Manufacturing method of novel water-based anti-corrosion material

By combining nano zinc oxide and ring (tyrosine-proline) in water-based anticorrosion new materials, the existing anticorrosion new materials have short service life and poor antibacterial properties in marine environments. Problem, significantly improving salt spray corrosion resistance and antibacterial properties, extending service life and avoiding marine pollution.

CN118994950AInactive Publication Date: 2024-11-22XIAN RONGSEN PAINT IND
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411318051.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-20
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing water-based anticorrosion new materials have short service life in marine environments, the paint film is prone to fall off, the antibacterial and stable performance are poor, and the marine environment is polluted.

Method used

Using a combination of nano zinc oxide and ring (tyrosine-proline), nano zinc oxide dispersion is prepared by sonication, and mixed it multiple times in a water-based anticorrosion new material to adjust flexibility, viscosity and gloss. and wettability, forming a dense protective layer and an antibacterial barrier.

Benefits of technology

It significantly improves the salt spray corrosion resistance and antibacterial ability of new water-based anticorrosion materials, extends the service life, avoids marine pollution, and provides the dual effects of physical barriers and chemical protection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118994950A_ABST
    Figure CN118994950A_ABST
Patent Text Reader

Abstract

The invention provides a manufacturing method of a novel water-based anti-corrosion material. The manufacturing method comprises the following steps: S1, material preparation: preparing 30 to 50 parts of inorganic resin, 20 to 30 parts of deionized water, 5 to 10 parts of nano zinc oxide, 5 to 10 parts of cyclo (tyrosine-proline), 0.5 to 2 parts of 3-aminopropyltrimethoxysilane, 1 to 3 parts of triphenyl phosphate and 0.5 to 1 part of Tinuvin 400; the invention discloses a high-temperature-resistant coating which is prepared from the following components in parts by weight: 2-3 parts of polyether modified dimethyl oxane, 1-3 parts of polydimethylsiloxane, 1-2 parts of sodium polyacrylate, 0.5-1 part of carboxymethyl cellulose, 2-3 parts of fumed silica, 5-10 parts of polyethylene glycol-400 and 1-2 parts of methyl cellulose. S2, preparing a nano zinc oxide dispersion liquid; S3, preparing a resin base material; S4, performing mixing; s9, adjusting the pH value; s10, removing impurities; the prepared water-based anti-corrosion new material is stable in performance and high in anti-corrosion capacity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of new antifouling materials, and specifically relates to a method for manufacturing a new water-based anticorrosive material. Background Art

[0002] Equipment used in the ocean, such as ships and drilling platforms, often have new water-based anti-corrosion materials coated on the surface. Toxic substances such as cuprous oxide and pesticides are often added to the new water-based anti-corrosion materials to make them resistant to sewage. This type of anti-sewage anti-corrosion material has a short service life (one year) and the paint film is easily lost in the ocean, polluting the marine environment.

[0003] The patent document with authorization (announcement) number CN112521783B discloses a new anti-fouling and anti-corrosion marine water-based anti-corrosion material, which is a mixture of polymerized o-p-methylaniline, polytrifluorochloroethylene, aldehyde-ketone resin, alkyl succinic acid imide, eucalyptus oil, azadirachtin, dicyclopentenyloxyethyl acrylate, hydroxypropyl methylcellulose, coumarone-indene resin and water-based chlorinated rubber in a mass ratio of 7-19:4.6-5.8:7.7-9.4:8-11.2:6-14:9-16:6-8:4-6:4-6:2.7-6.1.

