Cable insulation material for self-repairing photovoltaic device as well as preparation method and application of cable insulation material
By vulcanizing the polymer and nanosilica fillers of polyethylene and polyaniline, cable insulating materials for photovoltaic devices with self-healing capabilities are prepared, which solves the problems of space charge accumulation and environmental pollution of traditional cable materials, and improves the Cable performance and stability.
Patent Information
- Application Number
- CN202411080593.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-11-22
AI Technical Summary
Cable materials for traditional photovoltaic devices are prone to accumulate space charge during use, resulting in degradation of electrical performance and poor anti-aging performance. The existing microcapsule technology has high cost and environmental pollution problems.
A polymer of vulcanized modified polyethylene and polyaniline is used to form a network structure through disulfide bonds, and combined with nano-silica fillers, a cable insulating material with self-healing ability is prepared to improve the electrical insulation and thermal stability of the cable.
The dual characteristics of suppressing space charge accumulation and self-healing are achieved, which improves the mechanical strength and thermal stability of the cable, extends the service life, and reduces the risk of environmental pollution.
Smart Images

Figure BDA0004983613140000141
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of electrical insulation materials, and in particular to a cable insulation material for a self-repairing photovoltaic device, and a preparation method and application thereof. Background Art
[0002] With the development of photovoltaic technology, the performance requirements for cables used in photovoltaic devices are constantly increasing. Traditional cable materials such as polyethylene, polyvinyl chloride (PVC), fluoroplastics, rubber, silicone rubber insulation materials, etc. are prone to accumulate space charges in long-term use, resulting in defects such as electrical trees and water trees, resulting in reduced electrical performance, poor anti-aging performance, and short service life. Therefore, it is urgent to develop a new type of cable material to improve the problem of space charge accumulation and have self-repair capabilities.
[0003] In order to solve the above problems, we should actively seek a new type of self-repairing cable insulation material for photovoltaic devices. In view of the problems of traditional cables accumulating space charge and poor self-repairing performance during use, researchers are working hard to find new materials that can effectively inhibit the accumulation of space charge and are committed to optimizing the performance of cables for photovoltaic devices, thereby improving their anti-aging performance and stability in practical applications.
[0004] For the existing disclosed microcapsule technology, when the material is damaged, under certain environmental conditions, the outer core materials of the two double-layer microcapsules meet first, that is, the epoxy resin undergoes cross-linking and curing, filling the microcracks and microdamages of the cable surface insulation material to complete the damage self-repair process and restore the material to its original state. However, there are still some problems with microcapsule technology. The self-repair system of the microcapsule material will still lose its repair ability due to the exhaustion of the repair agent, making the product costly. The degradation rate of the microcapsule material is slow, which may lead to long-term existence in the environment, causing potential impacts on the ecosystem, and posing problems such as environmental pollution and sustainability. Therefore, the development of a cable insulation material for photovoltaic devices with strong stability and self-repairing properties has important practical significance and market demand. Summary of the invention
[0005] In view of this, the purpose of the present invention is to propose a cable insulation material for self-repairing photovoltaic devices and a preparation method and application thereof, so as to improve the problem of space charge accumulation and have self-repairing ability.
[0006] Based on the above purpose, the present invention provides a cable insulation material for a self-repairing photovoltaic device, comprising the following components in parts by weight:
[0007] 50-55 parts of polyethylene, 35-40 parts of vulcanizing agent, 20-25 parts of polyaniline, 15-20 parts of dimethylformamide, 10-15 parts of nano-silicon dioxide, 5-10 parts of cross-linking agent, 1-3 parts of antioxidant and 1-2 parts of absorbent; wherein, the polyethylene and the vulcanizing agent are reacted through vulcanization to obtain vulcanized modified polyethylene, and the vulcanized modified polyethylene forms a network structure with self-repairing ability through disulfide bonds.
[0008] The material uses vulcanized modified polyethylene to form a network structure with self-repairing ability through disulfide bonds, and is blended with polyaniline (PANI) with good conductivity to form a polymer that can inhibit the accumulation of space charges. 2 ), the material has good compatibility, improves the electrical insulation of the cable, and can further inhibit the accumulation of space charge when mixed with vulcanized modified polyethylene. The repaired material has high mechanical strength and good thermal stability, which effectively improves the problem of space charge accumulation and has self-repairing ability.
[0009] Preferably, the vulcanizing agent is 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane.
