alkoxy-terminated 107 glue, 1-6 parts of silicon-aza-cyclopentane compound, 10-15 parts of hydrophobic fumed silica, 1-3 parts of crosslinking agent, 0.1-0.5 parts of coupling agent, 0.1-0.5 parts of catalyst, and 5-10 parts of dimethyl silicone oil; The high-strength alkoxy-terminated 107 glue is the high-strength alkoxy-terminated 107 glue described in any one of claims 1 to 3 or the high-strength alkoxy-terminated 107 glue prepared by the preparation method of the high-strength alkoxy-terminated 107 glue described in any one of claims 4 to 5.
7. The dealcoholized silicone rubber according to claim 6, Features: The crosslinking agent includes a mixture of one or more of methyltrimethoxysilane and cyanoethyltrimethoxysilane.
8. The dealcoholized silicone rubber according to claim 6, Features: The silicon-aza-cyclopentane compound is prepared by reacting hexamethyldisilazane with an amino-functionalized diorganosiloxane oligomer.
9. The dealcoholized silicone rubber according to claim 6, Features: The synthesis of the silicon-aza-cyclopentane compound comprises the following steps: Step a: α,ω dihydroxy polydimethylsiloxane and aminopropyltrimethoxysilane are mixed in a mass ratio of (1.3-1.6):1, a small amount of formic acid aqueous solution is added dropwise, and the mixture is reacted at 55-65° C. for 0.5-1.5 h to obtain an amino-functionalized diorganosiloxane oligomer; Step b: Mix the amino-functionalized diorganosiloxane oligomer, hexamethyldisilazane and trimethylchlorosilane, and react at 95-105° C. for 7-9 hours to obtain a silicon-aza-cyclopentane compound.
10. A method for preparing the dealcoholized silicone rubber according to any one of claims 6 to 9, Features: The following steps are involved: Step A: mixing high-strength alkoxy-terminated 107 glue and dimethyl silicone oil at 30-50° C. under vacuum stirring for 5-10 minutes to obtain a first mixture; Step B: mixing the first mixture with the crosslinking agent, the coupling agent and the silicon-aza-cyclopentane compound under vacuum for 5-10 minutes to obtain a second mixture; Step C: vacuum-dispersing the second mixture and hydrophobic fumed silica for 15-30 minutes at high speed, and then dispersing them at high speed for 5-10 minutes while vacuuming to obtain a third mixture; Step D: Mix the third mixture with the catalyst under vacuum for 5-10 minutes to obtain dealcoholized silicone rubber.
Citation Information
Patent Citations
Alkoxyl end-capped dealcoholized silicone sealant and preparation method thereof
CN103756628A
Single-component low-viscosity fast-curing dealcoholization type RTV (Room Temperature Vulcanization) silicone rubber and preparation method thereof
CN114702676A
Alkoxy-terminated polysiloxane with self-adhesion characteristic as well as preparation method and application of alkoxy-terminated polysiloxane
CN115772264A
High-strength 107 glue as well as preparation method and application thereof
CN116179149A
Ultra-low viscosity liquid silicone rubber, cross-linking agent theerefo, and preparation method therefor
WO2023035283A1
Cited By
Alkoxy-terminated polysiloxane and preparation method thereof
CN121554495A
Silazane capping agent, capped polydimethylsiloxane, cured silicone rubber sealant, and preparation method and application thereof