Waterproof and mildew-proof shaving board and processing method thereof

By combining modified soybean meal adhesive with paraffin emulsion and calcium chloride solution, the problem of insufficient water resistance of traditional soybean meal adhesive is solved, the waterproof performance and durability of particleboard are improved, and mold growth is reduced.

CN118994932APending Publication Date: 2024-11-22HUBEI YINGLIN IND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411127157.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Traditional soybean meal adhesives are insufficient in particleboard applications and are prone to hydrolysis, leading to the breeding of mold and affecting the waterproof performance and durability of particleboard.

Method used

Modified soybean meal adhesive is made of soybean meal powder, urea, lithium bromide, distilled water and acetic vinegar emulsion, etc., and is used as waterproofing agent and wetting agent with paraffin emulsion and calcium chloride solution. It is made of waterproof and mildew-proof by hot pressing. particle board.

Benefits of technology

It improves the waterproof performance and durability of particleboard, reduces mold growth, and extends the service life of particleboard.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004996909500000141
    Figure BDA0004996909500000141
Patent Text Reader

Abstract

The invention discloses a waterproof and mildewproof shaving board and a processing method thereof, and belongs to the technical field of shaving board processing.The waterproof and mildewproof shaving board is prepared by mixing a modified soybean meal adhesive with a pretreated straw raw material and modifying the soybean meal adhesive with lithium bromide and urea; oxygen atoms and nitrogen atoms contained in the urea react with hydroxyl groups in the soybean protein to destroy hydrogen bonds which keep a polypeptide chain space structure, so that a polymer is expanded, lithium ions in lithium bromide and oxygen of the hydroxyl groups in soybean protein molecules are subjected to a coordination reaction to destroy a hydrogen bond network structure of the soybean protein, so that a soybean protein structure is expanded, and the soybean protein structure is expanded; according to the present invention, internal hydrophobic groups are exposed, solubility is increased, the wetting agent of the neutral solution is adopted to pre-treat the straw so as to improve wettability, the waterproof performance detection results of the shaving board show that the shaving board has excellent water resistance, and the modified soybean meal adhesive is not easily hydrolyzed so as to reduce mold breeding; and therefore, the waterproof performance and durability of the shaving board are ensured.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of particle board processing, in particular to a waterproof and mildew-proof particle board and a processing method thereof. Background Art

[0002] Particleboard is also called particle board. It is a man-made board made of wood or wood fiber material fragments. These fragments are dried, mixed with additives such as glue, hardener and waterproofing agent, and pressed under a certain temperature and pressure. The particles of particleboard are arranged unevenly, but this structure makes it have good sound absorption and sound insulation performance, as well as moderate lateral load-bearing capacity.

[0003] Particleboard has the characteristics of uniform density, smooth surface, stable size and easy processing. It is suitable for furniture manufacturing, construction industry and interior decoration, especially in occasions where sound absorption and sound insulation performance are required. The internal structure of particleboard is a cross-staggered granular shape, which means that its performance in all directions is basically the same, which is suitable for making parts that need to withstand a certain load.

[0004] Currently, straw is usually used as raw material in particleboard production, and soybean meal adhesive is used to complete the processing of particleboard. The surface wettability of straw is poor, and the waxy substances and impurities on the surface affect the bonding of straw fibers and soybean meal adhesive, which limits the production and application of straw particleboard. In addition, traditional soybean meal adhesives are not water-resistant enough in particleboard applications and are prone to hydrolysis, leading to the growth of mold, which affects the waterproof performance and durability of the particleboard. Summary of the invention

[0005] In order to overcome the above defects, the present invention provides a waterproof and mildew-proof particleboard and a processing method thereof, which solves the problem that traditional soybean meal adhesives are insufficiently water-resistant in particleboard applications, are easily hydrolyzed, and lead to the growth of mold, thus affecting the waterproof performance and durability of the particleboard.

[0006] To achieve the above object, the present invention provides the following technical solution: a waterproof and mildew-proof particleboard, the particleboard is made of straw raw material, modified soybean meal adhesive, waterproofing agent and wetting agent;

[0007] The modified soybean meal adhesive is made of soybean meal powder, urea, lithium bromide, distilled water, acetic acid propylene emulsion and MDI curing agent;

[0008] The waterproofing agent is paraffin emulsion, and the wetting agent is calcium chloride solution.

[0009] As a further embodiment of the present invention: the mass ratio of the soybean meal powder, urea, lithium bromide and distilled water is 8-10:7-8:0.1-0.15:40-45.

