Ready-to-use hydrogel as well as preparation method and application thereof

By introducing bisphosphonic acid groups onto pectin and binding them with metal ions to form a hydrogel, the problems of low cell activity and dryness maintenance in cell sphere culture are solved, providing a convenient three-dimensional cell culture material that promotes cell adhesion and proliferation and is suitable for three-dimensional culture of various cell types.

CN118994644AActive Publication Date: 2024-11-22SOUTH CHINA UNIV OF TECH

Patent Information

Application Number
CN202411251204.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-06
Publication Date
2024-11-22
Estimated Expiration
2044-09-06

AI Technical Summary

Technical Problem

Existing technologies produce cell spheres with problems such as low cell activity and inability to maintain cell stemness. While pectin hydrogels are widely used in drug delivery, there is a lack of materials that are simple to prepare, easy to operate, and have excellent mechanical properties for three-dimensional culture.

Method used

By introducing bisphosphonic acid groups onto pectin and utilizing the binding ability of bisphosphonic acid with divalent metal ions, a monovalent metal ion solution is added to form a hydrogel, thus preparing a ready-to-use hydrogel kit suitable for cell culture.

Benefits of technology

The prepared hydrogel promotes cell adhesion, proliferation and differentiation, has better cell spheroidization effect, has a wide range of material sources, is easy to use, adapts to the needs of cell culture in multiple scenarios, and has excellent mechanical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005032331570000051
    Figure BDA0005032331570000051
  • Figure HDA0005032331580000011
    Figure HDA0005032331580000011
  • Figure HDA0005032331580000012
    Figure HDA0005032331580000012
Patent Text Reader

Abstract

The invention belongs to the field of hydrogel materials, and relates to a preparation method of hydrogel, which comprises the following steps: dissolving diphosphonic acid modified pectin in water or an aqueous solution, adding a divalent metal cation solution, mixing to obtain a precursor solution, adding a gelling solution to initiate crosslinking to form hydrogel, and drying to obtain the hydrogel. Wherein the gelling solution is a solution containing monovalent metal ions and having a pH value of 7-9. The hydrogel has a wide application prospect in the field of ready-to-use reagents. The precursor solution is added to a cell culture device and lyophilized, and can be used for preparing a ready-to-use kit. Dropwise adding a cell suspension into the ready-to-use hydrogel kit, and adding a cell culture solution to obtain the hydrogel encapsulated with cells for three-dimensional culture.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of hydrogel materials, and specifically relates to a hydrogel for 3D cell culture and a preparation method thereof. Background Art

[0002] Hydrogels are three-dimensional polymer networks with high water content and good biocompatibility. Since hydrogels can mimic many aspects of the natural extracellular matrix, they have become the main candidates for therapeutic drug and cell delivery carriers in biomedical engineering. Compared with static hydrogels cross-linked by covalent chemical crosslinking, physically cross-linked dynamic hydrogels can better mimic the dynamic structural characteristics of the natural extracellular matrix and regulate cell activities, including adhesion, migration, proliferation, differentiation, polarization and apoptosis, through cell mechanical transduction signals. The use of hydrogels to establish cell-to-cell interactions is crucial for the in vitro three-dimensional culture of stem cells and multicellular structures (such as in vitro tumors and organoids).

[0003] In tissue engineering and regenerative medicine, stem cell and tumor cell sphere culture are both of great significance. As seed cells for cell therapy and tissue and organ replacement therapy, stem cells can be used as carriers for disease gene therapy and for establishing drug screening platforms. Cell spheres can improve the therapeutic effect of stem cells by increasing cell survival rate, enhancing cytokine secretion and maintaining cell pluripotency. For tumor cells, due to their morphology and spatial arrangement, cell spheres are more accurate in drug screening than the results obtained by 2D cultured cells. 3D cells can simulate several important characteristics of tumors and microenvironments, including phenotypic heterogeneity, growth dynamics and cell-to-cell interactions. However, there are a series of problems with the cell spheres produced in the prior art, such as low cell activity and inability to maintain cell stemness. The emergence of the above problems is often related to the materials used to produce cell spheres. Therefore, it is an urgent problem to prepare a hydrogel material with a simple process that can culture stem cells and maintain the stemness of tumor cell spheres.

