Polyurethane / polyaryletherketone elastomer as well as preparation method and application thereof

By introducing polyaryletherketone oligomer into polyurethane elastomer, polyurethane/polyaryletherketone elastomer is solved, and the elasticity of polyurethane elastomer is achieved in the extremely cold environment is achieved. , suitable for extremely cold overseas exploration and artificial muscle materials.

CN118994602AActive Publication Date: 2024-11-22LANZHOU INSTITUTE OF CHEMICAL PHYSICS CHINESE ACADEMY OF SCIENCES

Patent Information

Application Number
CN202411101025.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-22
Estimated Expiration
2044-08-12

AI Technical Summary

Technical Problem

The elasticity of existing polyurethane elastomers in low temperature environments (<0℃) is greatly reduced, making it difficult to maintain a high elastic state, limiting their application in extreme environments.

Method used

By introducing the polyaryletherketone oligomer into the polyurethane elastomer, grafting reaction is carried out to form a polyurethane/polyaryletherketone elastomer, destroying the crystallinity of the polyether diol segments and improving the elastic properties under low temperature environments.

Benefits of technology

Under low temperature environment (<0℃), polyurethane/polyaryletherketone elastomers show excellent elastic properties, suitable for extremely cold overseas exploration sealing materials and artificial muscle materials, have broad application prospects, and are self-reinforced through mechanical training The effect matches the mechanical properties of skeletal muscle.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118994602A_ABST
    Figure CN118994602A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of polyurethane elastomers, and particularly relates to a polyurethane / polyaryletherketone elastomer as well as a preparation method and application thereof. The invention provides a polyurethane / polyaryletherketone elastomer. The polyurethane / polyaryletherketone elastomer comprises a polyurethane matrix and a polyaryletherketone oligomer grafted on the polyurethane matrix. The polyaryletherketone (oligomer) with a rigid structure is introduced into the polyurethane elastomer, so that the crystallinity of a polyether glycol chain segment in the polyurethane elastomer at a low temperature is destroyed, and the polyurethane / polyaryletherketone elastomer has excellent elasticity in a low-temperature environment (less than 0 DEG C); wide application prospects are realized in extremely cold overseas exploration materials or sealing materials; moreover, the mechanical training self-strengthening effect and typical strain self-adaptive strengthening of the polyurethane / polyaryletherketone elastomer provided by the invention are matched with the mechanical properties of skeletal muscles, and the polyurethane / polyaryletherketone elastomer has excellent application potential in the field of artificial muscle materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polyurethane elastomers, and in particular relates to a polyurethane / polyaryletherketone elastomer and a preparation method and application thereof. Background Art

[0002] Polyurethane elastomers have good elasticity, ductility and chemical resistance, and can be used in tires, cable sheaths, cushions, hoses or pipes. However, the operating temperature of existing polyurethane elastomers is basically above 0°C. When used in extreme environments such as Antarctica, the Moon, and Mars where there is not enough sunlight and the temperature is extremely low (below -30°C), the elasticity of the polymer elastomer drops significantly, making it difficult to maintain a high elastic state, which limits its application in low temperature environments (<0°C). Summary of the invention

[0003] The purpose of the present invention is to provide a polyurethane / polyaryletherketone elastomer and a preparation method and application thereof. The polyurethane / polyaryletherketone elastomer provided by the present invention has high elasticity in a low temperature environment (<0°C).

[0004] In order to achieve the above object, the present invention provides the following technical solutions:

[0005] The invention provides a polyurethane / polyaryletherketone elastomer, comprising a polyurethane matrix and a polyaryletherketone oligomer grafted on the polyurethane matrix.

[0006] Preferably, the mass ratio of the polyurethane matrix to the polyaryletherketone oligomer in the polyurethane / polyaryletherketone elastomer is 1:0.05-0.7.

[0007] Preferably, the preparation method of the polyurethane matrix comprises the following steps:

[0008] The polyether diol, diisocyanate, chain extender, polymerization catalyst and organic polar solvent are mixed and polymerized to obtain a polyurethane matrix.

[0009] Preferably, the polyether diol includes one or more of polytetrahydrofuran diol, propylene glycol polyether and trimethylolpropane polyether;

[0010] The diisocyanate includes one or more of isophorone diisocyanate, 4,4-diphenylmethane diisocyanate and 4,4-diisocyanate dicyclohexylmethane;

[0011] The polymerization catalyst includes dibutyltin dilaurate;

[0012] The molar ratio of the polyether diol to the diisocyanate is 1:3.5-4.5;

[0013] The mass ratio of the polyether diol to the polymerization catalyst is 1:0.001-0.008.