[0004] However, in the above scheme, the antibacterial and stability performance of the new water-based anticorrosion material is still poor, and the paint film is easy to fall off in the ocean, polluting the marine environment. In view of this, a method for manufacturing a new water-based anticorrosion material is urgently needed. Summary of the invention

[0005] In order to solve the above technical problems, the present invention discloses a method for manufacturing a new water-based anticorrosive material, comprising the following steps:

[0006] S1. Material preparation: 30-50 parts of inorganic resin, 20-30 parts of deionized water, 5-10 parts of nano zinc oxide, 5-10 parts of cyclo(tyrosine-proline), 0.5-2 parts of 3-aminopropyltrimethoxysilane, 1-3 parts of triphenyl phosphate, 0.5-1 parts of Tinuvin 400, 2-3 parts of polyether-modified dimethyl oxane, 1-3 parts of polydimethylsiloxane, 1-2 parts of sodium polyacrylate, 0.5-1 parts of carboxymethyl cellulose, 2-3 parts of fumed silica, 5-10 parts of polyethylene glycol-400, 1-2 parts of methyl cellulose;

[0007] S2, preparation of nano zinc oxide dispersion: taking the nano zinc oxide described in step S1 and 1 / 2 of sodium polyacrylate, using sodium polyacrylate as a dispersant and water as a solvent, and mixing and dispersing the nano zinc oxide through ultrasonic treatment to obtain a nano zinc oxide dispersion;

[0008] S3, preparation of resin base material: mixing an inorganic resin and deionized water, and heating under stirring conditions to fully dissolve the resin to obtain a resin base material;

[0009] S4, primary mixing: adding the nano zinc oxide dispersion and cyclo(tyrosine-proline) to the resin base prepared in step S3, and uniformly dispersing them under stirring to obtain a mixed slurry 1;

[0010] S5, secondary mixing: after the mixed slurry 1 prepared in step S4 is allowed to stand for 5-10 minutes, 3-aminopropyltrimethoxysilane, triphenyl phosphate and Tinuvin 400 are added to the mixed slurry 1 in sequence, and stirring is continued until the mixed slurry is uniformly dispersed to obtain a mixed slurry 2;

[0011] S6, three-time mixing: under stirring, adding polyether-modified dimethyl oxane and polydimethylsiloxane to the mixed slurry 2 prepared in S5 in sequence, and continuing to stir until uniformly dispersed, so as to adjust the flexibility and water resistance of the new water-based anticorrosive material; obtaining a mixed slurry 3;

[0012] S7, mixing for the fourth time: adding the remaining sodium polyacrylate and carboxymethyl cellulose to the mixed slurry three prepared in step S6 under stirring, continuing to stir until uniformly dispersed, adjusting the viscosity and stability of the new water-based antiseptic material, and obtaining a mixed slurry four;

[0013] S8, fifth mixing: adding fumed silica, polyethylene glycol-400 and methylcellulose to the mixed slurry 4 prepared in step S7 under stirring, continuing to stir until uniformly dispersed, adjusting the glossiness, wettability and consistency of the new water-based antiseptic material, and obtaining a mixed slurry 5;

[0014] S9, adjusting pH: under stirring, adding acetic acid to the mixed slurry 5 to adjust the pH value of the slurry to between 7.0 and 8.5, to obtain a rough material of the water-based anticorrosive new material;

[0015] S10, impurity removal: remove impurities by filtering to obtain a finished product of the new water-based anticorrosive material.

[0016] Preferably, in step S1, the prepared materials are: 30 parts of inorganic resin, 20 parts of deionized water, 5 parts of nano zinc oxide, 5 parts of cyclo(tyrosine-proline), 0.5 parts of 3-aminopropyltrimethoxysilane, 1 part of triphenyl phosphate, 0.5 parts of Tinuvin400, 2 parts of polyether-modified dimethyl oxane, 1 part of polydimethylsiloxane, 1 part of sodium polyacrylate, 0.5 parts of carboxymethyl cellulose, 2 parts of fumed silica, 5 parts of polyethylene glycol-400, and 1 part of methyl cellulose.

[0017] Preferably, in step S1, the prepared materials are: 50 parts of inorganic resin, 30 parts of deionized water, 10 parts of nano zinc oxide, 10 parts of cyclo(tyrosine-proline), 2 parts of 3-aminopropyltrimethoxysilane, 3 parts of triphenyl phosphate, 1 part of Tinuvin400, 3 parts of polyether-modified dimethyl oxane, 3 parts of polydimethylsiloxane, 2 parts of sodium polyacrylate, 1 part of carboxymethyl cellulose, 3 parts of fumed silica, 10 parts of polyethylene glycol-400, and 2 parts of methyl cellulose.