[0004] Pectin is a natural polymer compound with good gelation and emulsification stabilization effects, and has been widely used in food, medicine, daily chemicals and textile industries. The carboxyl group and divalent metal ions in pectin have strong ion coordination effects. It has been reported in the prior art that the free carboxyl ions on low-ester pectin interact with the free divalent calcium ions to form a three-dimensional rigid hydrogel. CN114502712A discloses a pectin acid-based hydrogel that can be used to culture cells. Pectin acid or salt is added with a cross-linking agent including a salt of a divalent ion, and a proton donor to obtain a hydrogel, and the proton donor is hydrolyzed in an aqueous solution to form an acid lactone, ester or other compound. However, there are many reports on the use of pectin hydrogels for drug delivery, and there is still a need to research and develop more pectin hydrogels that can be used for three-dimensional culture, which are simple to prepare, easy to operate, and have excellent mechanical properties. Summary of the invention

[0005] In view of the needs in the above-mentioned prior art, the object of the present invention is to provide a new method for preparing a hydrogel, which comprises the following steps: dissolving bisphosphonic acid-modified pectin in water or an aqueous solution, adding a divalent metal cation solution to mix to obtain a precursor solution, and adding a gelling solution to initiate crosslinking to form a hydrogel, wherein the gelling solution is a solution containing monovalent metal ions with a pH of 7-9.

[0006] The bisphosphonic acid in the bisphosphonic acid-modified pectin includes, but is not limited to, one or more of pamidronic acid, tiludronic acid, alendronic acid, neridronic acid, olpadronic acid, and ibandronic acid. The pectin modified with the bisphosphonic acid group is added to a metal divalent ion solution to form a precursor solution, and no gelling reaction occurs. When a solution containing monovalent metal ions is added, the pectin quickly gels to form a hydrogel.

[0007] In certain embodiments, the divalent metal cation solution includes but is not limited to metal cations Mg 2+ , Ca 2+ , Sr. 2+ , Ba 2+ , Mn 2+ , Fe 2+ ,Co 2+ , Ni 2+ , Cu 2+ , Zn 2+ The monovalent metal ion solution includes but is not limited to Na + , K + wait.

[0008] In certain embodiments, the gelling solution is an aqueous solution containing monovalent metal ions, a physiological buffer solution or a cell culture medium; the culture medium includes but is not limited to MEM, DMEM, αMEM, IMDM and RPMI-1640.

[0009] In some embodiments, the grafting rate of bisphosphonic acid-modified pectin is 5%-20%; in some embodiments, the mass percentage of bisphosphonic acid-modified pectin in the precursor solution is 0.5-10%, preferably 1%-6%, and the concentration of divalent metal cations is not less than 50mM; after adding the gelling solution, the concentration range of monovalent metal cations is 100-300mM.

[0010] In some embodiments, the preparation method of the bisphosphonic acid modified pectin comprises grafting bisphosphonic acid to pectin molecules through an amidation reaction, and preferably the bisphosphonic acid group is one or more of pamidronate, alendronate, neridronate or ibandronate. In some preferred embodiments, the preparation method of the bisphosphonic acid modified pectin comprises dissolving the bisphosphonic acid compound in a buffer, adding pectin and NHS to mix, slowly dripping an aqueous solution of EDC into the above-mentioned pectin mixed solution, and continuously stirring the reaction at room temperature. After adding hydroxylamine hydrochloride to the reactant, dialyzing and then freeze-drying.

[0011] Another object of the present invention is to provide a ready-to-use hydrogel kit. The kit includes a hydrogel precursor, which is a freeze-dried product of a mixed solution containing bisphosphonic acid-modified pectin and divalent metal cations. After adding a gelling solution to the kit, a hydrogel is formed, and the gelling solution is a solution with a pH of 7-9 containing monovalent metal cations.

[0012] In certain embodiments, the divalent metal cations in the mixed solution include but are not limited to Mg. 2+ , Ca 2+ , Sr. 2+ , Ba 2+ , Mn 2+ , Fe 2+ ,Co 2+ , Ni 2+ , Cu 2+ , Zn 2+ One or more of; the monovalent metal cation is Na + or K + At least one of .

[0013] In certain embodiments, the bisphosphonic acid in the bisphosphonic acid-modified pectin includes, but is not limited to, one or more of pamidronic acid, tiludronic acid, alendronic acid, neridronic acid, olpadronic acid, and ibandronic acid.

[0014] In certain embodiments, the bisphosphonic acid-modified pectin is further grafted with a short peptide group, preferably, the short peptide group is an RGD group. The hydrogel precursor is a freeze-dried product of a mixed solution containing pectin modified with bisphosphonic acid and RGD groups (PT-BP-RGD) and divalent metal cations.

