Hydrophobic material, preparation process thereof and application of hydrophobic material in preparation of meteorological balloons
By synthesizing hydrophobic materials such as acrylate, polyacrylamide, oleicamide and erucicamide and meteorological balloon latex, the problem of blasting risks and insufficient hydrophobicity of meteorological balloons in high altitude and low temperature environments is solved, and the problem of insufficient hydrophobicity of meteorological balloons is achieved. Higher hydrophobicity and expansion properties improve the stability and reliability of meteorological balloons.
Patent Information
- Application Number
- CN202411242317.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-05
- Publication Date
- 2024-11-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Meteorological balloons cause condensate adhesion and ice crystal friction in high altitude due to low temperatures, increasing the risk of blasting. Existing hydrophobic materials are prone to cracks and fall off during the expansion process, affecting the hydrophobic effect.
Hydrophobic materials synthesized by raw materials such as acrylate, polyacrylamide, oleicamide and erucicamide are well fused with the latex of meteorological balloons through copolymerization reaction to achieve uniform dispersion, reduce surface tension, and enhance tensile strength and expansion.
It significantly improves the hydrophobicity and expansion of meteorological balloons, reduces the risk of blasting in low-temperature environments, and improves the success rate and service life of the lift-off.
Smart Images

Figure BDA0005029648310000051 
Figure BDA0005029648310000061 
Figure BDA0005029648310000071
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of weather balloon preparation, in particular to a hydrophobic material and a preparation process thereof, and application in the preparation of weather balloons. Background Art
[0002] Weather balloons are mainly used for high-altitude meteorological detection business. After being filled with a certain amount of hydrogen, they carry a sonde to the sky to survey the weather and climate, so as to realize the systematic collection and analysis of meteorological and climate data. It can be said that weather balloons have an important impact on the level of forecasting of meteorological and climate changes, the accuracy and timeliness of meteorological data. With the increasing application of high-altitude temperature, humidity, wind speed and other meteorological elements in daily life, the requirements for the launch height and performance of weather balloons are becoming increasingly stringent. In the process of rising to high altitudes, weather balloons may encounter low temperature extreme weather. As the temperature at high altitude drops, ice crystals formed by condensed water are easy to adhere to the surface of the weather balloon skin, causing the weather balloon to be rubbed by ice crystals when rising, increasing the risk of the weather balloon exploding. Therefore, it is necessary to improve the hydrophobicity of weather balloons.
[0003] In order to improve the hydrophobicity of weather balloons in the prior art, hydrophobic materials are often coated on the surface of weather balloons to reduce the adhesion of condensed water. However, since weather balloons need to expand during use and their volume changes greatly, it is difficult for simply coated hydrophobic materials to change synchronously, and they are prone to cracking and falling off, affecting the hydrophobic effect. Therefore, a better solution is to add an appropriate amount of hydrophobic material to the latex used to prepare the balloon, so that the hydrophobic material and the weather balloon can be integrated to achieve synchronous changes. However, such a solution requires good fusion between the hydrophobic material and the latex. If the fusion is not high, microscopic defects such as tiny cracks may appear inside the weather balloon. When the weather balloon gradually rises to high altitudes, as the pressure inside the balloon becomes smaller and smaller and the external pressure becomes larger and larger, these microscopic defects may gradually expand and eventually cause the balloon to burst.
[0004] Therefore, the development of hydrophobic materials that have good hydrophobic properties and can be well integrated with the latex used to make weather balloons has become an important research direction in the field of weather balloon preparation technology. Summary of the invention
[0005] In order to develop a hydrophobic material that has good hydrophobic properties and can be well integrated with the latex used to prepare weather balloons, the present invention provides a hydrophobic material and its preparation process, and its application in the preparation of weather balloons. The hydrophobic material synthesized by the four specific raw materials of acrylate, polyacrylamide, oleamide, and erucamide in the present application not only has good integration with the latex used to prepare weather balloons, but also can significantly enhance the expansion and hydrophobicity of weather balloons, significantly reduce the risk of explosion of weather balloons in low temperature environments, improve the success rate of weather balloons, and increase the service life of high-altitude weather balloons.