[0010] Preferably, the crosslinking agent is one of dibenzoyl peroxide, diisopropylbenzene peroxide, triethoxysilane or vinyltrimethoxysilane.
[0011] Preferably, the antioxidant is one or more of butylphenol glycol, p-phenylenediamine, and butylated hydroxyanisole.
[0012] Preferably, the absorbent is one of phenyltriazine compounds or substituted acrylonitrile compounds.
[0013] Preferably, the particle size of the nano-silicon dioxide is 30-40 nm. 2 ) can increase the diffusion rate of charge carriers, and combined with polyaniline (PANI) with good conductivity, it can promote the migration and uniform distribution of charges within the material and reduce the accumulation of space charges.
[0014] The present invention also provides a method for preparing the cable insulation material for the self-repairing photovoltaic device, comprising the following steps:
[0015] Step 1: adding polyethylene and a vulcanizing agent into deionized water according to the formula amount, stirring magnetically at 90-100° C. for 50-60 minutes, and obtaining vulcanized modified polyethylene through vulcanization reaction;
[0016] Step 2: Mix polyaniline and dimethylformamide according to the formula amount, stir magnetically for 10-20 minutes at 20-25° C., then add the sulfurized modified polyethylene obtained in step 1, stir magnetically for 20-30 minutes at 60-70° C., and obtain a polymer of sulfurized modified polyethylene and polyaniline;
[0017] Step 3, after ultrasonic dispersion of the polymer obtained in step 3, a cross-linking agent is added to obtain a cross-linked polymer with a network structure after a cross-linking reaction;
[0018] Step 4: adding the cross-linked polymer obtained in step 3 to dimethylformamide, stirring and dissolving at 50-60° C., then adding an antioxidant and an absorbent according to the formula amount, and subjecting the antioxidant, the absorbent and the cross-linked polymer to ultrasonic treatment to fully combine; wherein the amount of dimethylformamide used in step 2 is equal to that used in step 4;
[0019] Step 5: Disperse the pretreated nano-silicon dioxide into the solution obtained in step 4, and after ultrasonic treatment at 70-75° C., cool to room temperature, and dry, obtain a cable insulation material for self-repairing photovoltaic devices.
[0020] Preferably, the cross-linking reaction in step 3 is to control the heating temperature to 70-80° C., stir for 20-25 minutes, and then cool and solidify at room temperature.
[0021] Preferably, the stirring and dissolving time at 50-60° C. in step 4 is 10-20 min, the ultrasonic frequency of the ultrasonic treatment is 50-60 kHz, and the ultrasonic treatment is 20-25 min.
[0022] Preferably, the ultrasonic frequency of the ultrasonic treatment in step 5 is 70-75kHz, the ultrasonic treatment is 30-35min, the drying temperature is 50-70°C, and the drying time is 10-13h.
[0023] The present invention also provides application of the cable insulation material for the self-repairing photovoltaic device in a cable sheath.
[0024] Beneficial effects of the present invention: The present invention uses a polymer of vulcanized modified polyethylene and polyaniline as a base material, achieving the dual characteristics of inhibiting space charge accumulation and self-repairing. By using a cross-linking agent, a three-dimensional network structure based on disulfide bonds is achieved, and self-repairing ability is further achieved. At the same time, a highly compatible nano-silica filler is introduced. This material has good compatibility and can be mixed with vulcanized modified polyethylene to further inhibit the accumulation of space charges, making material fusion more adaptable and improving the electrical insulation and thermal stability of the cable. DETAILED DESCRIPTION
[0025] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments.
[0026] It should be noted that, unless otherwise defined, the technical terms or scientific terms used in the present invention should have the common meanings understood by persons having ordinary skills in the field to which the present invention belongs.
[0027] Example 1
[0028] A cable insulation material for a self-repairing photovoltaic device that inhibits space charge accumulation comprises the following components by weight: 55 parts of polyethylene (PE), 40 parts of a vulcanizing agent (2,5-dimethyl-2,5-di(tert-butylperoxy)hexane), 25 parts of polyaniline (PANI), 20 parts of dimethylformamide (DMF) (the two amounts are equal, both are 10 parts), nano silicon dioxide (SiO 2 ) 15 parts, cross-linking agent dibenzoyl peroxide (BPO) 10 parts, antioxidant glycol butylphenol 3 parts, absorbent phenyltriazine 2 parts.