[0018] Preferably, in step S1, the prepared materials are: 40 parts of inorganic resin, 25 parts of deionized water, 8 parts of nano zinc oxide, 8 parts of cyclo(tyrosine-proline), 1 part of 3-aminopropyltrimethoxysilane, 2 parts of triphenyl phosphate, 0.8 parts of Tinuvin 400, 2.5 parts of polyether-modified dimethyl oxane, 2 parts of polydimethylsiloxane, 1.5 parts of sodium polyacrylate, 0.8 parts of carboxymethyl cellulose, 2.5 parts of fumed silica, 8 parts of polyethylene glycol-400, and 1.5 parts of methyl cellulose.

[0019] Preferably, in step S2, when preparing the nano zinc oxide dispersion, the frequency of ultrasonic treatment is 30-35 kHz, and the treatment time is 15-20 min.

[0020] Preferably, in step S2, when preparing the nano zinc oxide dispersion, the material-liquid ratio is 1:8-10.

[0021] Preferably, in step S3, when preparing the resin base material: heating to 50° C.-60° C. to fully dissolve the resin to obtain the resin base material.

[0022] On the other hand, the present invention discloses a new water-based anti-corrosion material prepared by the above method for manufacturing the new water-based anti-corrosion material.

[0023] On the other hand, the present invention discloses the application of the above new water-based anti-corrosion material to equipment used in the ocean, such as ships, drilling platforms, etc.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] 1. The present invention provides a method for manufacturing a new water-based anti-corrosion material. The new water-based anti-corrosion material prepared by the technical solution of the present invention has stable performance and strong anti-corrosion ability, which prolongs the service life of the new water-based anti-corrosion material. Moreover, the present invention uses natural antibacterial agents to improve performance and does not pollute the ocean.

[0026] 2. The present invention adopts a combination of nano zinc oxide and cyclo(tyrosine-proline) to significantly improve the salt spray corrosion resistance of the new water-based anticorrosion material, and the two produce a synergistic effect, which may be because: the dense protective layer formed by nano zinc oxide is combined with the coating adhesion enhanced by cyclo(tyrosine-proline), providing the coating with a dual effect of physical barrier and chemical protection; the joint use of cyclo(tyrosine-proline) and nano zinc oxide dispersion can also synergistically enhance the antibacterial ability of the new water-based anticorrosion material, which may be because: the photocatalytic bactericidal effect of nano zinc oxide is combined with the antibacterial effect of the natural antibacterial agent cyclo(tyrosine-proline), which may form a stronger antibacterial barrier, and it may also be because the high specific surface area and nano effect of nano zinc oxide can increase the contact area with bacteria and increase the release rate of zinc ions.

[0027] 3. The present invention disperses nano zinc oxide and then ultrasonically treats it to obtain a nano zinc oxide dispersion, which avoids the agglomeration of nano particles, improves the uniformity of nano zinc oxide in the new water-based anticorrosion material, and ensures the quality stability of the new water-based anticorrosion material; moreover, the nano particles in the nano zinc oxide dispersion have excellent ultraviolet absorption and scattering capabilities, can more effectively shield ultraviolet rays, and protect the substrate under the new water-based anticorrosion material from damage by ultraviolet rays; at the same time, nano zinc oxide itself has antibacterial properties, and the form of the dispersion allows the antibacterial properties to be fully exerted in the new water-based anticorrosion material, thereby improving the antibacterial and mildew-proof capabilities of the new water-based anticorrosion material. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 The present invention is a flow chart of the method for manufacturing the new water-based anticorrosive material. DETAILED DESCRIPTION

[0029] Embodiment 1: This embodiment provides a method for manufacturing a new water-based anticorrosive material, comprising the following steps:

[0030] S1. Material preparation: 30 parts of inorganic resin, 20 parts of deionized water, 5 parts of nano zinc oxide, 5 parts of cyclo(tyrosine-proline), 0.5 parts of 3-aminopropyltrimethoxysilane, 1 part of triphenyl phosphate, 0.5 parts of Tinuvin 400, 2 parts of polyether-modified dimethyl oxane, 1 part of polydimethylsiloxane, 1 part of sodium polyacrylate, 0.5 parts of carboxymethyl cellulose, 2 parts of fumed silica, 5 parts of polyethylene glycol-400, and 1 part of methyl cellulose;

[0031] S2, preparation of nano zinc oxide dispersion: taking the nano zinc oxide described in step S1 and 1 / 2 of sodium polyacrylate, using sodium polyacrylate as a dispersant and water as a solvent, and mixing and dispersing the nano zinc oxide through ultrasonic treatment to obtain a nano zinc oxide dispersion;

[0032] S3, preparation of resin base material: mixing an inorganic resin and deionized water, and heating under stirring conditions to fully dissolve the resin to obtain a resin base material;

[0033] S4, primary mixing: adding the nano zinc oxide dispersion and cyclo(tyrosine-proline) to the resin base prepared in step S3, and uniformly dispersing them under stirring to obtain a mixed slurry 1;

[0034] S5, secondary mixing: after the mixed slurry 1 prepared in step S4 is allowed to stand for 5 minutes, 3-aminopropyltrimethoxysilane, triphenyl phosphate and Tinuvin 400 are added to the mixed slurry 1 in sequence, and stirring is continued until the mixed slurry is uniformly dispersed to obtain a mixed slurry 2;

[0035] S6, three-time mixing: under stirring, adding polyether-modified dimethyl oxane and polydimethylsiloxane to the mixed slurry 2 prepared in S5 in sequence, and continuing to stir until the mixture is evenly dispersed to obtain a mixed slurry 3;

[0036] S7, mixing for the fourth time: adding the remaining sodium polyacrylate and carboxymethyl cellulose to the mixed slurry three prepared in step S6 under stirring, and continuing to stir until the mixture is evenly dispersed to obtain mixed slurry four;

[0037] S8, fifth mixing: adding fumed silica, polyethylene glycol-400 and methylcellulose to the mixed slurry 4 prepared in step S7 under stirring, and continuing to stir until the mixture is evenly dispersed to obtain a mixed slurry 5;

[0038] S9, adjusting pH: under stirring, adding acetic acid to the mixed slurry 5 to adjust the pH value of the slurry to between 7.0, to obtain a rough material of the water-based anticorrosive new material;

[0039] S10, impurity removal: remove impurities by filtering to obtain a finished product of a new water-based anticorrosive material. The preparation process is shown in Figure 1 .

[0040] Moreover, in the step S2, when preparing the nano zinc oxide dispersion, the frequency of the ultrasonic treatment is 30 kHz and the treatment is 15 minutes.

[0041] Moreover, in the step S2, when the nano zinc oxide dispersion is prepared, the material-liquid ratio is 1:8.

[0042] Furthermore, in the step S3, when preparing the resin base material: heating to 50° C. to fully dissolve the resin, thereby obtaining the resin base material.

[0043] Embodiment 2: This embodiment provides a method for manufacturing a new water-based anticorrosive material, comprising the following steps:

[0044] S1. Material preparation: 50 parts of inorganic resin, 30 parts of deionized water, 10 parts of nano zinc oxide, 10 parts of cyclo(tyrosine-proline), 2 parts of 3-aminopropyltrimethoxysilane, 3 parts of triphenyl phosphate, 1 part of Tinuvin 400, 3 parts of polyether-modified dimethyl oxane, 3 parts of polydimethylsiloxane, 2 parts of sodium polyacrylate, 1 part of carboxymethyl cellulose, 3 parts of fumed silica, 10 parts of polyethylene glycol-400, and 2 parts of methyl cellulose;

[0045] S2, preparation of nano zinc oxide dispersion: taking the nano zinc oxide described in step S1 and 1 / 2 of sodium polyacrylate, using sodium polyacrylate as a dispersant and water as a solvent, and mixing and dispersing the nano zinc oxide through ultrasonic treatment to obtain a nano zinc oxide dispersion;