[0010] As a further solution of the present invention: the mass ratio of the acetic acid propylene glycol emulsion to the MDI curing agent is 8-9:7-8.

[0011] A method for processing a waterproof and mildew-proof particleboard, the processing method comprising the following steps:

[0012] S1. preparing modified soybean meal adhesive;

[0013] S2, pretreatment of straw raw materials;

[0014] S3, pressed low density straw particle board.

[0015] As a further solution of the present invention: the specific steps of S1 are as follows:

[0016] S101, add 10 parts of soybean meal, 7-8 parts of urea, 0.1 parts of lithium bromide, and 40-45 parts of distilled water into a flask, fix the flask in a 30°C constant temperature water bath, turn on an electric stirrer and stir for 30-40 minutes;

[0017] S102, then add 85-90 parts of acetic acid propylene emulsion and stir for 8-10 minutes, then add 7-8 parts of MDI curing agent and stir for 5-8 minutes to prepare modified soybean meal adhesive.

[0018] As a further solution of the present invention: the specific steps of S2 are as follows:

[0019] S201, crushing straw raw materials to obtain straw crushed materials with a particle size of 3-4 mm, adding them into a beaker, and preparing 20% ​​calcium chloride solution, adding it into the beaker, and soaking for 20-24 hours;

[0020] S202, then take out the straw chips and put them into a forced air drying oven at a temperature of 80-85°C and dry them for 4-5 hours.

[0021] As a further solution of the present invention: the specific steps of S3 are as follows:

[0022] S301, adding modified soybean meal adhesive to the pretreated straw fragments, stirring for 5-8 minutes, then pouring in the waterproofing agent paraffin emulsion and stirring again for 3-5 minutes;

[0023] S302, coating one side of two carrier plates with paraffin wax, and placing a mixture of straw chips and modified soybean meal adhesive into the mixture for hot pressing;

[0024] S303. After hot pressing, take out the board and place it in a cool place for 72 hours to complete the processing of the waterproof and mildew-proof particle board.

[0025] As a further solution of the present invention: in S302, the waterproofing agent accounts for 5-15% of the mass of the particleboard, and the amount of the modified soybean meal adhesive applied is 28-30%.

[0026] As a further solution of the present invention: in the hot pressing treatment, the hot pressing pressure is 1.2-1.4 MPa, the hot pressing time is 1200-1500 s, and the hot pressing temperature is 170-180°C.

[0027] Compared with the prior art, the beneficial effects of the present invention are as follows: a modified soybean meal adhesive is used to mix with pretreated straw raw materials to press a low-density straw particleboard, and lithium bromide and urea are used to modify the soybean meal adhesive, oxygen atoms and nitrogen atoms contained in urea react with hydroxyl groups in soybean protein to destroy the hydrogen bonds that maintain the spatial structure of the polypeptide chain and unfold the polymer, lithium ions in lithium bromide coordinate with oxygen of hydroxyl groups in soybean protein molecules to destroy the hydrogen bond network structure of soybean protein, unfold the soybean protein structure, expose internal hydrophobic groups, and increase solubility, a neutral solution wetting agent is used to pretreat the straw to improve wettability, and through the particleboard waterproof performance test, the particleboard has excellent waterproof performance, because the modified soybean meal adhesive is not easy to hydrolyze, can reduce mold growth, and thus ensure the waterproof performance and durability of the particleboard. DETAILED DESCRIPTION

[0028] The technical solution of the present application is further described in detail below in conjunction with specific implementation methods.

[0029] The invention provides a technical solution: a waterproof and mildew-proof particle board and a processing method thereof.

[0030] Embodiment 1:

[0031] A waterproof and mildew-proof particle board, the particle board is made of straw raw material, modified soybean meal adhesive, waterproofing agent and wetting agent;

[0032] The modified soybean meal adhesive is made of soybean meal powder, urea, lithium bromide, distilled water, acetic acid propylene emulsion and MDI curing agent;

[0033] The waterproofing agent is paraffin emulsion and the wetting agent is calcium chloride solution.

[0034] The mass ratio of soybean meal, urea, lithium bromide and distilled water is 8-10:7-8:0.1-0.15:40-45.

[0035] The mass ratio of acetic acid acrylic emulsion to MDI curing agent is 8-9:7-8.