[0029] The method for preparing the cable insulation material for self-repairing photovoltaic devices for inhibiting space charge accumulation of this embodiment comprises the following steps:
[0030] Step (1): adding a formulated amount of polyethylene (PE) and a vulcanizing agent 2,5-dimethyl-2,5-di(tert-butyl)peroxide to deionized water, stirring in a magnetic stirrer at 100° C. for 55 minutes, and obtaining a vulcanized modified polyethylene through a vulcanization reaction.
[0031] Step (2): Mix a low-concentration polyaniline (PANI) in a formula amount with 10 parts of dimethylformamide (DMF), stir in a magnetic stirrer at 25° C. for 20 minutes, then add the sulfurized modified polyethylene in step (1), stir in a magnetic stirrer at about 70° C. for 30 minutes at a rotation speed of 100 rpm, and obtain a polymer of sulfurized modified polyethylene and polyaniline.
[0032] Step (3): The polymer obtained in step (2) is dispersed by ultrasonic treatment, and then a cross-linking agent is added. The heating temperature is controlled to 70° C., stirred for 20 minutes, and cooled and solidified at room temperature to obtain a cross-linked polymer with a network structure.
[0033] Step (4): Add the product of step (3) to 10 parts of dimethylformamide (DMF), stir in a magnetic stirrer at 50°C for 20 minutes to fully dissolve it, add the antioxidant and absorbent according to the formula, and perform ultrasonic treatment at an ultrasonic frequency of 60kHz for 20 minutes to allow the antioxidant and absorbent to fully combine with the product.
[0034] Step (5): Nano-silicon dioxide (SiO2 ) for pretreatment to fully dissolve the nano-silica in the solvent. Disperse the pretreated nano-silica filler into the solution of step (4), stir it thoroughly, and then perform ultrasonic treatment at an ultrasonic frequency of 70kHz to make it uniformly filled. Perform ultrasonic treatment for 30 minutes, and control the temperature at 70°C to make the nano-filler uniformly wrapped in the cross-linked polymer. When the temperature drops to room temperature, place the obtained material in an oven at 60°C and dry it for 12 hours to obtain a self-repairable cable sheath material for photovoltaic devices.
[0035] Example 2
[0036] A cable insulation material for a self-repairing photovoltaic device capable of inhibiting space charge accumulation comprises the following components by weight: 60 parts of polyethylene (PE), 35 parts of a vulcanizing agent (2,5-dimethyl-2,5-di(tert-butylperoxy)hexane), 25 parts of polyaniline (PANI), 20 parts of dimethylformamide (DMF) (the two amounts are equal, both are 10 parts), 17 parts of nano zinc oxide (ZnO), 10 parts of a cross-linking agent dibenzoyl peroxide (BPO), 3 parts of an antioxidant diol butylphenol, and 2 parts of an absorbent substituted acrylonitrile compound.
[0037] The method for preparing the cable insulation material for self-repairing photovoltaic devices for inhibiting space charge accumulation of this embodiment comprises the following steps:
[0038] Step (1): Add a formulated amount of polyethylene (PE) and a vulcanizing agent 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane to deionized water, stir in a magnetic stirrer at 100° C. for 55 minutes, and obtain a vulcanized modified polyethylene through a vulcanization reaction.
[0039] Step (2): Mix a low-concentration polyaniline (PANI) in a formula amount with 10 parts of dimethylformamide (DMF), stir in a magnetic stirrer at 25° C. for 20 minutes, then add the sulfurized modified polyethylene in step (1), stir in a magnetic stirrer at about 70° C. for 30 minutes at a rotation speed of 100 rpm, and obtain a polymer of sulfurized modified polyethylene and polyaniline.
[0040] Step (3): The polymer obtained in step (2) is dispersed by ultrasonic treatment, and then a cross-linking agent is added. The heating temperature is controlled to 70° C., stirred for 20 minutes, and cooled and solidified at room temperature to obtain a cross-linked polymer with a network structure.
[0041] Step (4): Add the product of step (3) to 10 parts of dimethylformamide (DMF), stir in a magnetic stirrer at 50°C for 20 minutes to fully dissolve it, add the antioxidant and absorbent according to the formula, and perform ultrasonic treatment at an ultrasonic frequency of 60kHz for 20 minutes to allow the antioxidant and absorbent to fully combine with the product.