[0015] In certain embodiments, the preparation method of the pectin modified with bisphosphonic acid and RGD groups is as follows: dissolving pectin in a buffer solution, reacting with an RGD peptide at room temperature in the presence of EDC and sulfo-NHS. Weighing a bisphosphonic acid compound and dissolving it in the above reaction solution, adding NHS and EDC, reacting at room temperature, and then adding hydroxylamine hydrochloride to terminate the reaction. The resulting solution is dialyzed and freeze-dried to obtain PT-BP-RGD.

[0016] Another object of the present application is to provide a method for preparing a ready-to-use hydrogel kit, comprising the following steps: 1) mixing a bisphosphonic acid-modified pectin solution and a solution containing divalent metal cations to obtain a precursor solution, adding the precursor solution into a cell culture device, and freeze-drying to obtain a ready-to-use hydrogel kit.

[0017] In certain embodiments, the method for preparing the bisphosphonic acid-modified pectin comprises grafting bisphosphonic acid onto pectin molecules through an amidation reaction, and preferably the bisphosphonic acid group is pamidronic acid, alendronic acid, neridronic acid or ibandronic acid.

[0018] Another object of the present application is to provide a method for culturing cells using the ready-to-use hydrogel kit, comprising the following steps: dropping a cell suspension into the ready-to-use hydrogel kit, adding a cell culture fluid / culture medium, and allowing the hydrogel to stand to obtain cell-encapsulated hydrogels for three-dimensional culture.

[0019] In certain embodiments, the lyophilized materials in the kit are first sterilized before use in cell culture.

[0020] In some embodiments, the method further comprises adding an EDTA solution to the hydrogel to degrade the hydrogel and recover the cells. For example, when an EDTA solution of not less than 10 mM is added to the hydrogel, the hydrogel can be degraded and the cells can be recovered by standing.

[0021] Beneficial technical effects

[0022] The technical solution of the present application is to introduce bisphosphonic acid groups into pectin to increase its binding ability with divalent metal ions, thereby enhancing the coordination between pectin molecules. After the modified pectin and divalent metal ions are mixed, a gelling solution is added to initiate gelling. In some embodiments, the gelling solution contains sodium ions or potassium ions, and these monovalent metal ions are commonly present in buffer solutions or cell culture media. Therefore, the hydrogel can be quickly gelled by adding conventional buffer solutions or cell culture media, and has broad application prospects in the field of ready-to-use reagents.

[0023] The hydrogel kit prepared by the preparation method of the present application has the following excellent technical effects:

[0024] 1. The hydrogel obtained by the preparation method of the present application is used to culture cells, which can promote cell adhesion, proliferation and differentiation. Compared with commercially available products, it has a better effect of promoting cell sphering.

[0025] 2. The preparation method of the present invention is simple, the material source is wide, and it is highly practical, and can be used as a matrix material for in vitro 3D culture of cells.

[0026] 3. The ready-to-use hydrogel kit obtained by the preparation method of the present application can form a hydrogel immediately after adding the cell culture medium, without the need for other gelling agents, and is easy to use.

[0027] 4. The content of the precursor in the ready-to-use hydrogel kit of the present application can be adjusted according to the needs of culturing cells to meet the needs of multiple scenarios and different applications. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 H NMR spectra of PT-BP and PT-BP-RGD.

[0029] Figure 2 a) Demonstration of PT-BP gelation induced by DMEM, DMEM inorganic salt component solution and aqueous solution containing NaHCO3, CaCl2 and NaCl; b) Rheological test G′ and G″ values ​​of the above solutions forming hydrogels. Figure 3 Schematic diagram of the preparation and use process of the hydrogel kit.

[0030] Figure 4 DMEM with different concentrations of Ca 2+ Mechanical properties of hydrogels formed from hydrogel precursors: a) storage modulus, b) Young's modulus and c) stress relaxation.

[0031] Figure 5 In the presence of different Ca 2+ Bright field microscope images of HepG2 cells after 7 days of culture in hydrogels with different concentrations.

[0032] Figure 6 Confocal scanning images of HepG2 cells cultured in pectin hydrogels after 0 and 7 days.

[0033] Figure 7 Bright field and live-dead staining fluorescence images of HepG2 cells after culturing in Matrigel and pectin hydrogel kit for 3 and 7 days, respectively.

[0034] Figure 8 Cell staining results of HepG2 cells after culturing in the pectin hydrogel kit for 3 and 7 days.