[0036] A method for processing a waterproof and mildew-proof particleboard, the processing method comprising the following steps:

[0037] S1. preparing modified soybean meal adhesive;

[0038] S101, add 10 parts of soybean meal, 7-8 parts of urea, 0.1 parts of lithium bromide, and 40-45 parts of distilled water into a flask, fix the flask in a 30°C constant temperature water bath, turn on an electric stirrer and stir for 30-40 minutes;

[0039] S102, then add 85-90 parts of acetic acid propylene emulsion and stir for 8-10 minutes, then add 7-8 parts of MDI curing agent and stir for 5-8 minutes to prepare modified soybean meal adhesive.

[0040] S2, pretreatment of straw raw materials;

[0041] S201, crushing straw raw materials to obtain straw crushed materials with a particle size of 3-4 mm, adding them into a beaker, and preparing 20% ​​calcium chloride solution, adding it into the beaker, and soaking for 20-24 hours;

[0042] S202, then take out the straw chips and put them into a forced air drying oven at a temperature of 80-85°C and dry them for 4-5 hours.

[0043] S3, pressed low-density straw particleboard;

[0044] S301, adding modified soybean meal adhesive to the pretreated straw fragments, stirring for 5-8 minutes, then pouring in the waterproofing agent paraffin emulsion and stirring again for 3-5 minutes;

[0045] S302, coating one side of two carrier plates with paraffin wax, and placing a mixture of straw chips and modified soybean meal adhesive into the mixture for hot pressing;

[0046] S303. After hot pressing, take out the board and place it in a cool place for 72 hours to complete the processing of the waterproof and mildew-proof particle board.

[0047] In S302, the waterproofing agent accounts for 7% of the particleboard mass, and the modified soybean meal adhesive is applied at a sizing amount of 28-30%;

[0048] During the hot pressing treatment, the hot pressing pressure is 1.2-1.4 MPa, the hot pressing time is 1200 s, and the hot pressing temperature is 170°C.

[0049] Embodiment 2:

[0050] A waterproof and mildew-proof particle board, the particle board is made of straw raw material, modified soybean meal adhesive, waterproofing agent and wetting agent;

[0051] The modified soybean meal adhesive is made of soybean meal powder, urea, lithium bromide, distilled water, acetic acid propylene emulsion and MDI curing agent;

[0052] The waterproofing agent is paraffin emulsion and the wetting agent is calcium chloride solution.

[0053] The mass ratio of soybean meal, urea, lithium bromide and distilled water is 8-10:7-8:0.1-0.15:40-45.

[0054] The mass ratio of acetic acid acrylic emulsion to MDI curing agent is 8-9:7-8.

[0055] A method for processing a waterproof and mildew-proof particleboard, the processing method comprising the following steps:

[0056] S1. preparing modified soybean meal adhesive;

[0057] S101, add 10 parts of soybean meal, 7-8 parts of urea, 0.1 parts of lithium bromide, and 40-45 parts of distilled water into a flask, fix the flask in a 30°C constant temperature water bath, turn on an electric stirrer and stir for 30-40 minutes;

[0058] S102, then add 85-90 parts of acetic acid propylene emulsion and stir for 8-10 minutes, then add 7-8 parts of MDI curing agent and stir for 5-8 minutes to prepare modified soybean meal adhesive.

[0059] S2, pretreatment of straw raw materials;

[0060] S201, crushing straw raw materials to obtain straw crushed materials with a particle size of 3-4 mm, adding them into a beaker, and preparing 20% ​​calcium chloride solution, adding it into the beaker, and soaking for 20-24 hours;

[0061] S202, then take out the straw chips and put them into a forced air drying oven at a temperature of 80-85°C and dry them for 4-5 hours.

[0062] S3, pressed low-density straw particleboard;

[0063] S301, adding modified soybean meal adhesive to the pretreated straw fragments, stirring for 5-8 minutes, then pouring in the waterproofing agent paraffin emulsion and stirring again for 3-5 minutes;

[0064] S302, coating one side of two carrier plates with paraffin wax, and placing a mixture of straw chips and modified soybean meal adhesive into the mixture for hot pressing;

[0065] S303. After hot pressing, take out the board and place it in a cool place for 72 hours to complete the processing of the waterproof and mildew-proof particle board.

[0066] In S302, the waterproofing agent accounts for 10% of the particleboard mass, and the modified soybean meal adhesive is applied at a sizing amount of 28-30%;

[0067] During the hot pressing treatment, the hot pressing pressure is 1.2-1.4 MPa, the hot pressing time is 1200 s, and the hot pressing temperature is 175°C.