[0006] In the first aspect, the present application provides a hydrophobic material using the following technical solution: A hydrophobic material comprises the following components in parts by weight: 8 to 13 parts of acrylate, 5.92 to 9.74 parts of polyacrylamide, 8.7 to 12.4 parts of oleamide, 3.68 to 7.56 parts of erucamide, and 34.7 to 40.3 parts of soft water.
[0007] In the above technical scheme, a hydrophobic material having good hydrophobic properties and good fusion with the latex for preparing weather balloons is successfully synthesized by copolymerization of four specific raw materials, namely acrylate, polyacrylamide, oleamide and erucic acid amide. The hydrophobic material of the present application is added to the latex for preparing weather balloons, and the hydrophobic material can form a stable interface with the natural latex and chloroprene latex in the latex, so as to achieve uniform mixing of the hydrophobic material and the latex, so that the hydrophobic material can be evenly dispersed in the weather balloon, and the hydrophobic material can reduce the surface tension of the weather balloon because of its uniform dispersion in the weather balloon, effectively reduce the adhesion of condensed water, and reduce the risk of explosion caused by ice crystal friction. In addition, the present application found in the study that the hydrophobic material prepared by the present application can also significantly improve the tensile strength and tensile growth rate of the weather balloon, which further enhances the expansibility of the weather balloon, so that the weather balloon has a higher release height.
[0008] Preferably, the hydrophobic material comprises the following components in parts by mass: 10.5 parts of acrylate, 6.86 parts of polyacrylamide, 10.5 parts of oleamide, 5.04 parts of erucamide, and 37.13 parts of soft water.
[0009] In the above technical scheme, by optimizing the dosage ratio of acrylate, polyacrylamide, oleamide and erucamide and adding an appropriate amount of soft water, the reaction stability of the hydrophobic material during the synthesis process is ensured, so that the overall performance of the hydrophobic material is better. Adding such a hydrophobic material to the latex for preparing meteorological balloons can further improve the hydrophobicity and expandability of the meteorological balloons, and ensure the stability and reliability of the meteorological balloons in extreme high-altitude environments.
[0010] Preferably, the acrylate is one of methyl acrylate, ethyl acrylate and butyl acrylate.
[0011] Preferably, the acrylate is ethyl acrylate.
[0012] In the above technical solution, the present application has found through research that when ethyl acrylate is added when preparing the hydrophobic material, the best hydrophobic performance and fusion effect with latex can be obtained. In addition, ethyl acrylate has a moderate molecular weight and is easy to disperse in latex, and will not have a negative impact on the physical properties of the weather balloon.
[0013] In a second aspect, the present application provides a preparation process for a hydrophobic material using the following technical solution: A process for preparing a hydrophobic material comprises the following steps: Step S1, pretreatment: acrylate, polyacrylamide, oleamide and erucamide are mixed and heated to 82-85° C. with stirring to obtain a preparatory solution; soft water is heated to 82-85° C.; Step S2: While stirring, slowly add the preparatory liquid into soft water, and continue stirring for 2 to 3 hours to obtain a hydrophobic material.
[0014] In the above technical scheme, the pretreatment step S1 ensures that acrylate, polyacrylamide, oleamide and erucamide are fully mixed and reach a suitable reaction temperature, creating good conditions for the subsequent copolymerization reaction. In step S2, the preparatory liquid is slowly added to the soft water and continuously stirred. By controlling the reaction time, the raw materials can fully react with each other, avoiding the problem of incomplete reaction, and ensuring that a hydrophobic material with good performance can be generated.
[0015] Preferably, the stirring speed of step 1 and step 2 is 300-500 rpm.
[0016] In the above technical solution, by controlling the stirring speed within 300-500 rpm, the raw materials can be mixed evenly, while avoiding excessive bubbles due to excessive stirring speed, which affects the quality of the hydrophobic material. In addition, the appropriate stirring speed helps to control the reaction temperature and ensure the stable reaction, thereby obtaining a hydrophobic material with better performance.
[0017] In a third aspect, the present application provides an application of a hydrophobic material in the preparation of a weather balloon using the following technical solution: an application of a hydrophobic material in the preparation of a weather balloon, wherein the hydrophobic material is added during the preparation of the weather balloon.