[0035] Fig. 9Cell stemness of HepG2 cells after culturing in pectin hydrogel kit for 3 and 7 days. Fig.10 Bright field microscope image of human mesenchymal stem cells (hMSCs) after 3 days of culture in the hydrogel kit.

[0036] Fig.11 Live-dead staining images of various tumor cells after culturing in the hydrogel kit for 3 days. DETAILED DESCRIPTION

[0037] The technical scheme of the present invention is further described below in conjunction with specific examples, but these examples are not intended to limit the present invention. Unless otherwise specified, reagents are all commercially available products. The pectin used in the following experiments is low-ester pectin purchased from Aladdin.

[0038] The bisphosphonic acid group has a strong coordination effect with metal ions. Its structure is as follows:

[0039]

[0040] Generally, the carboxyl groups on the pectin molecules are combined with divalent metal ions by electrostatic forces to form gels, and the bisphosphonic acid groups can enhance the combination with divalent metal ions. The inventors of the present application found that due to the modification of the bisphosphonic acid groups on pectin, no gel was formed after mixing with divalent metal ions. After further adding a monovalent metal ion solution, the formation of a hydrogel was triggered. Since cell culture media generally contain monovalent metal ions (such as sodium ions), the hydrogel can be triggered to gel after adding cell culture media. This feature makes it have broad application prospects in the field of ready-to-use hydrogels.

[0041] Example 1

[0042] Preparation of bisphosphonic acid-modified pectin

[0043] The preparation of bisphosphonic acid-modified pectin can be carried out by introducing bisphosphonic acid groups into the side chains of pectin by conventional methods in the art. In this embodiment, bisphosphonates containing amino groups are introduced into the side chains of pectin by reacting the amino groups with carboxylic acids on pectin. The reaction is carried out in an aqueous phase under mild conditions. It should be understood that the invention purpose of this application can also be achieved by grafting bisphosphonic acid groups in other conventional ways.

[0044] 1) Preparation of bisphosphonic acid modified pectin (PT-BP)

[0045] The preparation method of the bisphosphonic acid modified pectin is as follows: dissolving the bisphosphonic acid compound in MES buffer, adding pectin and NHS to mix, dissolving EDC in MES buffer, slowly dripping into the above pectin mixed solution, stirring continuously at room temperature for 24 hours, adding hydroxylamine hydrochloride to the reactant, dialyzing and then freeze-drying.

[0046] Specifically, 5.04 g of alendronate sodium trihydrate was added to 80 mL of MES buffer (pH = 6.5) and heated to about 60°C until completely dissolved. After cooling to room temperature, 1 g of pectin and 0.89 g of NHS were added and mixed. 2.98 g of EDC was dissolved in 20 mL of MES buffer and slowly dripped into the above-mentioned pectin mixed solution within 30-60 minutes. The reaction was stirred continuously at room temperature for 24 hours. After adding 1.08 g of hydroxylamine hydrochloride to the reactant, it was dialyzed (molecular weight cutoff 3500 Da) and then freeze-dried. The bisphosphonate (BP) substitution degree (DS) of the PT-BP obtained by the reaction was estimated to be 12.5% ​​by 1H NMR (Bruker Advance 400 MHz spectrometer).

[0047] By changing the amount of sodium alendronate added, bisphosphonic acid-modified pectins with substitution degrees of 7.5%, 10%, 12.5%, 15% and 20% were prepared respectively.

[0048] 2) Preparation of bisphosphonic acid and peptide modified pectin (PT-BP-RGD)

[0049] The preparation method of the pectin modified with bisphosphonic acid and RPG group is as follows: pectin is dissolved in MES buffer, and RGD peptide and EDC are added. Sulfo-NHS is dissolved in MES buffer and added to the above solution, and reacted at room temperature. The bisphosphonic acid compound is dissolved in the above reaction solution, and NHS is added. EDC is dissolved in MES buffer and slowly added dropwise to the previous solution, and reacted at room temperature. Finally, hydroxylamine hydrochloride is added to terminate the reaction. The obtained solution is dialyzed and freeze-dried to obtain PT-BP-RGD.