[0068] Embodiment 3:

[0069] A waterproof and mildew-proof particle board, the particle board is made of straw raw material, modified soybean meal adhesive, waterproofing agent and wetting agent;

[0070] The modified soybean meal adhesive is made of soybean meal powder, urea, lithium bromide, distilled water, acetic acid propylene emulsion and MDI curing agent;

[0071] The waterproofing agent is paraffin emulsion and the wetting agent is calcium chloride solution.

[0072] The mass ratio of soybean meal, urea, lithium bromide and distilled water is 8-10:7-8:0.1-0.15:40-45.

[0073] The mass ratio of acetic acid acrylic emulsion to MDI curing agent is 8-9:7-8.

[0074] A method for processing a waterproof and mildew-proof particleboard, the processing method comprising the following steps:

[0075] S1. preparing modified soybean meal adhesive;

[0076] S101, add 10 parts of soybean meal, 7-8 parts of urea, 0.1 parts of lithium bromide, and 40-45 parts of distilled water into a flask, fix the flask in a 30°C constant temperature water bath, turn on an electric stirrer and stir for 30-40 minutes;

[0077] S102, then add 85-90 parts of acetic acid propylene emulsion and stir for 8-10 minutes, then add 7-8 parts of MDI curing agent and stir for 5-8 minutes to prepare modified soybean meal adhesive.

[0078] S2, pretreatment of straw raw materials;

[0079] S201, crushing straw raw materials to obtain straw crushed materials with a particle size of 3-4 mm, adding them into a beaker, and preparing 20% ​​calcium chloride solution, adding it into the beaker, and soaking for 20-24 hours;

[0080] S202, then take out the straw chips and put them into a forced air drying oven at a temperature of 80-85°C and dry them for 4-5 hours.

[0081] S3, pressed low-density straw particleboard;

[0082] S301, adding modified soybean meal adhesive to the pretreated straw fragments, stirring for 5-8 minutes, then pouring in the waterproofing agent paraffin emulsion and stirring again for 3-5 minutes;

[0083] S302, coating one side of two carrier plates with paraffin wax, and placing a mixture of straw chips and modified soybean meal adhesive into the mixture for hot pressing;

[0084] S303. After hot pressing, take out the board and place it in a cool place for 72 hours to complete the processing of the waterproof and mildew-proof particle board.

[0085] In S302, the waterproofing agent accounts for 13% of the particleboard mass, and the modified soybean meal adhesive is applied at a rate of 28-30%;

[0086] During the hot pressing treatment, the hot pressing pressure is 1.2-1.4 MPa, the hot pressing time is 1200 s, and the hot pressing temperature is 180°C.

[0087] Embodiment 4:

[0088] A waterproof and mildew-proof particle board, the particle board is made of straw raw material, modified soybean meal adhesive, waterproofing agent and wetting agent;

[0089] The modified soybean meal adhesive is made of soybean meal powder, urea, lithium bromide, distilled water, acetic acid propylene emulsion and MDI curing agent;

[0090] The waterproofing agent is paraffin emulsion and the wetting agent is calcium chloride solution.

[0091] The mass ratio of soybean meal, urea, lithium bromide and distilled water is 8-10:7-8:0.1-0.15:40-45.

[0092] The mass ratio of acetic acid acrylic emulsion to MDI curing agent is 8-9:7-8.

[0093] A method for processing a waterproof and mildew-proof particleboard, the processing method comprising the following steps:

[0094] S1. preparing modified soybean meal adhesive;

[0095] S101, add 10 parts of soybean meal, 7-8 parts of urea, 0.1 parts of lithium bromide, and 40-45 parts of distilled water into a flask, fix the flask in a 30°C constant temperature water bath, turn on an electric stirrer and stir for 30-40 minutes;

[0096] S102, then add 85-90 parts of acetic acid propylene emulsion and stir for 8-10 minutes, then add 7-8 parts of MDI curing agent and stir for 5-8 minutes to prepare modified soybean meal adhesive.

[0097] S2, pretreatment of straw raw materials;

[0098] S201, crushing straw raw materials to obtain straw crushed materials with a particle size of 3-4 mm, adding them into a beaker, and preparing 20% ​​calcium chloride solution, adding it into the beaker, and soaking for 20-24 hours;

[0099] S202, then take out the straw chips and put them into a forced air drying oven at a temperature of 80-85°C and dry them for 4-5 hours.