[0042] Step (5): pre-treat nano zinc oxide (ZnO) to fully dissolve the nano zinc oxide in the solvent. Disperse the pre-treated nano zinc oxide filler into the solution of step (4), stir it fully and then perform ultrasonic treatment at an ultrasonic frequency of 70kHz to make it uniformly filled. Perform ultrasonic treatment for 30 minutes and control the temperature at 70°C to make the nano filler uniformly wrapped in the cross-linked polymer. When the temperature drops to room temperature, place the obtained material in an oven at 60°C and dry it for 12 hours to obtain a self-repairable photovoltaic device cable sheath material.
[0043] Example 3
[0044] A cable insulation material for a self-repairing photovoltaic device that inhibits space charge accumulation comprises the following components by weight: 50 parts of polyethylene (PE), 38 parts of a vulcanizing agent (2,5-dimethyl-2,5-di(tert-butylperoxy)hexane), 25 parts of polyaniline (PANI), 22 parts of dimethylformamide (DMF) (the two amounts are equal, both are 11 parts), and nano silicon dioxide (SiO 2 ) 14 parts, cross-linking agent triethoxysilane (TES) 12 parts, antioxidant p-phenylenediamine (p-Phenylenediamine) 3 parts, absorbent phenyltriazine 2 parts.
[0045] The method for preparing the cable insulation material for self-repairing photovoltaic devices for inhibiting space charge accumulation of this embodiment comprises the following steps:
[0046] Step (1): Add a formulated amount of polyethylene (PE) and a vulcanizing agent 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane into deionized water, stir in a magnetic stirrer at 110° C. for 60 minutes, and obtain a vulcanized modified polyethylene through a vulcanization reaction.
[0047] Step (2): Mix a low-concentration polyaniline (PANI) in a formula amount with 11 parts of dimethylformamide (DMF), stir in a magnetic stirrer at 25° C. for 20 minutes, then add the sulfurized modified polyethylene in step (1), stir in a magnetic stirrer at about 70° C. for 30 minutes at a rotation speed of 120 rpm, and obtain a polymer of sulfurized modified polyethylene and polyaniline.
[0048] Step (3): The polymer obtained in step (2) is dispersed by ultrasonic treatment, and then a cross-linking agent is added. The heating temperature is controlled to 85° C., stirred for 35 minutes, and cooled and solidified at room temperature to obtain a cross-linked polymer with a network structure.
[0049] Step (4): Add the product of step (3) to 11 parts of dimethylformamide (DMF), stir in a magnetic stirrer at 50°C for 20 minutes to fully dissolve it, add the antioxidant and absorbent according to the formula, and perform ultrasonic treatment at an ultrasonic frequency of 60kHz for 20 minutes to allow the antioxidant and absorbent to fully combine with the product.
[0050] Step (5): Nano-silicon dioxide (SiO 2 ) to fully dissolve the nano-silica in the solvent. The pretreated nano-silica filler is dispersed into the solution of step (4), and then fully stirred and ultrasonically treated at an ultrasonic frequency of 72kHz to make it uniformly filled. The ultrasonic treatment is performed for 30 minutes, and the temperature is controlled at 75°C to make the nano-filler uniformly wrapped in the cross-linked polymer. When the temperature drops to room temperature, the obtained material is placed in an oven at 65°C and dried for 12 hours to obtain a self-repairable cable sheath material for photovoltaic devices.
[0051] Example 4
[0052] A cable insulation material for a self-repairing photovoltaic device that inhibits space charge accumulation comprises the following components by weight: 50 parts of polyethylene (PE), 35 parts of a vulcanizing agent (2,5-dimethyl-2,5-di(tert-butylperoxy)hexane), 25 parts of polyaniline (PANI), 20 parts of dimethylformamide (DMF) (the two amounts are equal, both are 10 parts), nano silicon dioxide (SiO 2 ) 15 parts, cross-linking agent dibenzoyl oxide (BPO) 10 parts, antioxidant butylated hydroxyanisole (BHA) 3 parts, absorbent substituted acrylonitrile compound 3 parts.
[0053] The method for preparing the cable insulation material for self-repairing photovoltaic devices for inhibiting space charge accumulation of this embodiment comprises the following steps:
[0054] Step (1): Add a formulated amount of polyethylene (PE) and a vulcanizing agent 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane into deionized water, stir in a magnetic stirrer at 120° C. for 50 minutes, and obtain a vulcanized modified polyethylene through a vulcanization reaction.