[0014] Preferably, the method for preparing the polyaryletherketone oligomer comprises the following steps:

[0015] 4,4-difluorobenzophenone, hexafluorobisphenol A, diphenolic acid, a polycondensation catalyst and a sulfone solvent are mixed to carry out a polycondensation reaction to obtain a polyaryletherketone oligomer.

[0016] Preferably, the molar ratio of hexafluorobisphenol A to 4,4-difluorobenzophenone is 1:1.6-2;

[0017] The molar ratio of the diphenolic acid to 4,4-difluorobenzophenone is 1:1.5-2;

[0018] Preferably, the polycondensation catalyst comprises potassium carbonate;

[0019] The mass ratio of the 4,4-difluorobenzophenone to the polycondensation catalyst is 1:1.05-1.30; the temperature of the polycondensation reaction is 130-190°C, and the time is 7.5-12 hours.

[0020] The present invention provides a method for preparing the polyurethane / polyaryletherketone elastomer described in the above technical solution, comprising the following steps:

[0021] The polyaryletherketone oligomer, polyurethane matrix and grafting catalyst are mixed and grafting reaction is carried out to obtain polyurethane / polyaryletherketone elastomer.

[0022] Preferably, the grafting catalyst comprises dibutyltin dilaurate;

[0023] The grafting reaction temperature is 60-80° C. and the time is 5-6.5 hours.

[0024] The present invention provides the use of the polyurethane / polyaryletherketone elastomer described in the above technical solution or the polyurethane / polyaryletherketone elastomer prepared by the preparation method described in the above technical solution in artificial muscle materials, extremely cold offshore exploration materials or sealing materials;

[0025] The operating temperature of the extremely cold overseas exploration material is ≤-30°C.

[0026] The present invention provides a polyurethane / polyaryletherketone elastomer, comprising a polyurethane matrix and a polyaryletherketone oligomer grafted onto the polyurethane matrix. The present invention introduces a polyaryletherketone (oligomer) with a rigid structure into the polyurethane elastomer, destroying the crystallinity of the polyether diol segment in the polyurethane elastomer at low temperatures, so that the polyurethane / polyaryletherketone elastomer has excellent elasticity in a low temperature environment (<0°C), and has broad application prospects in extremely cold offshore exploration sealing materials; moreover, the mechanical training self-reinforcement effect and typical strain adaptive reinforcement of the polyurethane / polyaryletherketone elastomer provided by the present invention match the mechanical properties of skeletal muscle, and has excellent application potential in the field of artificial muscle materials.

[0027] The preparation method provided by the invention has the advantages of simple operation, low cost and suitability for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0029] Figure 1 The stress-strain curves of the elastomers prepared in Examples 1 to 3 and Comparative Example 1 are shown;

[0030] Figure 2 This is a stress-strain curve of the polyurethane / polyaryletherketone elastomer prepared in Example 1 after mechanical training;

[0031] Figure 3 The stress-strain curves of the elastomers prepared in Examples 1 to 3 and Comparative Example 1 at -40°C;

[0032] Figure 4 The figure is a graph showing the change in tensile strength of the polyurethane / polyaryletherketone elastomer material prepared in Example 1 as a function of the number of cycles in a 100-cycle loading-unloading test;

[0033] Figure 5 The tear energy test diagram of the polyurethane / polyaryletherketone elastomer material prepared in Example 1;

[0034] Figure 6 The shape memory cycle curve of the polyurethane / polyaryletherketone elastomer material prepared in Example 1. DETAILED DESCRIPTION

[0035] The invention provides a polyurethane / polyaryletherketone elastomer, comprising a polyurethane matrix and a polyaryletherketone oligomer grafted on the polyurethane matrix.

[0036] In the present invention, unless otherwise specified, the required materials are commercially available products well known to those skilled in the art.

[0037] In the present invention, the mass ratio of the polyurethane matrix and the polyaryletherketone oligomer in the polyurethane / polyaryletherketone elastomer is preferably 1:0.05-0.7, more preferably 1:0.1-0.62, and most preferably 1:0.12-0.6; the tensile strength of the polyurethane / polyaryletherketone elastomer is preferably ≥30MPa, more preferably 33-70MPa, and most preferably 50-60MPa; the elongation at break of the polyurethane / polyaryletherketone elastomer is preferably ≥500%, more preferably 520-800%, and most preferably 650-750%.

[0038] In the present invention, the method for preparing the polyurethane matrix preferably comprises the following steps: mixing polyether diol, diisocyanate, chain extender, polymerization catalyst and organic polar solvent, and performing polymerization reaction to obtain the polyurethane matrix.