[0050] Specifically, 1g pectin was weighed with a tray balance and dissolved in 80mL MES buffer (pH=6.5). After complete dissolution, 98mg polypeptide GGGYGRGDSPG and 99mg EDC were added. 56mg sulfo-NHS was weighed and dissolved in 20mL MES buffer and slowly added to the solution, and reacted at room temperature for 24h. 5.04g alendronate sodium was weighed and dissolved in the solution at 60℃. After cooling to room temperature, 0.89g NHS was added. 2.98g EDC was dissolved in 20mL MES buffer and slowly added to the previous solution, and reacted at room temperature for 24h. Finally, 1.079g hydroxylamine hydrochloride was added to terminate the reaction. The obtained solution was dialyzed and freeze-dried to obtain PT-BP-RGD. RGD is the minimum sequence recognized by cell membrane integrins in ECM. By introducing the RGD group, the adhesion and migration of cells on the surface of hydrogel materials can be further improved. Pectin grafted with RGD can better simulate the microenvironment in tissues. The preparation method can be carried out in an aqueous phase with mild conditions and simple operation.

[0051] Figure 1 The H-NMR spectra of PT-BP and PT-BP-RGD are shown respectively, in which PT-BP-RGD shows the characteristic peak of RGD between 7.0-7.5, indicating that RGD is successfully grafted onto PT-BP.

[0052] Example 2

[0053] Preparation of hydrogel by modifying pectin with bisphosphonic acid

[0054] The bisphosphonic acid-modified pectin prepared in Example 1 was added to ultrapure water and mixed to obtain a 6% pectin aqueous solution. At the same time, 200 mM Ca 2+ 1 mL of aqueous solution was added, and the two were mixed in equal volumes to obtain a non-gelled solution, which was used as a precursor solution. After 50 μl of cell culture medium DMEM was added to the above precursor solution, rapid gelation was observed. This example also tried other proportions of pectin aqueous solution, and it was found that when the pectin concentration in the precursor solution was in the range of 1%-10%, hydrogels could be formed.

[0055] On this basis, the inventors explored the mechanism of PT-BP gelation induced by cell culture medium. According to the composition of inorganic salts in cell culture medium (as shown in Table 1), 50 μl of inorganic salt solutions of different combinations were added to the precursor solution in this example to observe the gelation, as shown in Table 2.

[0056] Table 1 Inorganic salt components in cell culture medium

[0057] serial number Inorganic salt Concentration (mM) A <![CDATA[CaCl2]]> 1.80 B <![CDATA[MgSO4]]> 0.81 C KCl 5.37 D <![CDATA[NaHCO3]]> 44.04 E NaCl 109.51 F <![CDATA[NaH2PO4]]> 0.91

[0058] Table 2 Gelation of different inorganic salt solution combinations

[0059] combination Whether it is gel combination Whether it is gel combination Whether it is gel A no A+C+F no A+C+D+F no A+D no A+C+D no A+C+D+E yes A+E no A+C+E no A+D+E+F yes A+F no A+E+F no B+C+E+F no A+B no A+D+E yes A+B+C+D+E yes A+C no A+D+F no A+C+D+E+F yes D+E no A+B+C+F no A+B+D+E+F yes A+B+C no A+B+D+E yes B+C+D+E+F yes A+B+D no A+B+D+F no A+B+C+D+E+F yes A+B+E no A+B+E+F no A+B+F no A+B+C+D no

[0060] By comparing the gelation of adding different DMEM components, the inventors found that the inorganic salt component in the culture medium is the key to triggering the gelation of PT-BP. After further arranging and reorganizing the various substances in the inorganic salt component, it was found that the three minimum components that can cause PT-BP to gel are NaHCO3, CaCl2 and NaCl. Therefore, this example further compares the gelation effects of three solutions, namely 1. culture medium DMEM; 2. inorganic salt component solution in DMEM; 3. solution prepared by NaHCO3, CaCl2 and NaCl. The results show that ( Figure 2 a) All three solutions can make PT-BP gel. The rheological test results of the hydrogels formed by different solutions and PT-BP showed that the properties of the hydrogels formed by the mixed solution of DMEM and NaHCO3, CaCl2, and NaCl and PT-BP were similar (see Figure 2 b). Therefore, it can be determined that due to the presence of monovalent cations in the cell culture medium, after being added to the pectin aqueous solution, they bind to the carboxyl groups on the pectin, reduce the electrostatic repulsion between pectins, and thus promote calcium ion-mediated cross-linking to form a hydrogel.

[0061] This example further investigates the effect of different concentrations of monovalent cations on the gelation of PT-BP, and finds that when the concentration of monovalent cations is within the range of 100-300 mM, the gelation can be promoted.

[0062] Furthermore, this example investigates the effect of different pH values ​​on gelation. Experimental parameters and data are shown in Table 3. When the pH value is in the range of 7-9, the addition of a solution containing sodium ions can promote gelation.