[0055] Step (2): Mix low concentration polyaniline (PANI) with 10 parts of dimethylformamide (DMF), stir in a magnetic stirrer at 25° C. for 20 minutes, then add the sulfurized modified polyethylene in step (1), stir in a magnetic stirrer at about 70° C. for 30 minutes at a speed of 100 rpm, to obtain a polymer of sulfurized modified polyethylene and polyaniline.
[0056] Step (3): The polymer obtained in step (2) is dispersed by ultrasonic treatment, and then a cross-linking agent is added. The heating temperature is controlled to 75° C., stirred for 30 minutes, and cooled and solidified at room temperature to obtain a cross-linked polymer with a network structure.
[0057] Step (4): Add the product of step (3) to 10 parts of dimethylformamide (DMF), stir in a magnetic stirrer at 55°C for 30 minutes to fully dissolve it, add the antioxidant and absorbent according to the formula, and perform ultrasonic treatment at an ultrasonic frequency of 65kHz for 35 minutes to allow the antioxidant and absorbent to fully combine with the product.
[0058] Step (5): Nano-silicon dioxide (SiO 2 ) for pretreatment to fully dissolve the nano-silica in the solvent. Disperse the pretreated nano-silica filler into the solution of step (4), stir it thoroughly, and then perform ultrasonic treatment at an ultrasonic frequency of 70kHz to make it uniformly filled. Perform ultrasonic treatment for 30 minutes, and control the temperature at 70°C to make the nano-filler uniformly wrapped in the cross-linked polymer. When the temperature drops to room temperature, place the obtained material in an oven at 60°C and dry it for 12 hours to obtain a self-repairable cable sheath material for photovoltaic devices.
[0059] Example 5
[0060] A cable insulation material for a self-repairing photovoltaic device that inhibits space charge accumulation comprises the following components by weight: 55 parts of polyethylene (PE), 40 parts of a vulcanizing agent (2,5-dimethyl-2,5-di(tert-butylperoxy)hexane), 25 parts of polyaniline (PANI), 20 parts of dimethylformamide (DMF) (the two amounts are equal, both are 10 parts), nano silicon dioxide (SiO 2 ) 15 parts, cross-linking agent 10 parts of triethoxysilane (TES), antioxidant butylated hydroxyanisole (BHA) 3 parts, absorbent phenyltriazine 2 parts.
[0061] The method for preparing the cable insulation material for self-repairing photovoltaic devices for inhibiting space charge accumulation of this embodiment comprises the following steps:
[0062] Step (1): Add polyethylene (PE) and a vulcanizing agent, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, into deionized water, stir in a magnetic stirrer at 95° C. for 65 minutes, and obtain a vulcanized modified polyethylene through a vulcanization reaction.
[0063] Step (2): Mix low concentration polyaniline (PANI) with 10 parts of dimethylformamide (DMF), stir in a magnetic stirrer at 30° C. for 45 minutes, then add the sulfurized modified polyethylene in step (1), stir in a magnetic stirrer at about 70° C. for 30 minutes at a rotation speed of 110 rpm, to obtain a polymer of sulfurized modified polyethylene and polyaniline.
[0064] Step (3): The polymer obtained in step (2) is dispersed by ultrasonic treatment, and then a cross-linking agent is added. The heating temperature is controlled to 70° C., stirred for 20 minutes, and cooled and solidified at room temperature to obtain a cross-linked polymer with a network structure.
[0065] Step (4): Add the product of step (3) to 10 parts of dimethylformamide (DMF), stir in a magnetic stirrer at 65°C for 35 minutes to fully dissolve it, add the antioxidant and absorbent according to the formula, and perform ultrasonic treatment at an ultrasonic frequency of 70kHz for 15 minutes to allow the antioxidant and absorbent to fully combine with the product.
[0066] Step (5): Nano-silicon dioxide (SiO 2 ) for pretreatment to fully dissolve the nano-silica in the solvent. Disperse the pretreated nano-silica filler into the solution of step (4), stir it thoroughly, and then perform ultrasonic treatment at an ultrasonic frequency of 70kHz to make it uniformly filled. Perform ultrasonic treatment for 30 minutes, and control the temperature at 70°C to make the nano-filler uniformly wrapped in the cross-linked polymer. When the temperature drops to room temperature, place the obtained material in an oven at 60°C and dry it for 12 hours to obtain a self-repairable cable sheath material for photovoltaic devices.