[0039] In the present invention, the polyether diol preferably includes one or more of polytetrahydrofuran diol, propylene glycol polyether and trimethylolpropane polyether, and more preferably polytetrahydrofuran diol.

[0040] In the present invention, the diisocyanate preferably includes one or more of isophorone diisocyanate (IPDI), 4,4-diphenylmethane diisocyanate (MDI) and 4,4-diisocyanate dicyclohexylmethane, and more preferably 4,4-diphenylmethane diisocyanate; the molar ratio of the polyether diol to the diisocyanate is preferably 1:3.5-4.5, more preferably 1:3.9-4.1, and most preferably 1:4-4.1.

[0041] In the present invention, the chain extender preferably includes one or more of 1,4-butanediol (BDO), 1,6-hexanediol and 1,8-octanediol; the mass ratio of the polyether diol to the chain extender is preferably 1:0.02-0.15, more preferably 1:0.03-0.14, and most preferably 1:0.04-0.12.

[0042] In the present invention, the polymerization catalyst preferably includes dibutyltin dilaurate; the mass ratio of the polyether diol to the polymerization catalyst is preferably 1:0.001-0.008, more preferably 1:0.002-0.006, and most preferably 1:0.004-0.005.

[0043] In the present invention, the organic polar solvent preferably includes one or more of N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAC), dimethyl sulfoxide (DMSO), toluene and tetrahydrofuran (THF); the ratio of the mass of the polyether diol to the volume of the organic polar solvent is preferably 1g:3-7mL, more preferably 1g:4.5-5.5mL, and most preferably 1g:4.8-5mL.

[0044] In the present invention, the mixing time is preferably 20 to 50 minutes, more preferably 30 to 40 minutes, and most preferably 30 to 35 minutes; the mixing preferably includes stirring mixing;

[0045] In the present invention, the polymerization reaction is preferably carried out under an inert gas atmosphere; the inert gas atmosphere preferably includes argon and / or nitrogen. In the present invention, the polymerization reaction temperature is preferably 75 to 85°C, more preferably 76 to 82°C, and most preferably 78 to 80°C; the polymerization reaction time is preferably 3.5 to 4.2 hours, more preferably 3.6 to 4.1 hours, and most preferably 3.9 to 4 hours.

[0046] In the present invention, the method for preparing the polyaryletherketone oligomer preferably comprises the following steps: mixing 4,4-difluorobenzophenone, hexafluorobisphenol A, diphenolic acid, a polycondensation catalyst and a sulfone solvent, and performing a polycondensation reaction to obtain the polyaryletherketone oligomer.

[0047] In the present invention, the molar ratio of hexafluorobisphenol A to 4,4-difluorobenzophenone is preferably 1:1.6-2, more preferably 1:1.83-1.86, and most preferably 1:1.84-1.85; the molar ratio of diphenolic acid to 4,4-difluorobenzophenone is preferably 1:1.5-2, more preferably 1:1.84-1.86, and most preferably 1:1.84-1.85.

[0048] In the present invention, the polycondensation catalyst preferably includes potassium carbonate, more preferably anhydrous potassium carbonate; the mass ratio of the 4,4-difluorobenzophenone to the polycondensation catalyst is preferably 1:1.05-1.3, more preferably 1:1.14-1.16, and most preferably 1:1.14-1.15.

[0049] In the present invention, the sulfone solvent preferably includes tetramethylene sulfone and / or cyclopentane sulfone; the ratio of the mass of the 4,4-difluorobenzophenone to the volume of the sulfone solvent is preferably 1 g: 5 to 8 mL, more preferably 1 g: 5.5 to 6.5 mL, and most preferably 1 g: 5.8 to 6 mL.

[0050] In the present invention, the polycondensation reaction is preferably carried out under an inert gas atmosphere; the inert gas atmosphere preferably includes argon and / or nitrogen. In the present invention, the temperature of the polycondensation reaction is preferably 130 to 190° C.; the time of the polycondensation reaction is preferably 7.5 to 12 hours, more preferably 8 to 11 hours, and most preferably 9 to 10 hours.

[0051] In the present invention, the polycondensation reaction preferably includes a first polycondensation reaction and a second polycondensation reaction in sequence. In the present invention, the temperature of the first polycondensation reaction is preferably 130-150°C, more preferably 135-145°C, and most preferably 138-140°C; the time of the first polycondensation reaction is preferably 2.5-4h, more preferably 2.8-3.5h, and most preferably 3-3.2h; the temperature of the second polycondensation reaction is preferably 180-200°C, more preferably 180-195°C, and most preferably 185-190°C; the time of the second polycondensation reaction is preferably 5-8h, more preferably 5.5-6.5h, and most preferably 6-7h.