[0046] S3, preparation of resin base material: mixing an inorganic resin and deionized water, and heating under stirring conditions to fully dissolve the resin to obtain a resin base material;

[0047] S4, primary mixing: adding the nano zinc oxide dispersion and cyclo(tyrosine-proline) to the resin base prepared in step S3, and uniformly dispersing them under stirring to obtain a mixed slurry 1;

[0048] S5, secondary mixing: after the mixed slurry 1 prepared in step S4 is allowed to stand for 10 minutes, 3-aminopropyltrimethoxysilane, triphenyl phosphate and Tinuvin 400 are added to the mixed slurry 1 in sequence, and stirring is continued until the mixed slurry is uniformly dispersed to obtain a mixed slurry 2;

[0049] S6, three-time mixing: under stirring, adding polyether-modified dimethyl oxane and polydimethylsiloxane to the mixed slurry 2 prepared in S5 in sequence, and continuing to stir until the mixture is evenly dispersed to obtain a mixed slurry 3;

[0050] S7, mixing for the fourth time: adding the remaining sodium polyacrylate and carboxymethyl cellulose to the mixed slurry three prepared in step S6 under stirring, and continuing to stir until the mixture is evenly dispersed to obtain mixed slurry four;

[0051] S8, fifth mixing: adding fumed silica, polyethylene glycol-400 and methylcellulose to the mixed slurry 4 prepared in step S7 under stirring, and continuing to stir until the mixture is evenly dispersed to obtain a mixed slurry 5;

[0052] S9, adjusting pH: under stirring, adding acetic acid to the mixed slurry 5 to adjust the pH value of the slurry to between 7.0 and 8.5, to obtain a rough material of the water-based anticorrosive new material;

[0053] S10, impurity removal: remove impurities by filtering to obtain a finished product of the new water-based anticorrosive material.

[0054] Moreover, in the step S2, when preparing the nano zinc oxide dispersion, the frequency of the ultrasonic treatment is 35 kHz and the treatment is performed for 20 minutes.

[0055] Moreover, in the step S2, when the nano zinc oxide dispersion is prepared, the material-liquid ratio is 1:10.

[0056] Furthermore, in the step S3, when preparing the resin base material: heating to 60° C. to fully dissolve the resin, thereby obtaining the resin base material.

[0057] Embodiment 3: This embodiment provides a method for manufacturing a new water-based anticorrosive material, comprising the following steps:

[0058] S1. Material preparation: 40 parts of inorganic resin, 25 parts of deionized water, 8 parts of nano zinc oxide, 8 parts of cyclo(tyrosine-proline), 1 part of 3-aminopropyltrimethoxysilane, 2 parts of triphenyl phosphate, 0.8 parts of Tinuvin 400, 2.5 parts of polyether-modified dimethyl oxane, 2 parts of polydimethylsiloxane, 1.5 parts of sodium polyacrylate, 0.8 parts of carboxymethyl cellulose, 2.5 parts of fumed silica, 8 parts of polyethylene glycol-400, and 1.5 parts of methyl cellulose;

[0059] S2, preparation of nano zinc oxide dispersion: taking the nano zinc oxide described in step S1 and 1 / 2 of sodium polyacrylate, using sodium polyacrylate as a dispersant and water as a solvent, and mixing and dispersing the nano zinc oxide through ultrasonic treatment to obtain a nano zinc oxide dispersion;

[0060] S3, preparation of resin base material: mixing an inorganic resin and deionized water, and heating under stirring conditions to fully dissolve the resin to obtain a resin base material;

[0061] S4, primary mixing: adding the nano zinc oxide dispersion and cyclo(tyrosine-proline) to the resin base prepared in step S3, and uniformly dispersing them under stirring to obtain a mixed slurry 1;

[0062] S5, secondary mixing: after the mixed slurry 1 prepared in step S4 is allowed to stand for 8 minutes, 3-aminopropyltrimethoxysilane, triphenyl phosphate and Tinuvin 400 are added to the mixed slurry 1 in sequence, and stirring is continued until the mixed slurry is uniformly dispersed to obtain a mixed slurry 2;