[0100] S3, pressed low-density straw particleboard;

[0101] S301, adding modified soybean meal adhesive to the pretreated straw fragments, stirring for 5-8 minutes, then pouring in the waterproofing agent paraffin emulsion and stirring again for 3-5 minutes;

[0102] S302, coating one side of two carrier plates with paraffin wax, and placing a mixture of straw chips and modified soybean meal adhesive into the mixture for hot pressing;

[0103] S303. After hot pressing, take out the board and place it in a cool place for 72 hours to complete the processing of the waterproof and mildew-proof particle board.

[0104] In S302, the waterproofing agent accounts for 10% of the particleboard mass, and the modified soybean meal adhesive is applied at a sizing amount of 28-30%;

[0105] During the hot pressing treatment, the hot pressing pressure is 1.2-1.4 MPa, the hot pressing time is 1350 s, and the hot pressing temperature is 170°C.

[0106] Embodiment 5:

[0107] A waterproof and mildew-proof particle board, the particle board is made of straw raw material, modified soybean meal adhesive, waterproofing agent and wetting agent;

[0108] The modified soybean meal adhesive is made of soybean meal powder, urea, lithium bromide, distilled water, acetic acid propylene emulsion and MDI curing agent;

[0109] The waterproofing agent is paraffin emulsion and the wetting agent is calcium chloride solution.

[0110] The mass ratio of soybean meal, urea, lithium bromide and distilled water is 8-10:7-8:0.1-0.15:40-45.

[0111] The mass ratio of acetic acid acrylic emulsion to MDI curing agent is 8-9:7-8.

[0112] A method for processing a waterproof and mildew-proof particleboard, the processing method comprising the following steps:

[0113] S1. preparing modified soybean meal adhesive;

[0114] S101, add 10 parts of soybean meal, 7-8 parts of urea, 0.1 parts of lithium bromide, and 40-45 parts of distilled water into a flask, fix the flask in a 30°C constant temperature water bath, turn on an electric stirrer and stir for 30-40 minutes;

[0115] S102, then add 85-90 parts of acetic acid propylene emulsion and stir for 8-10 minutes, then add 7-8 parts of MDI curing agent and stir for 5-8 minutes to prepare modified soybean meal adhesive.

[0116] S2, pretreatment of straw raw materials;

[0117] S201, crushing straw raw materials to obtain straw crushed materials with a particle size of 3-4 mm, adding them into a beaker, and preparing 20% ​​calcium chloride solution, adding it into the beaker, and soaking for 20-24 hours;

[0118] S202, then take out the straw chips and put them into a forced air drying oven at a temperature of 80-85°C and dry them for 4-5 hours.

[0119] S3, pressed low-density straw particleboard;

[0120] S301, adding modified soybean meal adhesive to the pretreated straw fragments, stirring for 5-8 minutes, then pouring in the waterproofing agent paraffin emulsion and stirring again for 3-5 minutes;

[0121] S302, coating one side of two carrier plates with paraffin wax, and placing a mixture of straw chips and modified soybean meal adhesive into the mixture for hot pressing;

[0122] S303. After hot pressing, take out the board and place it in a cool place for 72 hours to complete the processing of the waterproof and mildew-proof particle board.

[0123] In S302, the waterproofing agent accounts for 13% of the particleboard mass, and the modified soybean meal adhesive is applied at a rate of 28-30%;

[0124] During the hot pressing treatment, the hot pressing pressure is 1.2-1.4 MPa, the hot pressing time is 1350 s, and the hot pressing temperature is 175°C.

[0125] Embodiment 6:

[0126] A waterproof and mildew-proof particle board, the particle board is made of straw raw material, modified soybean meal adhesive, waterproofing agent and wetting agent;

[0127] The modified soybean meal adhesive is made of soybean meal powder, urea, lithium bromide, distilled water, acetic acid propylene emulsion and MDI curing agent;

[0128] The waterproofing agent is paraffin emulsion and the wetting agent is calcium chloride solution.

[0129] The mass ratio of soybean meal, urea, lithium bromide and distilled water is 8-10:7-8:0.1-0.15:40-45.

[0130] The mass ratio of acetic acid acrylic emulsion to MDI curing agent is 8-9:7-8.

[0131] A method for processing a waterproof and mildew-proof particleboard, the processing method comprising the following steps:

[0132] S1. preparing modified soybean meal adhesive;

[0133] S101, add 10 parts of soybean meal, 7-8 parts of urea, 0.1 parts of lithium bromide, and 40-45 parts of distilled water into a flask, fix the flask in a 30°C constant temperature water bath, turn on an electric stirrer and stir for 30-40 minutes;

[0134] S102, then add 85-90 parts of acetic acid propylene emulsion and stir for 8-10 minutes, then add 7-8 parts of MDI curing agent and stir for 5-8 minutes to prepare modified soybean meal adhesive.