[0052] After completing the first polycondensation reaction, the present invention preferably further comprises dehydrating the first polycondensation reaction liquid obtained by the first polycondensation reaction. In the present invention, the dehydrating agent used for the dehydration preferably comprises toluene; the volume ratio of the first polycondensation reaction liquid to the dehydrating agent is preferably 1:0.2-0.4, more preferably 1:0.3-0.35, and most preferably 1:0.32-0.34. The present invention promotes the polycondensation reaction to proceed in the forward direction by dehydrating the reaction system.

[0053] After the polycondensation reaction is completed, the present invention preferably further comprises pouring the reaction solution obtained from the polycondensation reaction into water, adjusting the pH value to 5.5-7, performing solid-liquid separation, and washing and drying the obtained solid.

[0054] In the present invention, the volume of water is preferably greater than the volume of the reaction solution. In the present invention, the adjusted pH value is preferably 5.5-7, more preferably 6-7; the acid used to adjust the pH value is preferably dilute hydrochloric acid; the present invention has no special limitation on the concentration of the dilute hydrochloric acid, and the dilute hydrochloric acid well known to those skilled in the art can be used to adjust the pH value of the system to 5.5-7, such as 11.5-12.5 mol / L. The present invention has no special limitation on the solid-liquid separation method, and the solid-liquid separation method well known in the art can be used, and it is specifically preferred to perform sedimentation and filtration in sequence. In the present invention, the washing includes alcohol washing and water washing in sequence; the alcohol for the alcohol washing preferably includes one or more of methanol, ethanol and isopropanol, more preferably methanol; the number of alcohol washing and water washing is independently preferably 2-4 times, more preferably 3 times. In the present invention, the drying temperature is preferably 60-80°C, more preferably 70-80°C, most preferably 75-80°C; the drying time is preferably 24-48h, more preferably 24-40h, most preferably 24-36h.

[0055] The present invention provides a method for preparing the polyurethane / polyaryletherketone elastomer described in the above technical solution, comprising the following steps:

[0056] The polyaryletherketone oligomer, polyurethane matrix and grafting catalyst are mixed and grafting reaction is carried out to obtain polyurethane / polyaryletherketone elastomer.

[0057] In the present invention, the polyurethane matrix is ​​preferably used in the form of a polyurethane solution; the polyurethane solution is preferably a reaction liquid for preparing the polyurethane matrix. In the present invention, the ratio of the mass of the polyaryletherketone oligomer to the volume of the polyurethane solution is preferably 1g:5-40mL, more preferably 1g:8-38mL, and most preferably 1g:8.2-35mL.

[0058] In the present invention, the grafting catalyst preferably includes dibutyltin dilaurate; the mass ratio of the polyaryletherketone oligomer to the grafting catalyst is preferably 1:0.001-0.025, more preferably 1:0.005-0.02, and most preferably 1:0.001-0.015.

[0059] In the present invention, the temperature of the grafting reaction is preferably 60 to 80°C, more preferably 75 to 80°C, and most preferably 76 to 78°C; the time of the grafting reaction is preferably 5 to 6.5 hours, more preferably 5.5 to 6.2 hours, and most preferably 5.8 to 6 hours. After completing the grafting reaction, the present invention preferably further comprises degassing, curing, and drying the grafted product obtained by the grafting reaction in sequence, and demolding after cooling to room temperature to obtain a polyurethane / polyaryletherketone elastomer.

[0060] In the present invention, the degassing preferably further comprises pouring the reaction solution obtained from the grafting reaction into a mold; the degassing temperature is preferably 75-85°C, more preferably 76-82°C, and most preferably 78-80°C.

[0061] In the present invention, the curing temperature is preferably 75-85°C, more preferably 76-82°C, most preferably 78-80°C; the curing time is preferably 20-26h, more preferably 21-25h, most preferably 23-24h.

[0062] In the present invention, the drying temperature is preferably 45-50°C, more preferably 46-49°C, most preferably 47-48°C; the drying time is preferably 30-50h, more preferably 35-45h, most preferably 38-42h.

[0063] The present invention provides the use of the polyurethane / polyaryletherketone elastomer described in the above technical scheme or the polyurethane / polyaryletherketone elastomer prepared by the preparation method described in the above technical scheme in artificial muscle materials, extremely cold overseas exploration materials or sealing materials; the use temperature of the extremely cold overseas exploration materials is ≤-30°C. The polyurethane / polyaryletherketone elastomer provided by the present invention has excellent elasticity in a low temperature environment (<0°C), and has broad application prospects in extremely cold overseas exploration materials or sealing materials with a use temperature of ≤-30°C; moreover, the mechanical training self-reinforcement effect and typical strain adaptive reinforcement of the polyurethane / polyaryletherketone elastomer provided by the present invention match the mechanical properties of skeletal muscle, and has excellent application potential in the field of artificial muscle materials.