[0018] In the above technical solution, by adding the hydrophobic material of the present application to the latex for preparing the weather balloon, the uniform distribution of the hydrophobic material inside the weather balloon can be ensured. Since the hydrophobic material exists inside the weather balloon and the hydrophobic material and the weather balloon have good fusion, it will not produce cracks or fall off during the balloon expansion process, nor will it cause microscopic defects to form inside the weather balloon, which makes the weather balloon have good hydrophobicity and expansion properties, and makes the weather balloon have higher anti-explosion ability in low temperature environment.
[0019] Preferably, the weather balloon comprises the following components in parts by mass: 100 parts of centrifugal concentrated natural latex, 5 to 11 parts of chloroprene latex, 0.1 to 0.3 parts of potassium hydroxide, 0.2 to 0.4 parts of casein, 1 to 2 parts of sulfur, 1 to 2 parts of antioxidant, 1 to 2 parts of antioxidant, 1 to 2 parts of accelerator, 0.5 to 3 parts of zinc oxide, 5 to 9 parts of dioctyl sebacate, and 6 to 12 parts of hydrophobic material.
[0020] In the above technical solution, by adding the hydrophobic material of the present application to the above optimized latex formula, the fusion of the hydrophobic material and the latex is further improved, so that the weather balloon has good hydrophobic properties and can maintain excellent expansion. The addition of the hydrophobic material not only allows the water droplets on the balloon surface to roll off quickly, reducing the residence time of the water droplets on the balloon surface, thereby reducing the risk of explosion caused by the freezing of the water droplets, but also improves the tensile strength and tensile elongation of the balloon.
[0021] Preferably, the method for preparing the weather balloon comprises the following steps: Step 1, pretreatment: sulfur, antioxidant D, antioxidant 616, accelerator DM and zinc oxide are respectively prepared into water dispersions; potassium hydroxide and casein are respectively prepared into aqueous solutions; dioctyl sebacate is prepared into an emulsion; Step 2: Add the raw materials to the centrifugal concentrated natural rubber latex in the following order: casein solution → potassium hydroxide solution → sulfur dispersion → antioxidant dispersion → antioxidant dispersion → accelerator dispersion → zinc oxide dispersion → dioctyl sebacate emulsion → chloroprene rubber latex. After the addition is completed, stir until fully mixed, then add the hydrophobic material and continue stirring for 4 to 5 hours to obtain latex; Step 3: The latex is subjected to dipping, demoulding, water soaking, inflation and shaping, vulcanization, testing and packaging to obtain a weather balloon.
[0022] In the above technical solution, in step 2, various dispersions and emulsions are sequentially added to the centrifugal concentrated natural latex, and sufficient mixing is ensured in each step, so that the uniformity of the latex formula can be ensured. In step 3, the latex is subjected to a series of processing steps such as dipping, demoulding, soaking in water, inflation and shaping, vulcanization, testing and packaging, and finally a weather balloon with good hydrophobicity and expansion properties is obtained.
[0023] Preferably, the temperature of step 2 is controlled at 5-30° C., and the stirring speed is 35-50 rpm.
[0024] In the above technical scheme, the present application ensures the stability of the latex when adding various dispersions and emulsions by controlling the temperature of step 2 within the range of 5 to 30°C, thereby avoiding deterioration or premature vulcanization of the latex due to excessively high temperature. By controlling the stirring speed at 35 to 50 rpm, the raw materials can be mixed evenly, while avoiding the generation of excessive bubbles due to excessive stirring speed, which affects the quality of the weather balloon.
[0025] In summary, the present application includes at least one of the following beneficial technical effects: 1. This application optimizes the formula of hydrophobic materials and specifically selects acrylate, polyacrylamide, oleamide and erucamide to synthesize hydrophobic materials, thereby ensuring the fusion of hydrophobic materials and latex, so that the weather balloon has excellent hydrophobicity and expansibility, thereby improving the overall performance of the weather balloon, improving the stability and reliability of the weather balloon in extreme high-altitude environments, increasing the launch height of the weather balloon, and increasing the success rate of the weather balloon's launch.
[0026] 2. This application ensures the reaction sufficiency of the hydrophobic material by optimizing the preparation process of the hydrophobic material, further improves the performance of the hydrophobic material, and ensures the quality of the hydrophobic material.