[0135] S2, pretreatment of straw raw materials;

[0136] S201, crushing straw raw materials to obtain straw crushed materials with a particle size of 3-4 mm, adding them into a beaker, and preparing 20% ​​calcium chloride solution, adding it into the beaker, and soaking for 20-24 hours;

[0137] S202, then take out the straw chips and put them into a forced air drying oven at a temperature of 80-85°C and dry them for 4-5 hours.

[0138] S3, pressed low-density straw particleboard;

[0139] S301, adding modified soybean meal adhesive to the pretreated straw fragments, stirring for 5-8 minutes, then pouring in the waterproofing agent paraffin emulsion and stirring again for 3-5 minutes;

[0140] S302, coating one side of two carrier plates with paraffin wax, and placing a mixture of straw chips and modified soybean meal adhesive into the mixture for hot pressing;

[0141] S303. After hot pressing, take out the board and place it in a cool place for 72 hours to complete the processing of the waterproof and mildew-proof particle board.

[0142] In S302, the waterproofing agent accounts for 7% of the particleboard mass, and the modified soybean meal adhesive is applied at a sizing amount of 28-30%;

[0143] During the hot pressing treatment, the hot pressing pressure is 1.2-1.4 MPa, the hot pressing time is 1350 s, and the hot pressing temperature is 180°C.

[0144] Embodiment 7:

[0145] A waterproof and mildew-proof particle board, the particle board is made of straw raw material, modified soybean meal adhesive, waterproofing agent and wetting agent;

[0146] The modified soybean meal adhesive is made of soybean meal powder, urea, lithium bromide, distilled water, acetic acid propylene emulsion and MDI curing agent;

[0147] The waterproofing agent is paraffin emulsion and the wetting agent is calcium chloride solution.

[0148] The mass ratio of soybean meal, urea, lithium bromide and distilled water is 8-10:7-8:0.1-0.15:40-45.

[0149] The mass ratio of acetic acid acrylic emulsion to MDI curing agent is 8-9:7-8.

[0150] A method for processing a waterproof and mildew-proof particleboard, the processing method comprising the following steps:

[0151] S1. preparing modified soybean meal adhesive;

[0152] S101, add 10 parts of soybean meal, 7-8 parts of urea, 0.1 parts of lithium bromide, and 40-45 parts of distilled water into a flask, fix the flask in a 30°C constant temperature water bath, turn on an electric stirrer and stir for 30-40 minutes;

[0153] S102, then add 85-90 parts of acetic acid propylene emulsion and stir for 8-10 minutes, then add 7-8 parts of MDI curing agent and stir for 5-8 minutes to prepare modified soybean meal adhesive.

[0154] S2, pretreatment of straw raw materials;

[0155] S201, crushing straw raw materials to obtain straw crushed materials with a particle size of 3-4 mm, adding them into a beaker, and preparing 20% ​​calcium chloride solution, adding it into the beaker, and soaking for 20-24 hours;

[0156] S202, then take out the straw chips and put them into a forced air drying oven at a temperature of 80-85°C and dry them for 4-5 hours.

[0157] S3, pressed low-density straw particleboard;

[0158] S301, adding modified soybean meal adhesive to the pretreated straw fragments, stirring for 5-8 minutes, then pouring in the waterproofing agent paraffin emulsion and stirring again for 3-5 minutes;

[0159] S302, coating one side of two carrier plates with paraffin wax, and placing a mixture of straw chips and modified soybean meal adhesive into the mixture for hot pressing;

[0160] S303. After hot pressing, take out the board and place it in a cool place for 72 hours to complete the processing of the waterproof and mildew-proof particle board.

[0161] In S302, the waterproofing agent accounts for 13% of the particleboard mass, and the amount of the modified soybean meal adhesive applied is 28-30%; in the hot pressing treatment, the hot pressing pressure is 1.2-1.4 MPa, the hot pressing time is 1500 s, and the hot pressing temperature is 170°C. Example 8:

[0162] A waterproof and mildew-proof particle board, the particle board is made of straw raw material, modified soybean meal adhesive, waterproofing agent and wetting agent;

[0163] The modified soybean meal adhesive is made of soybean meal powder, urea, lithium bromide, distilled water, acetic acid propylene emulsion and MDI curing agent;

[0164] The waterproofing agent is paraffin emulsion and the wetting agent is calcium chloride solution.

[0165] The mass ratio of soybean meal, urea, lithium bromide and distilled water is 8-10:7-8:0.1-0.15:40-45.