[0064] In order to further illustrate the present invention, a polyurethane / polyaryletherketone elastomer provided by the present invention and its preparation method and application are described in detail below in conjunction with the accompanying drawings and embodiments, but they should not be construed as limiting the scope of protection of the present invention.

[0065] In all the embodiments and comparative examples of the present invention, the tensile testing machine used is a Shimadzu AG-X (5000N) electronic universal testing machine.

[0066] Example 1

[0067] 16.15g 4,4-difluorobenzophenone, 13.45g hexafluorobisphenol A and 11.45g diphenolic acid were dissolved in 100mL cyclopentane sulfone, and 11.8852g anhydrous potassium carbonate was added as a catalyst. The obtained mixed solution was subjected to polycondensation reaction for 3h under argon atmosphere at 140°C, and 30mL toluene was used to remove the water generated by the polycondensation reaction, and then the reaction system was heated to 190°C for polycondensation reaction for 6h. After the polycondensation reaction was completed, the obtained reaction solution (gray-brown viscous liquid) was poured into excess deionized water, and the pH value was adjusted to 6-7 with dilute hydrochloric acid with a concentration of 12.1mol / L to precipitate the obtained polyaryletherketone. The precipitate obtained by precipitation was filtered, and the filter residue was washed with methanol and water three times respectively, and then vacuum dried in an oven at 80°C for 24h to obtain polyaryletherketone (beige).

[0068] 10g of polytetrahydrofuran diol was added to a three-necked flask with mechanical stirring, and 1.13g of 1,4-butanediol and 50mL of N,N-dimethylformamide were added. The mixture was stirred evenly under a nitrogen atmosphere, and the stirring was continued for 30 minutes to fully dissolve and evenly mix the polytetrahydrofuran diol polyether diol and 1,4-butanediol. 5.125g of 4,4-diphenylmethane diisocyanate was dissolved in 20mL of N,N-dimethylformamide. After the mixture was fully dissolved, 0.05mL of dibutyltin dilaurate was added and stirred evenly. The obtained solution was added to the above three-necked flask, and the polymerization reaction was carried out at 80°C and under a nitrogen atmosphere for 4 hours to obtain a polyurethane solution.

[0069] 2.38 g of the obtained polyaryletherketone was dissolved in 20 mL of N,N-dimethylformamide, and 0.05 mL of dibutyltin dilaurate was added. After mixing evenly, the obtained polyurethane solution was added and the grafting reaction was carried out for 6 hours. After the reaction was completed, the obtained reaction solution was poured into a polytetrafluoroethylene mold and degassed in a vacuum oven at 80°C, cured in a blast oven at 80°C for 24 hours, and dried in a vacuum oven at 50°C for 40 hours. After cooling to room temperature, the mold was demolded to obtain a polyurethane / polyaryletherketone elastomer.

[0070] Example 2

[0071] 16.15g 4,4-difluorobenzophenone, 13.45g hexafluorobisphenol A and 11.45g diphenolic acid were dissolved in 100mL cyclopentane sulfone, and 11.8852g anhydrous potassium carbonate was added as a catalyst. The obtained mixed solution was subjected to polycondensation reaction for 3h under argon atmosphere at 140°C, and 30mL toluene was used to remove the water generated by the polycondensation reaction, and then the reaction system was heated to 190°C for polycondensation reaction for 6h. After the polycondensation reaction was completed, the obtained reaction solution (gray-brown viscous liquid) was poured into excess deionized water, and the pH value was adjusted to 6-7 with dilute hydrochloric acid with a concentration of 12.1mol / L to precipitate the obtained polyaryletherketone. The precipitate obtained by precipitation was filtered, and the filter residue was washed with methanol and water three times respectively, and then vacuum dried in an oven at 80°C for 24h to obtain polyaryletherketone (beige).

[0072] 10g of polytetrahydrofuran diol was added to a three-necked flask with mechanical stirring, and 1.01g of 1,4-butanediol and 50mL of N,N-dimethylformamide were added. The mixture was stirred evenly under a nitrogen atmosphere, and the stirring was continued for 30 minutes to fully dissolve and evenly mix the polytetrahydrofuran diol polyether diol and 1,4-butanediol. 5.125g of 4,4-diphenylmethane diisocyanate was dissolved in 20mL of N,N-dimethylformamide. After the mixture was fully dissolved, 0.05mL of dibutyltin dilaurate was added and stirred evenly. The obtained solution was added to the above three-necked flask, and the polymerization reaction was carried out at 80°C and under a nitrogen atmosphere for 4 hours to obtain a polyurethane solution.