[0027] 3. This application further improves the hydrophobicity and expandability of the weather balloon by optimizing the latex formula and preparation method of the weather balloon, so that the weather balloon has a higher explosion resistance in a low temperature environment while maintaining excellent tensile strength and tensile elongation. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 : Figure 1 The left side is the weather balloon of Example 5. Figure 1 The weather balloon of Example 1 is shown on the right. DETAILED DESCRIPTION
[0029] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments.
[0030] Example 1 A hydrophobic material is prepared from acrylate, polyacrylamide, oleamide, erucamide and soft water.
[0031] Specifically, the acrylic acid ester is ethyl acrylate.
[0032] Among them, some sources of raw materials are shown in Table 1.
[0033] Table 1: raw material source Ethyl acrylate Jiangmen Xinying Adhesive Products Co., Ltd. Polyacrylamide Jiangmen Xinying Adhesive Products Co., Ltd. Oleamide Jiangmen Xinying Adhesive Products Co., Ltd. Erucamide PMC Erucic Acid Amide from PMC Corporation of the United States The preparation method of the hydrophobic material comprises the following steps: Step S1, pretreatment: acrylate, polyacrylamide, oleamide and erucamide are mixed and heated to 83°C at a stirring speed of 400 rpm to obtain a preliminary solution; soft water is heated to 83°C.
[0034] Step S2: While stirring at 400 rpm, slowly add the preparatory liquid into soft water, and continue stirring at 400 rpm for 2.5 hours to obtain a hydrophobic material.
[0035] Example 2 A hydrophobic material, which is different from Example 1 in that the amounts of various raw materials used are inconsistent.
[0036] The preparation method of the hydrophobic material comprises the following steps: Step S1, pretreatment: acrylate, polyacrylamide, oleamide and erucamide are mixed and heated to 85°C at a stirring speed of 300 rpm to obtain a preliminary solution; soft water is heated to 85°C.
[0037] Step S2: While stirring at 300 rpm, slowly add the preparatory liquid into soft water, and continue stirring at 300 rpm for 3 hours to obtain a hydrophobic material.
[0038] Example 3 A hydrophobic material, which is different from Example 1 in that the amounts of various raw materials used are inconsistent.
[0039] The preparation method of the hydrophobic material comprises the following steps: Step S1, pretreatment: acrylate, polyacrylamide, oleamide and erucamide are mixed and heated to 82°C at a stirring speed of 500 rpm to obtain a preliminary solution; soft water is heated to 82°C.
[0040] Step S2: While stirring at 500 rpm, slowly add the preparatory liquid into soft water, and continue stirring at 500 rpm for 2 hours to obtain a hydrophobic material.
[0041] The amounts (kg) of the various raw materials of the hydrophobic materials of Examples 1-3 are shown in Table 2.
[0042] Table 2: Comparative Example 1 A hydrophobic material, which is different from Example 1 in that the acrylic ester is replaced by 5# machine oil.
[0043] Among them, 5# mechanical oil was purchased from Guangzhou Baichun Trading Co., Ltd.
[0044] Comparative Example 2 A hydrophobic material, which is different from Example 1 in that polyacrylamide is replaced by sodium polyacrylamide.
[0045] Comparative Example 3 A hydrophobic material, which is different from Example 1 in that oleic acid amide is replaced by salicylamide.
[0046] Comparative Example 4 A hydrophobic material, which is different from Example 1 in that erucic acid amide is replaced by acetamide.
[0047] Application Example 1 A weather balloon comprises the following raw materials: centrifugally concentrated natural rubber latex, chloroprene rubber latex, potassium hydroxide, casein, sulfur, an antioxidant, an antioxidant, an accelerator, zinc oxide, dioctyl sebacate, and a hydrophobic material.
[0048] Among them, the antioxidant is antioxidant D, which was purchased from Henan Kailun Chemical Co., Ltd.
[0049] The antioxidant was antioxidant 616, which was purchased from Jiangsu Feiya Chemical Industry Co., Ltd.
[0050] The accelerator was accelerator DM, which was purchased from Guangzhou Liben Rubber Raw Materials Trading Co., Ltd.
[0051] The hydrophobic material is derived from Example 1.