[0063] Table 3 Effect of pH on gelation

[0064] ① ② ③ ④ ⑤ ⑥ ⑦ Pectin-COOH 66mM 66mM 66mM 66mM 66mM 66mM 66mM <![CDATA[Ca 2+ ]]> 1.8mM 1.8mM 1.8mM 1.8mM 1.8mM 1.8mM 1.8mM NaCl 109mM 109mM 109mM 109mM 109mM 109mM 109mM <![CDATA[NaHCO3]]> 44mM - - - - - - NaOH - 44mM - 80mM - - - <![CDATA[Na2CO3]]> - - 44mM - 33mM 22mM - <![CDATA[Na3PO4]]> - - - - - - 44mM Whether it is gel Glue Glue No glue Glue Glue Glue No glue pH 7-8 7-8 9-10 8-9 8-9 7-8 9-10

[0065] Example 3

[0066] Preparation of ready-to-use hydrogel kit

[0067] Based on the research of Example 2, the inventors found that the pectin can be used to prepare a ready-to-use hydrogel; further, it can also be used to prepare a ready-to-use hydrogel kit, which may include, for example, one or more hydrogel precursors involved in the present application. The kit includes various forms of instruments with cavities for cell culture, or surfaces for cell culture, including various culture plates, culture dishes, tubes, or various devices for placing or culturing cells in instruments.

[0068] The hydrogel precursor-containing components of the kit may be present in separate containers, or multiple components may be present in a single container.

[0069] The operation process of one embodiment of preparing a ready-to-use hydrogel kit in this example is shown in Figure 3 The modified bisphosphonic acid pectin was dissolved in water and Ca 2+ The aqueous solution is mixed to form a precursor solution which is added to the culture device of the kit. After freeze drying, a kit with a surface covered with a hydrogel precursor is obtained. When in use, a cell culture medium mixed with cells is directly added to the culture wells to form a hydrogel encapsulating the cells. The 96-well culture plate shown in the figure is only a certain embodiment of the culture device, and the precursor can be easily covered on various culture surfaces by freeze drying.

[0070] Specifically, in one embodiment of the present invention, 60 mg of PT-BP-RGD was dissolved in 1 mL of ultrapure water to obtain a 6% PT-BP-RGD aqueous solution, and 200 mM Ca 2+ 1 mL of aqueous solution was added, and the two were evenly mixed to obtain a final concentration of 3% PT-BP-RGD and 100 mM Ca 2+ To make the material fluffy after freeze-drying and facilitate cell penetration, the precursor solution was diluted by half to obtain a final concentration of 1.5% PT-BP-RGD and 50 mM Ca 2+ 4 mL of precursor solution. At this time, the precursor solution is dispensed into a 96-well plate at 100 μL per well for freeze-drying to prepare a ready-to-use hydrogel kit. Through microscopic observation, it can be seen that the precursor solution evenly covers and adsorbs the surface of the well plate after freeze-drying, and is sponge-like.

[0071] In the kit obtained by the above method, the surface of the culture well is covered with a hydrogel precursor. The amount or thickness of the precursor can be adjusted according to actual needs by adjusting the concentration or amount of the precursor solution added to the well plate.

[0072] Example 4

[0073] This example investigates the 2+ The effect of aqueous solution concentration on gel formation. 2 + When the concentration of the aqueous solution is in the range of 50-200 mM, the prepared precursors can all form gels. 2+ The concentration of DMEM has a correlation with the mechanical properties of the hydrogel. 2+ The rheological and mechanical properties of the PT-BP-RGD freeze-dried materials after forming hydrogels ( Figure 4 ). The results showed that as Ca 2+ As the concentration increases, the energy storage and Young's modulus of the hydrogel increase, and the stress relaxation rate accelerates. 2+ The concentration can adjust the hardness and other mechanical properties of the hydrogel according to the needs of the cells to be cultured.

[0074] Example 5

[0075] Ready-to-use kits for cell culture

[0076] All cells involved in this example were purchased from ATCC (American Type Culture Collection), and the cells were cultured in DMEM with 10% bovine serum and 1% double antibody for 3 days. Then, the cells were collected by trypsin, and after counting the cells, 5×10 5 Resuspend cells in 50 μL of cell culture medium.