[0073] 3.57 g of the obtained polyaryletherketone was dissolved in 20 mL of N,N-dimethylformamide, and 0.05 mL of dibutyltin dilaurate was added. After mixing evenly, the obtained polyurethane solution was added and the grafting reaction was carried out for 6 hours. After the reaction was completed, the obtained reaction solution was poured into a polytetrafluoroethylene mold and degassed in a vacuum oven at 80°C, cured in a blast oven at 80°C for 24 hours, and dried in a vacuum oven at 50°C for 40 hours. After cooling to room temperature, the mold was demolded to obtain a polyurethane / polyaryletherketone elastomer.

[0074] Example 3

[0075] 16.15g 4,4-difluorobenzophenone, 13.45g hexafluorobisphenol A and 11.45g diphenolic acid were dissolved in 100mL cyclopentane sulfone, and 11.8852g anhydrous potassium carbonate was added as a catalyst. The obtained mixed solution was subjected to polycondensation reaction for 3h under argon atmosphere at 140°C, and 30mL toluene was used to remove the water generated by the polycondensation reaction, and then the reaction system was heated to 190°C for polycondensation reaction for 6h. After the polycondensation reaction was completed, the obtained reaction solution (gray-brown viscous liquid) was poured into excess deionized water, and the pH value was adjusted to 6-7 with dilute hydrochloric acid with a concentration of 12.1mol / L to precipitate the obtained polyaryletherketone. The precipitate obtained by precipitation was filtered, and the filter residue was washed with methanol and water three times respectively, and then vacuum dried in an oven at 80°C for 24h to obtain polyaryletherketone (beige).

[0076] 10g of polytetrahydrofuran diol was added to a three-necked flask with mechanical stirring, and 0.451g of 1,4-butanediol and 50mL of N,N-dimethylformamide were added. The mixture was stirred evenly under a nitrogen atmosphere, and the stirring was continued for 30 minutes to fully dissolve and evenly mix the polytetrahydrofuran diol polyether diol and 1,4-butanediol. 5.125g of 4,4-diphenylmethane diisocyanate was dissolved in 20mL of N,N-dimethylformamide. After the mixture was fully dissolved, 0.05mL of dibutyltin dilaurate was added and stirred evenly. The obtained solution was added to the above three-necked flask, and the polymerization reaction was carried out at 80°C and under a nitrogen atmosphere for 4 hours to obtain a polyurethane solution.

[0077] 9.52 g of the obtained polyaryletherketone was dissolved in 20 mL of N,N-dimethylformamide, and 0.05 mL of dibutyltin dilaurate was added. After mixing evenly, the obtained polyurethane solution was added and the grafting reaction was carried out for 6 hours. After the reaction was completed, the obtained reaction solution was poured into a polytetrafluoroethylene mold and degassed in a vacuum oven at 80°C, cured in a blast oven at 80°C for 24 hours, and dried in a vacuum oven at 50°C for 40 hours. After cooling to room temperature, the mold was demolded to obtain a polyurethane / polyaryletherketone elastomer.

[0078] Comparative Example 1

[0079] 10g of polytetrahydrofuran diol was added to a three-necked flask with mechanical stirring, and 1.35g of 1,4-butanediol and 50mL of N,N-dimethylformamide were added. The mixture was stirred evenly under nitrogen atmosphere, and the stirring was continued for 30 minutes to fully dissolve and evenly mix the polytetrahydrofuran diol polyether diol and 1,4-butanediol. 5.125g of 4,4-diphenylmethane diisocyanate was dissolved in 20mL of N,N-dimethylformamide. After the mixture was fully dissolved, 0.05mL of dibutyltin dilaurate was added and stirred evenly. The obtained solution was added to the above three-necked flask, and the polymerization reaction was carried out at 80°C and nitrogen atmosphere for 4h. The obtained reaction solution was poured into a polytetrafluoroethylene mold, and degassed in a vacuum oven at 80°C, cured in a blast oven at 80°C for 24h, and dried in a vacuum oven at 50°C for 40h. After cooling to room temperature, the mold was demoulded to obtain a pure polyurethane elastomer.

[0080] The properties of the polyurethane / polyaryletherketone elastomers prepared in Examples 1 to 3 and the polyurethane elastomer prepared in Comparative Example 1 were tested. The test results are shown in Tables 1 and Figures 1 to 6 The test method is as follows:

[0081] The mechanical properties (tensile strength and elongation at break) of the prepared elastomer at room temperature were tested using a universal testing machine at a tensile speed of 100 mm / min. The sample shape was cut into a dumbbell shape according to the international standard GB / T528-2009.