[0166] The mass ratio of acetic acid acrylic emulsion to MDI curing agent is 8-9:7-8.

[0167] A method for processing a waterproof and mildew-proof particleboard, the processing method comprising the following steps:

[0168] S1. preparing modified soybean meal adhesive;

[0169] S101, add 10 parts of soybean meal, 7-8 parts of urea, 0.1 parts of lithium bromide, and 40-45 parts of distilled water into a flask, fix the flask in a 30°C constant temperature water bath, turn on an electric stirrer and stir for 30-40 minutes;

[0170] S102, then add 85-90 parts of acetic acid propylene emulsion and stir for 8-10 minutes, then add 7-8 parts of MDI curing agent and stir for 5-8 minutes to prepare modified soybean meal adhesive.

[0171] S2, pretreatment of straw raw materials;

[0172] S201, crushing straw raw materials to obtain straw crushed materials with a particle size of 3-4 mm, adding them into a beaker, and preparing 20% ​​calcium chloride solution, adding it into the beaker, and soaking for 20-24 hours;

[0173] S202, then take out the straw chips and put them into a forced air drying oven at a temperature of 80-85°C and dry them for 4-5 hours.

[0174] S3, pressed low-density straw particleboard;

[0175] S301, adding modified soybean meal adhesive to the pretreated straw fragments, stirring for 5-8 minutes, then pouring in the waterproofing agent paraffin emulsion and stirring again for 3-5 minutes;

[0176] S302, coating one side of two carrier plates with paraffin wax, and placing a mixture of straw chips and modified soybean meal adhesive into the mixture for hot pressing;

[0177] S303. After hot pressing, take out the board and place it in a cool place for 72 hours to complete the processing of the waterproof and mildew-proof particle board.

[0178] In S302, the waterproofing agent accounts for 7% of the particleboard mass, and the modified soybean meal adhesive is applied at a sizing amount of 28-30%;

[0179] During the hot pressing treatment, the hot pressing pressure is 1.2-1.4 MPa, the hot pressing time is 1500 s, and the hot pressing temperature is 175°C.

[0180] Comparative Example:

[0181] Particleboard is made from straw raw material, soybean meal adhesive, waterproofing agent and wetting agent;

[0182] The waterproofing agent is paraffin emulsion and the wetting agent is calcium chloride solution.

[0183] The processing method of particleboard includes the following steps:

[0184] Straw raw material pretreatment;

[0185] Crush the straw raw material to obtain straw crushed materials with a particle size of 3-4 mm and add them into a beaker, and prepare 20% calcium chloride solution and add it into the beaker, and soak for 20-24 hours;

[0186] Secondly, take out the straw fragments and put them into a forced air drying oven at a temperature of 80-85°C and dry them for 4-5 hours.

[0187] Pressed low-density straw particleboard;

[0188] Add soybean meal adhesive to the pretreated straw fragments and stir for 5-8 minutes, then pour in the waterproofing agent paraffin emulsion and stir again for 3-5 minutes;

[0189] Paraffin wax is applied on one side of two carrier plates, and a mixture of straw chips and soybean meal adhesive is placed in the plates for hot pressing;

[0190] After hot pressing, take out the board and place it in a cool place for 72 hours to complete the processing of the particle board.

[0191] In S302, the waterproofing agent accounts for 7% of the particleboard mass, and the soybean meal adhesive is applied at a rate of 28-30%;

[0192] During the hot pressing treatment, the hot pressing pressure is 1.2-1.4 MPa, the hot pressing time is 1500 s, and the hot pressing temperature is 170°C.

[0193] The following table is obtained based on Examples 1-8 and Comparative Examples:

[0194]

[0195] The difference between Examples 1-8 and the comparative example is that Examples 1-8 use modified soybean meal adhesive, while the comparative example uses unmodified soybean meal adhesive.

[0196] From the comparison in the above table, it can be seen that: when the hot pressing time is 1500s, the hot pressing temperature is 175℃, and the waterproofing agent accounts for 7% of the particleboard mass, the pressed particleboard has the lowest 2h water absorption expansion rate; while the particleboard made of the control example using unmodified soybean meal adhesive has the highest moisture content.