[0077] This example first investigated the 2+ The effect of the kit of the precursor of the concentration on culturing cells. A suspension of 500,000 HepG2 cells was directly added to the 96-well hydrogel kit prepared according to Example 4 at 50 μL / well. After incubation for 1 hour, culture medium (100 μL of DMEM with 10% fetal bovine serum and 1% double antibody) was added and cultured and the medium was changed every other day. After culturing for 3 to 7 days, the cell morphology was observed, and cell live and dead staining and immunofluorescence staining experiments were performed.

[0078] Figure 5 It shows that in the presence of different Ca 2+ The state of HepG2 cells after 7 days of culture in hydrogels with different concentrations. Electron microscopy results showed that HepG2 cells in all groups formed cell spheres with a diameter of about 100 μm. In subsequent experiments, 100 mM Ca was used to better ensure the integrity of the hydrogel during the staining process. 2+ Conditioned cells for study.

[0079] The cell growth was observed using a Zeiss confocal microscope LSM880. Figure 6 HepG2 cells were grown on hydrogel (100 mM Ca 2+ ) after 0 and 7 days. The results show that the hydrogel kit prepared by the method of the present application can effectively promote the sphering of HepG2 cells.

[0080] Furthermore, this example uses a commercially available Matrigel kit and adopts the same method to culture cells as a control, and uses a fluorescence microscope to observe the bright field and live-dead fluorescence staining during cell growth. The operation of cell live color staining is as follows:

[0081] 1. Prepare staining solution: Calcein AM (Biyuntian) and Propidium iodide (Biyuntian) are diluted 1:1000 in PBS (HyClone);

[0082] 2. Wash the hydrogel in a 24-well plate with PBS three times, 1 mL each time, then add 1 mL of staining solution and stain at 37°C for 30 min;

[0083] 3. Wash three times with 1 mL of PBS each time.

[0084] Figure 7 The results show that HepG2 cells were cultured in Matrigel and hydrogel kits for 3 and 7 days respectively. The results show that compared with Matrigel, the cells in the kit of the present application have more obvious spheroidization.

[0085] This example further investigates the cell proliferation of cells cultured in the hydrogel kit. The experimental method is fluorescent staining, and the specific operation is as follows: the hydrogel absorbs the culture medium, transfers to a 24-well plate, and washes 3 times with 1 mL PBS, each time for 3 minutes. Add 1 mL of paraformaldehyde and fix at room temperature for 2-3 hours. Wash 3 times with 1 mL PBS, each time for 3 minutes, permeate with 0.2% Triton-x-100 (Sigma) PBS solution for 30 minutes, and wash 3 times with 1 mL PBS, each time for 3 minutes. 6.2.5% bovine serum albumin (BSA, Sigma) is blocked at 37°C for 3 hours, and washed 3 times with 1 mL 1% BSA, each time for 3 minutes. Dilute the primary antibody Ki67 and OCT4 (1:500) (Proteintech) with 1% BSA, respectively, and incubate at 4°C overnight. Wash once with PBS containing 0.1% Tween (Aladdin), and wash 3 times with PBS, each time for 3 minutes. Fluorescent secondary antibody Alexa Fluor 488 (Thermo Fisher) was diluted with 1% BSA (1:500), incubated in a dark and humid environment for 3 hours, washed once with 0.1% Tween PBS, and washed three times with PBS, each time for 3 minutes. DAPI (Biyuntian) (1:500) was diluted with PBS and incubated for 30 minutes, and washed three times with PBS, each time for 3 minutes. Figure 8 The proliferation of HepG2 cells after 3 and 7 days of culture in the hydrogel kit is shown. The results show that after 3 and 7 days of cell culture, the cells in the hydrogel kit have obvious proliferation. This shows that the mechanical properties of the hydrogel reagent of the present application promote cell proliferation and sphering. Fig. 9 The results show that the stemness of HepG2 cells can be maintained after 3 and 7 days of cell culture in the hydrogel kit. The results show that the cells can maintain their stemness in the hydrogel kit after 3 and 7 days of cell culture. This proves that the hydrogel of the present application has better dynamic mechanical properties of simulating extracellular matrix.

[0086] Example 6

[0087] This example investigates the effect of using the hydrogel kit to culture mesenchymal stem cells. The specific experimental method is as follows: The third generation hMSCs (ATCC) were cultured in α-MEM with 17% bovine serum, 1% double antibody, 1% L-glutamine and 5ng / mL FGF2 for 10 days. The fourth generation hMSCs obtained by trypsin collection were counted and 5×10 5 The cells were resuspended in 50 μL cell culture medium and dropped into the hydrogel kit. After incubation for 1 h, 100 μL cell culture medium was added and cultured for 3 days. Fig.10This is a bright field microscope image of human mesenchymal stem cells (hMSCs) cultured in a hydrogel kit for 3 days. By observing the cell proliferation, the stem cells can spread well in the hydrogel kit.