[0082] The shape memory performance (elasticity) of the polyurethane / polyaryletherketone elastomer prepared in Example 1 was tested using a TA 850 dynamic thermomechanical analyzer. The polyurethane / polyaryletherketone elastomer was cut into a size of 20mm×3mm×0.2mm, then heated to 30°C, stretched to 50% at a deformation rate of 5% / min; maintained at a deformation rate of 50%, cooled to -50°C at 5°C / min; the external force was removed, the temperature was raised to 30°C, and maintained for 20 minutes. The above thermodynamic process was repeated 4 times;

[0083] The polyurethane / polyaryletherketone elastomer prepared in Example 1 was subjected to mechanical training enhancement test using a universal testing machine at a tensile rate of 100 mm / min. A cyclic loading and unloading tensile test was performed at a strain of 150%. After 10 loading and unloading cycles, the rectangular specimen was cut into a dumbbell shape according to GB / T528-2009. After the loading and unloading cycles, the mechanical properties of the specimen were tested at a tensile rate of 100 mm / min at room temperature.

[0084] The polyurethane / polyaryletherketone elastomer prepared in Example 1 was subjected to mechanical training enhancement test using a universal testing machine at a tensile rate of 100 mm / min. 100 cycles of loading and unloading tensile tests were performed at a strain of 100% to examine its anti-fatigue performance.

[0085] The elastomers prepared in Examples 1 to 3 and Comparative Example 1 were cut into specimens with a single-side notch shape, and the notch length was 1 mm. The specimens were subjected to a tensile test at room temperature using a universal testing machine to test the fracture energy of the specimens. Under the conditions of a tensile speed of 3 mm / min, a gauge length of 10 mm, and a width of 5 mm, the notched and non-notched specimens were tested, and the tear energy of the specimens was calculated, and the calculation formula is shown in Formula I:

[0086]

[0087] Where c = 1 mm represents the notch length, λ represents the elongation at break of the notched specimen, and w represents the area of ​​the stress-strain curve of the unnotched specimen integrated to λ.

[0088] Table 1 Comparison of mechanical properties of the elastomers prepared in Examples 1 to 3 and Comparative Example 1

[0089] Test items Example 1 Example 2 Example 3 Comparative Example 1 Tensile strength(MPa) 58.82±2.54 55.63±4.37 33.64±2.57 21.7±1.45 Elongation at break (%) 771.45±33.47 729.24±27.89 520.67±45.94 697.13±52.86 <![CDATA[Toughness (MJ / m 3 )]]> 183.77±11.03 164.08±16.44 73.43±13.63 89.10±11.64

[0090] Figure 1 The stress-strain curves of the elastomers prepared in Examples 1 to 3 and Comparative Example 1 are shown in Tables 1 and Figure 1 It can be seen that the polyurethane / polyaryletherketone elastomers prepared in Examples 1 to 3 have relatively high mechanical properties, and the mechanical properties of the polyurethane elastomer can be regulated by regulating the content of the polyaryletherketone oligomer.

[0091] Figure 2 The stress-strain curve of the polyurethane / polyaryletherketone elastomer prepared in Example 1 after mechanical training. Figure 2 It can be seen that the mechanical strength and elastic modulus of the polyurethane / polyaryletherketone elastomer prepared in Example 1 are significantly improved after 10 loading-unloading cycle tests under different strains. This is mainly because the semi-crystalline polyaryletherketone polymer forms oriented crystals during the stretching process, and the dynamic dissociation and combination of high-density hydrogen bonds in the polymer network interlock the oriented structure, thereby improving the mechanical strength of the elastomer in the subsequent stretching process.

[0092] Figure 3 The stress-strain curves of the elastomers prepared in Examples 1 to 3 and Comparative Example 1 at -40°C are shown in FIG. Figure 3It can be seen that the polyurethane / polyaryletherketone elastomers prepared in Examples 1 to 3 have relatively high mechanical properties at low temperatures, and the mechanical properties of the elastomers at low temperatures can be regulated by adjusting the content of polyaryletherketone.

[0093] Figure 4 The figure is a graph showing the change in tensile strength of the polyurethane / polyaryletherketone elastomer material prepared in Example 1 as a function of the number of cycles in a 100-cycle loading-unloading test. Figure 4 It can be seen that the polyurethane / polyaryletherketone elastomer prepared in Example 1 has good fatigue resistance. After 100 loading-unloading cycle tests, its mechanical strength has not been significantly reduced. This excellent performance helps to improve the sealing performance of the material.