[0052] The method for preparing a weather balloon comprises the following steps: Step 1, pretreatment: sulfur, antioxidant D, antioxidant 616, accelerator DM and zinc oxide are prepared into water dispersions respectively; potassium hydroxide and casein are prepared into aqueous solutions respectively; dioctyl sebacate is prepared into an emulsion.
[0053] Step 2: The temperature is controlled at 15°C, and the raw materials are added to the centrifugal concentrated natural latex in the following order: casein solution → potassium hydroxide solution → sulfur dispersion → antioxidant D dispersion → antioxidant 616 dispersion → accelerator DM dispersion → zinc oxide dispersion → dioctyl sebacate emulsion → chloroprene rubber latex. After the addition is completed, stir at 40 rpm until fully mixed, then add the hydrophobic material and continue stirring at 40 rpm for 4.5 hours to obtain latex.
[0054] Step 3: The latex is subjected to dipping, demoulding, water soaking, inflation and shaping, vulcanization, testing and packaging to obtain a weather balloon.
[0055] The specific method for preparing the aqueous dispersion of sulfur, antioxidant D, antioxidant 616, accelerator DM and zinc oxide in step 1 is shown in Table 3.
[0056] Table 3: Wherein, the specific method for preparing the aqueous solution of potassium hydroxide and casein in step 1 is shown in Table 4.
[0057] Table 4: Wherein, the specific steps of preparing dioctyl sebacate into an emulsion in step 1 are as follows: Step a: Take 21 kg of dioctyl sebacate, 3.366 kg of oleic acid, and 1.47 kg of solid paraffin, mix and heat to 85° C. to obtain liquid 1; take 1.87 kg of triethanolamine and 37.1 kg of soft water, mix and heat to 85° C. to obtain liquid 2.
[0058] Step b: Slowly add liquid 1 into liquid 2, mix and emulsify completely, then add 5.194 kg of casein, continue stirring evenly, and obtain dioctyl sebacate emulsion.
[0059] Wherein, the impregnation in step 3 refers to evenly impregnating the latex on the weather balloon mold.
[0060] The vulcanization in step 3 refers to direct steam vulcanization at 110° C. for 15 minutes.
[0061] Application Example 2 A weather balloon, which is different from Application Example 1 in that the amounts of various raw materials used are inconsistent.
[0062] Among them, the hydrophobic material comes from Example 2.
[0063] The method for preparing a weather balloon comprises the following steps: Step 1, pretreatment: sulfur, antioxidant D, antioxidant 616, accelerator DM and zinc oxide are prepared into water dispersions respectively; potassium hydroxide and casein are prepared into aqueous solutions respectively; dioctyl sebacate is prepared into an emulsion.
[0064] Step 2: The temperature is controlled at 30°C, and the raw materials are added to the centrifugal concentrated natural latex in the following order: casein solution → potassium hydroxide solution → sulfur dispersion → antioxidant D dispersion → antioxidant 616 dispersion → accelerator DM dispersion → zinc oxide dispersion → dioctyl sebacate emulsion → chloroprene rubber latex. After the addition is completed, stir at 35 rpm until fully mixed, then add the hydrophobic material and continue stirring at 35 rpm for 5 hours to obtain latex.
[0065] Step 3: The latex is subjected to dipping, demoulding, water soaking, inflation and shaping, vulcanization, testing and packaging to obtain a weather balloon.
[0066] Application Example 3 A weather balloon, which is different from Application Example 1 in that the amounts of various raw materials used are inconsistent.
[0067] Among them, the hydrophobic material comes from Example 3.
[0068] The method for preparing a weather balloon comprises the following steps: Step 1, pretreatment: sulfur, antioxidant D, antioxidant 616, accelerator DM and zinc oxide are prepared into water dispersions respectively; potassium hydroxide and casein are prepared into aqueous solutions respectively; dioctyl sebacate is prepared into an emulsion.
[0069] Step 2: The temperature is controlled at 5°C, and the raw materials are added to the centrifugal concentrated natural latex in the following order: casein solution → potassium hydroxide solution → sulfur dispersion → antioxidant D dispersion → antioxidant 616 dispersion → accelerator DM dispersion → zinc oxide dispersion → dioctyl sebacate emulsion → chloroprene rubber latex. After the addition is completed, stir at 50 rpm until fully mixed, then add the hydrophobic material and continue stirring at 50 rpm for 4 hours to obtain latex.