[0088] Example 7

[0089] This example investigates the use of the hydrogel kit for culturing a variety of tumor cells (all from ATCC), and the experimental method is the same as the aforementioned HepG2 cells. Fig.11 The live-death staining experiment shows that various tumor cells were cultured in the hydrogel kit for 3 days. The experimental results show that various tumor cells have good sphering effect in the hydrogel kit, indicating that the hydrogel of the present application has adaptive dynamic mechanical properties and can be used to simulate the growth environment of various cells.

[0090] The above is an exemplary description of the present invention. It should be noted that, without departing from the core of the present invention, any simple deformation, modification or other implementation method that can be obtained by those skilled in the art without expending creative labor should be deemed to fall within the scope of protection of this application.

Claims

1. A method for preparing a hydrogel, comprising the following steps: The bisphosphonic acid-modified pectin is dissolved in water or aqueous solution, a divalent metal cation solution is added and mixed to obtain a precursor solution, and a gelling solution is added to initiate crosslinking to form a hydrogel, wherein the gelling solution is a solution containing monovalent metal ions at a pH of 7-9.

2. The preparation method according to claim 1, characterized in that The bisphosphonic acid in the bisphosphonic acid-modified pectin is selected from one or more of pamidronic acid, tiludronic acid, alendronic acid, neridronic acid, olpadronic acid and ibandronic acid.

3. The preparation method according to claim 1 or 2, characterized in that: The mass percentage of the bisphosphonic acid-modified pectin in the precursor solution is 0.5-10%, and the concentration of the divalent metal cation is not less than 50mM; after adding the gelling solution, the concentration of the monovalent metal cation ranges from 100-300mM.

4. The preparation method according to claim 1 or 2, characterized in that: The divalent metal cation solution includes Mg 2 + , Ca 2+ , Sr. 2+ , Ba 2+ , Mn 2+ , Fe 2+ ,Co 2+ , Ni 2+ , Cu 2+ , Zn 2+ One or more of; the monovalent metal ion solution includes Na + , K + One or both of the following.

5. Use of the hydrogel prepared by the preparation method according to any one of claims 1 to 4 in cell culture and tissue culture.

6. A ready-to-use hydrogel kit, comprising a hydrogel precursor, characterized in that: The hydrogel precursor is a product obtained by freeze-drying a mixed solution containing pectin modified with bisphosphonic acid and divalent metal cations.

7. The ready-to-use hydrogel kit according to claim 6, characterized in that At least one of the following a)-c): a) the bisphosphonic acid in the bisphosphonic acid-modified pectin is selected from one or more of pamidronic acid, tiludronic acid, alendronic acid, neridronic acid, olpadronic acid and ibandronic acid; b) The divalent metal cation is selected from Mg 2+ , Ca 2+ , Sr. 2+ , Ba 2+ , Mn 2+ , Fe 2+ ,Co 2+ , Ni 2+ , Cu 2+ , Zn 2+ One or more of the following; c) The mass percentage of bisphosphonic acid-modified pectin in the mixed solution is 0.5-10%, and the concentration of divalent metal cations is not less than 50 mM.

8. The ready-to-use hydrogel kit according to claim 6 or 7, characterized in that: The bisphosphonic acid-modified pectin is further grafted with a short peptide group, preferably, the short peptide group is an RGD group.

9. A method for preparing the ready-to-use hydrogel kit according to any one of claims 6 to 8, comprising the following steps: The bisphosphonic acid-modified pectin solution and the solution containing divalent metal cations are mixed to obtain a precursor solution, and the precursor solution is added into a cell culture device and freeze-dried to obtain a ready-to-use hydrogel kit.

10. A method for culturing cells using the ready-to-use hydrogel kit according to any one of claims 6 to 8, comprising the following steps: The cell suspension is dropped into the ready-to-use hydrogel kit, and a cell culture fluid is added to obtain a hydrogel encapsulating cells for three-dimensional culture.

Citation Information

Patent Citations

  • Kit and method for preparing digestible sphere-stable hydrogel

    CN114502712A

  • Core-shell polymer nanoparticle

    CN112469396A

  • Pectin culture media and method

    US4282317A

Cited By

  • Strontium-doped polypeptide hydrogel, preparation method, composite biological scaffold and application