[0094] Figure 5 This is a tear energy test diagram of the polyurethane / polyaryletherketone elastomer material prepared in Example 1. Figure 5 It can be seen that the polyurethane / polyaryletherketone elastomer prepared in Example 1 has good tear resistance, and its tear energy is greater than 40 kJ / m 2 The semi-crystalline rigid structure of polyaryletherketone can avoid stress concentration and prevent crack propagation.

[0095] Figure 6 The shape memory cycle curve of the polyurethane / polyaryletherketone elastomer material prepared in Example 1. Figure 6 It can be seen that the polyurethane / polyaryletherketone elastomer prepared in Example 1 has good low-temperature shape memory performance, and its shape fixation rate and shape recovery rate are both greater than 95%.

[0096] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. Other embodiments can be obtained based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.

Claims

1. A polyurethane / polyaryletherketone elastomer, It is characterized in that The invention comprises a polyurethane matrix and a polyaryletherketone oligomer grafted on the polyurethane matrix.

2. The polyurethane / polyaryletherketone elastomer according to claim 1, It is characterized in that The mass ratio of the polyurethane matrix to the polyaryletherketone oligomer in the polyurethane / polyaryletherketone elastomer is 1:0.05-0.

7.

3. The polyurethane / polyaryletherketone elastomer according to claim 1, It is characterized in that The preparation method of the polyurethane matrix comprises the following steps: The polyether diol, diisocyanate, chain extender, polymerization catalyst and organic polar solvent are mixed and polymerized to obtain a polyurethane matrix.

4. The polyurethane / polyaryletherketone elastomer according to claim 3, It is characterized in that The polyether diol includes one or more of polytetrahydrofuran diol, propylene glycol polyether and trimethylolpropane polyether; The diisocyanate includes one or more of isophorone diisocyanate, 4,4-diphenylmethane diisocyanate and 4,4-diisocyanate dicyclohexylmethane; The polymerization catalyst includes dibutyltin dilaurate; The molar ratio of the polyether diol to the diisocyanate is 1:3.5-4.5; The mass ratio of the polyether diol to the polymerization catalyst is 1:0.001-0.

008.

5. The polyurethane / polyaryletherketone elastomer according to claim 1, It is characterized in that The preparation method of the polyaryletherketone oligomer comprises the following steps: 4,4-difluorobenzophenone, hexafluorobisphenol A, diphenolic acid, a polycondensation catalyst and a sulfone solvent are mixed to carry out a polycondensation reaction to obtain a polyaryletherketone oligomer.

6. The polyurethane / polyaryletherketone elastomer according to claim 5, It is characterized in that The molar ratio of hexafluorobisphenol A to 4,4-difluorobenzophenone is 1:1.6-2; The molar ratio of the diphenolic acid to 4,4-difluorobenzophenone is 1:1.5-2.

7. The polyurethane / polyaryletherketone elastomer according to claim 5 or 6, It is characterized in that The polycondensation catalyst includes potassium carbonate; The mass ratio of the 4,4-difluorobenzophenone to the polycondensation catalyst is 1:1.05-1.30; the temperature of the polycondensation reaction is 130-190°C, and the time is 7.5-12 hours.

8. The method for preparing the polyurethane / polyaryletherketone elastomer according to any one of claims 1 to 7, It is characterized in that The following steps are involved: The polyaryletherketone oligomer, polyurethane matrix and grafting catalyst are mixed and grafting reaction is carried out to obtain polyurethane / polyaryletherketone elastomer.

9. The preparation method according to claim 8, It is characterized in that The grafting catalyst includes dibutyltin dilaurate; The grafting reaction temperature is 60-80° C. and the time is 5-6.5 hours.

10. Use of the polyurethane / polyaryletherketone elastomer according to any one of claims 1 to 7 or the polyurethane / polyaryletherketone elastomer prepared by the preparation method according to any one of claims 8 to 9 in artificial muscle materials, extremely cold offshore exploration materials or sealing materials; The operating temperature of the extremely cold offshore exploration sealing material is ≤-30°C.

Citation Information

Patent Citations

  • Carboxyl-containing polyetheretherketone-modified acrylic water-based resin

    CN109337020A

  • Environment-friendly coating of polyaryletherketone modified waterborne polyurethane resin

    CN112876977A

  • Polyaryletherketone oligomer with side group containing carboxyl, thermosetting shape memory polyaryletherketone and preparation method of thermosetting shape memory polyaryletherketone

    CN116715842A

  • Polyaryletherketone with carboxyl-containing side chain and preparation method of polyaryletherketone

    CN118146497A

  • Polyarylene sulfide composition

    JP2006045293A

Cited By

  • Methacrylate-terminated polyurethane prepolymer, preparation method and two-component dual-curing photosensitive resin