[0070] Step 3: The latex is subjected to dipping, demoulding, water soaking, inflation and shaping, vulcanization, testing and packaging to obtain a weather balloon.
[0071] The amount of each raw material used in Application Examples 1-3 (dry weight / kg) is shown in Table 5.
[0072] Table 5: Comparative application example 1 A weather balloon, which is different from Application Example 1 in that the hydrophobic material comes from Comparative Example 1.
[0073] Comparative Application Example 2 A weather balloon, which is different from Application Example 1 in that the hydrophobic material comes from Comparative Example 2.
[0074] Comparative Application Example 3 A weather balloon, which is different from Application Example 1 in that the hydrophobic material comes from Comparative Example 3.
[0075] Comparative Application Example 4 A weather balloon, which is different from Application Example 1 in that the hydrophobic material comes from Comparative Example 4.
[0076] Comparative Application Example 5 A weather balloon, which is different from Application Example 1 in that it does not contain hydrophobic material.
[0077] Hydrophobicity test: Spray the same amount of water on the surface of the weather balloons in Example 1 and Comparative Example 5, and observe the degree of water retention on the surface of the two. The test results are shown in Figure 1 ,observe Figure 1 , Figure 1 On the left is the weather balloon of Example 5, with water droplets hanging on its surface. Figure 1 The right side is the weather balloon of Example 1, and there are no water droplets visible to the naked eye on the surface, which shows that the weather balloon of Example 1 has good hydrophobic properties.
[0078] Appearance inspection: Visually inspect the surface of the weather balloons of Example 1-3 and Comparative Application Example 1-5 to see if there are holes, cracks, bubbles, thin spots, flow marks, rubber strips, uneven thickness and other appearance defects. The inspection results are shown in Table 6.
[0079] Tensile strength and tensile elongation test: According to the test standards of QX / T222-2013 "Natural latex balloons by immersion method for weather balloons" and Q / SYQX 1-2022 "Weather balloons", the tensile strength and tensile elongation of the weather balloons of corresponding application examples 1-3 and comparative application examples 1-5 were tested. The test results are shown in Table 7.
[0080] Table 6: Group Appearance Application Example 1 No appearance defects such as holes, cracks, bubbles, thin spots, flow marks, glue strips, uneven thickness, etc. Application Example 2 No appearance defects such as holes, cracks, bubbles, thin spots, flow marks, glue strips, uneven thickness, etc. Application Example 3 No appearance defects such as holes, cracks, bubbles, thin spots, flow marks, glue strips, uneven thickness, etc. Comparative application example 1 No appearance defects such as holes, cracks, bubbles, thin spots, flow marks, glue strips, uneven thickness, etc. Comparative Application Example 2 No appearance defects such as holes, cracks, bubbles, thin spots, flow marks, glue strips, uneven thickness, etc. Comparative Application Example 3 No appearance defects such as holes, cracks, bubbles, thin spots, flow marks, glue strips, uneven thickness, etc. Comparative Application Example 4 No appearance defects such as holes, cracks, bubbles, thin spots, flow marks, glue strips, uneven thickness, etc. Comparative Application Example 5 No appearance defects such as holes, cracks, bubbles, thin spots, flow marks, glue strips, uneven thickness, etc. Table 7: Specifically combined with application examples 1-3 and comparative application examples 1-5, it is not difficult to see that the weather balloon prepared in the application example of this application has good hydrophobicity, tensile strength and tensile elongation. In other words, the weather balloon in the application example of this application has good hydrophobicity and expansion.
[0081] Specifically, in combination with Application Example 1 and Comparative Application Examples 1-4, the difference between Application Example 1 and Comparative Application Examples 1-4 is that the hydrophobic materials used in Application Example 1 and Comparative Application Examples 1-4 are inconsistent. The hydrophobic materials used in Comparative Application Examples 1-4 replace acrylate, polyacrylamide, oleamide and erucamide with other similar raw materials, respectively. Application Example 1 obviously has good hydrophobicity and swelling properties. It can be seen that only by specifically selecting acrylate, polyacrylamide, oleamide and erucamide to synthesize hydrophobic materials can the fusion of hydrophobic materials and latex be ensured, so that the weather balloon has excellent hydrophobicity and swelling properties, thereby improving the overall performance of the weather balloon.