[0067] Example 6
[0068] A cable insulation material for a self-repairing photovoltaic device that inhibits space charge accumulation comprises the following components by weight: 55 parts of polyethylene (PE), 40 parts of a vulcanizing agent (2,5-dimethyl-2,5-di(tert-butylperoxy)hexane), 25 parts of polyaniline (PANI), 20 parts of dimethylformamide (DMF) (the two amounts are equal, both are 10 parts), nano silicon dioxide (SiO 2 ) 15 parts, cross-linking agent dibenzoyl peroxide (BPO), 13 parts, antioxidant butylated hydroxyanisole (BHA) 2 parts, absorbent phenyltriazine 2 parts.
[0069] The method for preparing the cable insulation material for self-repairing photovoltaic devices for inhibiting space charge accumulation of this embodiment comprises the following steps:
[0070] Step (1): polyethylene (PE) and a vulcanizing agent 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane are added to deionized water, stirred in a magnetic stirrer at 100° C. for 55 minutes, and a vulcanized modified polyethylene is obtained through a vulcanization reaction.
[0071] Step (2): Mix low concentration polyaniline (PANI) with 10 parts of dimethylformamide (DMF), stir in a magnetic stirrer at 25° C. for 20 minutes, then add the sulfurized modified polyethylene in step (1), stir in a magnetic stirrer at about 70° C. for 30 minutes at a speed of 100 rpm, to obtain a polymer of sulfurized modified polyethylene and polyaniline.
[0072] Step (3): The polymer obtained in step (2) is dispersed by ultrasonic treatment, and then a cross-linking agent is added. The heating temperature is controlled to 80° C., stirred for 45 minutes, and cooled and solidified at room temperature to obtain a cross-linked polymer with a network structure.
[0073] Step (4): Add the product of step (3) to 10 parts of dimethylformamide (DMF), stir in a magnetic stirrer at 65°C for 25 minutes to fully dissolve it, add the antioxidant and absorbent according to the formula, and perform ultrasonic treatment at an ultrasonic frequency of 75kHz for 35 minutes to allow the antioxidant and absorbent to fully combine with the product.
[0074] Step (5): Nano-silicon dioxide (SiO 2 ) to fully dissolve the nano-silica in the solvent. The pretreated nano-silica filler is dispersed into the solution of step (4), and then ultrasonically treated at an ultrasonic frequency of 72kHz to uniformly fill it. The ultrasonic treatment is performed for 35 minutes, and the temperature is controlled at 70°C to uniformly wrap the nano-filler in the cross-linked polymer. When the temperature drops to room temperature, the obtained material is placed in an oven at 60°C and dried for 12 hours to obtain a self-repairable cable sheath material for photovoltaic devices.
[0075] Comparative Example 1
[0076] A method for preparing a cable insulation material for photovoltaic devices comprises the following steps:
[0077] Step (1): Add 70 parts of polyethylene (PE) and 50 parts of a vulcanizing agent (2,5-dimethyl-2,5-di(tert-butylperoxy)hexane) into deionized water, stir in a magnetic stirrer at 90° C. for 75 minutes, and obtain a vulcanized modified polyethylene through a vulcanization reaction.
[0078] Step (2): Mix 25 parts of low concentration polyaniline (PANI) and 10 parts of dimethylformamide (DMF), stir in a magnetic stirrer at 45° C. for 35 minutes, then add the sulfurized modified polyethylene in step (1), stir in a magnetic stirrer at about 80° C. for 35 minutes at a rotation speed of 130 rpm, to obtain a polymer of sulfurized modified polyethylene and polyaniline.
[0079] Repeat steps (3), (4), (5) in Example 1, extend the ultrasonic treatment time in step (5) to 45 min, adjust the oven temperature used during drying to 75° C., and extend the drying time to 14 h.
[0080] Comparative Example 2
[0081] A method for preparing a cable insulation material for photovoltaic devices comprises the following steps:
[0082] Step (1): 55 parts of polyethylene (PE) and 40 parts of a vulcanizing agent (2,5-dimethyl-2,5-di(tert-butylperoxy)hexane) are added to deionized water, stirred in a magnetic stirrer at 100° C. for 30 minutes, and a vulcanized modified polyethylene is obtained through a vulcanization reaction.
[0083] Step (2): 45 parts of low concentration polyaniline (PANI) and 15 parts of dimethylformamide (DMF) are mixed, and stirred in a magnetic stirrer at 45° C. for 35 minutes. The sulfurized polyethylene in step (1) is then added thereto, and stirred in a magnetic stirrer at about 80° C. for 40 minutes at a rotation speed of 125 rpm to obtain a polymer of sulfurized polyethylene and polyaniline.