[0197] From the above, it is known that the modified soybean meal adhesive is used to mix with the pretreated straw raw material to press the low-density straw particleboard, and the soybean meal adhesive is modified by lithium bromide and urea. The oxygen atoms and nitrogen atoms contained in urea react with the hydroxyl groups in the soybean protein to destroy the hydrogen bonds that maintain the spatial structure of the polypeptide chain and unfold the polymer. The lithium ions in the lithium bromide react with the oxygen of the hydroxyl groups in the soybean protein molecules to destroy the hydrogen bond network structure of the soybean protein, unfold the soybean protein structure, expose the internal hydrophobic groups, and increase the solubility. The straw is pretreated with a neutral solution wetting agent to improve wettability.

[0198] Through the test of particleboard waterproof performance, the results showed that the particleboard has excellent waterproof properties. Because the modified soybean meal adhesive is not easy to hydrolyze, it can reduce the growth of mold, thereby ensuring the waterproof performance and durability of the particleboard.

[0199] The terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, a feature defined as "first" or "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.

[0200] In the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection, an electrical connection, or a communication; it can be a direct connection, or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0201] In the present invention, unless otherwise clearly specified and limited, the first feature "on" or "under" the second feature may be that the first and second features are in direct contact, or the first and second features are in indirect contact through an intermediate medium. In the description of this specification, the description with reference to the terms "one scheme", "some schemes", "examples", "specific examples", or "some examples" means that the specific features, structures, materials or characteristics described in conjunction with the scheme or example are included in at least one scheme or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same scheme or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more schemes or examples in a suitable manner.

Claims

1. A waterproof and mildew-proof particle board, Features: The particleboard is made of straw raw material, modified soybean meal adhesive, waterproofing agent and wetting agent; The modified soybean meal adhesive is made of soybean meal powder, urea, lithium bromide, distilled water, acetic acid propylene emulsion and MDI curing agent; The waterproofing agent is paraffin emulsion, and the wetting agent is calcium chloride solution.

2. A waterproof and mildew-proof particle board according to claim 1, Features: The mass ratio of the soybean meal powder, urea, lithium bromide and distilled water is 8-10:7-8:0.1-0.15:40-45.

3. A waterproof and mildew-proof particle board according to claim 1, Features: The mass ratio of the acetic acid acrylic emulsion to the MDI curing agent is 8-9:7-8.

4. A method for processing a waterproof and mildew-proof particleboard, according to the waterproof and mildew-proof particleboard according to any one of claims 1 to 3, It is characterized in that The processing method comprises the following steps: S1. preparing modified soybean meal adhesive; S2, pretreatment of straw raw materials; S3, pressed low density straw particle board.

5. A method for processing a waterproof and mildew-proof particle board according to claim 4, It is characterized in that The specific steps of S1 are as follows: S101, add 10 parts of soybean meal, 7-8 parts of urea, 0.1 parts of lithium bromide, and 40-45 parts of distilled water into a flask, fix the flask in a 30°C constant temperature water bath, turn on an electric stirrer and stir for 30-40 minutes; S102, then add 85-90 parts of acetic acid propylene emulsion and stir for 8-10 minutes, then add 7-8 parts of MDI curing agent and stir for 5-8 minutes to prepare modified soybean meal adhesive.

6. A method for processing a waterproof and mildew-proof particle board according to claim 4, It is characterized in that The specific steps of S2 are as follows: S201, crushing straw raw materials to obtain straw crushed materials with a particle size of 3-4 mm, adding them into a beaker, and preparing 20% ​​calcium chloride solution, adding it into the beaker, and soaking for 20-24 hours; S202, then take out the straw chips and put them into a forced air drying oven at a temperature of 80-85°C and dry them for 4-5 hours.

7. A method for processing a waterproof and mildew-proof particle board according to claim 4, It is characterized in that The specific steps of S3 are as follows: S301, adding modified soybean meal adhesive to the pretreated straw fragments, stirring for 5-8 minutes, then pouring in the waterproofing agent paraffin emulsion and stirring again for 3-5 minutes; S302, applying paraffin wax on one side of two carrier plates, and placing a mixture of straw chips and modified soybean meal adhesive for hot pressing; S303. After hot pressing, take out the board and place it in a cool place for 72 hours to complete the processing of the waterproof and mildew-proof particle board.

8. A method for processing a waterproof and mildew-proof particle board according to claim 7, Features: In the S302, the waterproofing agent accounts for 5-15% of the particleboard mass, and the amount of the modified soybean meal adhesive applied is 28-30%.

9. A method for processing a waterproof and mildew-proof particle board according to claim 7, Features: In the hot pressing treatment, the hot pressing pressure is 1.2-1.4 MPa, the hot pressing time is 1200-1500 s, and the hot pressing temperature is 170-180°C.