[0082] Specifically combined with the analysis of Application Example 1 and Comparative Application Example 5, the difference between Application Example 1 and Comparative Application Example 5 is that: Comparative Application Example 5 does not use hydrophobic materials, and Application Example 1 obviously has good hydrophobicity and expansibility. It can be seen that adding the hydrophobic material of the present application to the weather balloon not only improves the hydrophobicity of the weather balloon, but also achieves an unexpected effect of improving the tensile strength and tensile elongation of the weather balloon, so that the weather balloon has excellent hydrophobicity and expansibility, improves the stability and reliability of the weather balloon in extreme high-altitude environments, increases the release height of the weather balloon, and increases the success rate of the weather balloon's launch.
[0083] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A hydrophobic material, It is characterized in that The invention comprises the following components in parts by weight: 8 to 13 parts of acrylate, 5.92 to 9.74 parts of polyacrylamide, 8.7 to 12.4 parts of oleamide, 3.68 to 7.56 parts of erucamide, and 34.7 to 40.3 parts of soft water.
2. A hydrophobic material according to claim 1, It is characterized in that The invention comprises the following components in parts by weight: 10.5 parts of acrylate, 6.86 parts of polyacrylamide, 10.5 parts of oleamide, 5.04 parts of erucamide, and 37.13 parts of soft water.
3. A process for preparing the hydrophobic material according to claim 1 or 2, It is characterized in that The following steps are involved: Step S1, pretreatment: acrylate, polyacrylamide, oleamide and erucamide are mixed and heated to 82-85° C. with stirring to obtain a preparatory solution; Heat soft water to 82~85℃; Step S2: While stirring, slowly add the preparatory liquid into soft water, and continue stirring for 2 to 3 hours to obtain a hydrophobic material.
4. A process for preparing a hydrophobic material according to claim 3, It is characterized in that The stirring speed of step 1 and step 2 is 300-500 rpm.
5. Use of the hydrophobic material according to claim 1 or 2 in preparing a weather balloon, It is characterized in that Add hydrophobic materials when preparing weather balloons.
6. Use of the hydrophobic material according to claim 5 in preparing a weather balloon, It is characterized in that The weather balloon comprises the following components in parts by mass: 100 parts of centrifugal concentrated natural latex, 5 to 11 parts of chloroprene latex, 0.1 to 0.3 parts of potassium hydroxide, 0.2 to 0.4 parts of casein, 1 to 2 parts of sulfur, 1 to 2 parts of antioxidant, 1 to 2 parts of antioxidant, 1 to 2 parts of accelerator, 0.5 to 3 parts of zinc oxide, 5 to 9 parts of dioctyl sebacate, and 6 to 12 parts of hydrophobic material.
7. Use of the hydrophobic material according to claim 6 in preparing a weather balloon, It is characterized in that The method for preparing the weather balloon comprises the following steps: Step 1, pretreatment: sulfur, antioxidant, antioxidant, accelerator and zinc oxide are respectively prepared into water dispersions; potassium hydroxide and casein are respectively prepared into aqueous solutions; dioctyl sebacate is prepared into an emulsion; Step 2: Add the raw materials to the centrifugal concentrated natural rubber latex in the following order: casein solution → potassium hydroxide solution → sulfur dispersion → antioxidant dispersion → antioxidant dispersion → accelerator dispersion → zinc oxide dispersion → dioctyl sebacate emulsion → chloroprene rubber latex. After the addition is completed, stir until fully mixed, then add the hydrophobic material and continue stirring for 4-5 hours to obtain latex; Step 3: The latex is subjected to dipping, demoulding, water soaking, inflation and shaping, vulcanization, testing and packaging to obtain a weather balloon.
8. Use of the hydrophobic material according to claim 7 in preparing a weather balloon, It is characterized in that The temperature of step 2 is controlled at 5-30° C. and the stirring speed is 35-50 rpm.
Citation Information
Cited By
Plastic model for producing polyurethane balloon and production process of plastic model
CN120307554A
Rubber composite material for high-altitude ice crystal sounding balloon and preparation method thereof
CN122832370A