[0084] Repeat steps (3), (4), (5) in Example 1, extend the ultrasonic treatment time in step (5) to 40 min, adjust the oven temperature used during drying to 75° C., and extend the drying time to 14 h.
[0085] Comparative Example 3
[0086] A method for preparing a cable insulation material for photovoltaic devices comprises the following steps:
[0087] Step (1): 40 parts of polyethylene (PE) and 25 parts of a vulcanizing agent (2,5-dimethyl-2,5-di(tert-butylperoxy)hexane) are added to deionized water, stirred in a magnetic stirrer at 120° C. for 25 minutes, and a vulcanized modified polyethylene is obtained through a vulcanization reaction.
[0088] Step (2): Mix 25 parts of low concentration polyaniline (PANI) and 10 parts of dimethylformamide (DMF), stir in a magnetic stirrer at 45° C. for 35 minutes, then add the sulfurized modified polyethylene in step (1), stir in a magnetic stirrer at about 65° C. for 45 minutes at a rotation speed of 120 rpm, to obtain a polymer of sulfurized modified polyethylene and polyaniline.
[0089] Repeat steps (3), (4), (5) in Example 1, extend the ultrasonic treatment time in step (5) to 45 min, adjust the oven temperature used during drying to 55° C., and extend the drying time to 13 h.
[0090] Comparative Example 4
[0091] A method for preparing a cable insulation material for photovoltaic devices comprises the following steps:
[0092] Step (1): 55 parts of polyethylene (PE) and 40 parts of a vulcanizing agent (2,5-dimethyl-2,5-di(tert-butylperoxy)hexane) are added to deionized water, stirred in a magnetic stirrer at 100° C. for 35 minutes, and a vulcanized modified polyethylene is obtained through a vulcanization reaction.
[0093] Step (2): 15 parts of low concentration polyaniline (PANI) and 10 parts of dimethylformamide (DMF) are mixed, and stirred in a magnetic stirrer at 35° C. for 30 minutes. The sulfurized polyethylene in step (1) is then added thereto, and stirred in a magnetic stirrer at about 65° C. for 35 minutes at a rotation speed of 110 rpm to obtain a polymer of sulfurized polyethylene and polyaniline.
[0094] Repeat steps (3), (4), (5) in Example 1, extend the ultrasonic treatment time in step (5) to 45 min, adjust the oven temperature used during drying to 55° C., and extend the drying time to 13 h.
[0095] Comparative Example 5
[0096] A method for preparing a cable insulation material for photovoltaic devices comprises the following steps:
[0097] Step (1): 40 parts of polyethylene (PE) and 25 parts of a vulcanizing agent (2,5-dimethyl-2,5-di(tert-butylperoxy)hexane) are added to deionized water, stirred in a magnetic stirrer at 120° C. for 25 minutes, and a vulcanized modified polyethylene is obtained through a vulcanization reaction.
[0098] Step (2): Mix 25 parts of low concentration polyaniline (PANI) and 10 parts of dimethylformamide (DMF), stir in a magnetic stirrer at 45° C. for 35 minutes, then add the sulfurized modified polyethylene in step (1), stir in a magnetic stirrer at about 65° C. for 45 minutes at a rotation speed of 120 rpm, to obtain a polymer of sulfurized modified polyethylene and polyaniline.
[0099] Repeat steps (3), (4), and (5) in Example 1, adjust the heating temperature in step (3) to 90°C, adjust the stirring temperature in step 4 to 75°C, extend the ultrasonic treatment time in step (5) to 45 min, adjust the oven temperature used during drying to 55°C, and extend the drying time to 13 h.
[0100] Performance tests were performed on Examples 1-6 and Comparative Examples 1-5, and the specific test results are shown in Table 1 below.
[0101] Table 1 Comparison of cable insulation material performance between Examples 1-6 and Comparative Examples 1-4
[0102]
[0103] It can be seen from the experimental results in the above table that the performance of the cable insulation material prepared in Example 1 is relatively excellent. It can be seen from the results of Example 1 and Comparative Examples 1-4 that excessively increasing the amount of polyethylene (PE) and vulcanizing agent, or increasing the stirring temperature and time, extending the ultrasonic treatment time, etc., will instead reduce the breakdown strength and tensile strength of the final product, and extend the self-repair time. It can be seen from the results of Example 1 and Comparative Example 5 that increasing the heating temperature in the preparation process will also lead to a decrease in product performance.
[0104] Those skilled in the art should understand that the discussion of any of the above embodiments is only exemplary and is not intended to imply that the scope of the present invention is limited to these examples; under the concept of the present invention, the technical features in the above embodiments or different embodiments can also be combined, the steps can be implemented in any order, and there are many other changes in different aspects of the present invention as described above, which are not provided in detail for the sake of simplicity. Any omissions, modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. A cable insulation material for self-repairing photovoltaic devices, characterized in that: The composition comprises the following components in parts by weight: 50-55 parts of polyethylene, 35-40 parts of vulcanizing agent, 20-25 parts of polyaniline, 15-20 parts of dimethylformamide, 10-15 parts of nano-silicon dioxide, 5-10 parts of cross-linking agent, 1-3 parts of antioxidant and 1-2 parts of absorbent; wherein, the polyethylene and the vulcanizing agent are reacted through vulcanization to obtain vulcanized modified polyethylene, and the vulcanized modified polyethylene forms a network structure with self-repairing ability through disulfide bonds.
2. The cable insulation material for self-repairing photovoltaic devices according to claim 1, characterized in that: The crosslinking agent is one or more of dibenzoyl peroxide, dicumyl peroxide, triethoxysilane or vinyl trimethoxysilane.
3. The cable insulation material for self-repairing photovoltaic devices according to claim 1, characterized in that: The antioxidant is one or more of glycol butylphenol, p-phenylenediamine and butylated hydroxyanisole.
4. The cable insulation material for self-repairing photovoltaic devices according to claim 1, characterized in that: The absorbent is one of phenyltriazine compounds or substituted acrylonitrile compounds.
5. The cable insulation material for self-repairing photovoltaic devices according to claim 1, characterized in that: The particle size of the nano silicon dioxide is 30-40 nm.
6. The method for preparing the cable insulation material for self-repairing photovoltaic devices according to any one of claims 1 to 5, characterized in that: The steps include: Step 1: adding polyethylene and a vulcanizing agent into deionized water according to the formula amount, stirring magnetically at 90-100° C. for 50-60 minutes, and obtaining vulcanized modified polyethylene through vulcanization reaction; Step 2: Mix polyaniline and dimethylformamide according to the formula amount, stir magnetically for 10-20 minutes at 20-25° C., then add the sulfurized modified polyethylene obtained in step 1, stir magnetically for 20-30 minutes at 60-70° C., and obtain a polymer of sulfurized modified polyethylene and polyaniline; Step 3, after ultrasonic dispersion of the polymer obtained in step 3, a cross-linking agent is added to obtain a cross-linked polymer with a network structure after a cross-linking reaction; Step 4: adding the cross-linked polymer obtained in step 3 to dimethylformamide, stirring and dissolving at 50-60° C., then adding an antioxidant and an absorbent according to the formula amount, and subjecting the antioxidant, the absorbent and the cross-linked polymer to ultrasonic treatment to fully combine; wherein the amount of dimethylformamide used in step 2 is equal to that used in step 4; Step 5: Disperse the pretreated nano-silicon dioxide into the solution obtained in step 4, ultrasonically treat at 70-75° C., cool to room temperature, and dry to obtain a cable insulation material for a self-repairing photovoltaic device.
7. The method for preparing the cable insulation material for self-repairing photovoltaic devices according to claim 6, characterized in that: In step 3, the cross-linking reaction is carried out by controlling the heating temperature to 70-80°C, stirring for 20-25 minutes, and then cooling and curing at room temperature.
8. The method for preparing the cable insulation material for self-repairing photovoltaic devices according to claim 6, characterized in that: The stirring and dissolving time at 50-60° C. in step 4 is 10-20 min, the ultrasonic frequency of the ultrasonic treatment is 50-60 kHz, and the ultrasonic treatment is 20-25 min.
9. The method for preparing the cable insulation material for self-repairing photovoltaic devices according to claim 6, characterized in that: In step 5, the ultrasonic frequency of the ultrasonic treatment is 70-75kHz, the ultrasonic treatment is 30-35min, the drying temperature is 50-70°C, and the drying time is 10-13h.
10. Use of the cable insulation material for self-repairing photovoltaic devices according to any one of claims 1 to 5 in cable sheaths.
Citation Information
Cited By
Composite material, semiconductive shielding material and high-voltage cable
CN120737484A