[0063] S6, three-time mixing: under stirring, adding polyether-modified dimethyl oxane and polydimethylsiloxane to the mixed slurry 2 prepared in S5 in sequence, and continuing to stir until the mixture is evenly dispersed to obtain a mixed slurry 3;

[0064] S7, mixing for the fourth time: adding the remaining sodium polyacrylate and carboxymethyl cellulose to the mixed slurry three prepared in step S6 under stirring, and continuing to stir until the mixture is evenly dispersed to obtain mixed slurry four;

[0065] S8, fifth mixing: adding fumed silica, polyethylene glycol-400 and methylcellulose to the mixed slurry 4 prepared in step S7 under stirring, and continuing to stir until the mixture is evenly dispersed to obtain a mixed slurry 5;

[0066] S9, adjusting pH: under stirring, adding acetic acid to the mixed slurry 5 to adjust the pH value of the slurry to between 7.0 and 8.5, to obtain a rough material of the water-based anticorrosive new material;

[0067] S10, impurity removal: remove impurities by filtering to obtain a finished product of the new water-based anticorrosive material.

[0068] Moreover, in the step S2, when preparing the nano zinc oxide dispersion, the frequency of the ultrasonic treatment is 30-35 kHz, and the treatment lasts for 18 minutes.

[0069] Moreover, in the step S2, when the nano zinc oxide dispersion is prepared, the material-liquid ratio is 1:9.

[0070] Furthermore, in the step S3, when preparing the resin base material: heating to 55° C. to fully dissolve the resin, thereby obtaining the resin base material.

[0071] Example 4: The new water-based anti-corrosion material prepared in Example 3 is used in marine equipment, specifically ships and drilling platforms.

[0072] Before painting, the surface of the marine equipment is thoroughly cleaned to remove oil, impurities and rust, and the surface is roughened by sandblasting, shot blasting and other methods to improve the adhesion of the coating. The new water-based anti-corrosion material prepared by the present invention is applied to the surface of the marine equipment.

[0073] Comparative Example 1

[0074] The difference between this comparative example and Example 3 is that no ring (tyrosine-proline) is added.

[0075] Comparative Example 2

[0076] The difference between this comparative example and Example 3 is that no nano zinc oxide is added.

[0077] Comparative Example 3

[0078] The difference between this comparative example and Example 3 is that nano zinc oxide and cyclo(tyrosine-proline) are not added.

[0079] Comparative Example 4

[0080] The difference between this comparative example and Example 3 is that: no dispersion of nano zinc oxide is prepared, and nano zinc oxide solid is directly added.

[0081] Comparative Example 5

[0082] The difference between this comparative example and Example 3 is that 2 parts of nano zinc oxide and 15 parts of cyclo(tyrosine-proline) are taken.

[0083] Comparative Example 6

[0084] The difference between this comparative example and Example 3 is that 15 parts of nano zinc oxide and 2 parts of cyclo(tyrosine-proline) are taken.

[0085] Experimental Section

[0086] Experiment 1: Salt spray test

[0087] A paint film sample was prepared using the new water-based anticorrosive materials of Examples 1-3 and Comparative Examples 1-6. After the edges and backs were sealed with a 1:1 mixture of paraffin and rosin, the above 9 paint film samples were placed in a salt spray test box at an angle of 30-45 degrees, sprayed with 5% salt water, and the temperature in the box was controlled to be 37°C, the humidity was 95%, and the pH value of the solution was 6.5-7.2. The samples were taken out every 24 hours and observed for surface defects. The test was stopped after 720 hours. The time when defects began to appear on the surface of the above samples was counted, as shown in Table 1.

[0088] Table 1 Salt spray test results

[0089]

[0090]

[0091] It can be seen from Table 1 that the new water-based anti-corrosion material prepared by the present invention has strong salt spray corrosion resistance, while comparative examples 1-6 are poor.

[0092] Using nano zinc oxide dispersion alone can improve the salt spray corrosion resistance of new water-based anti-corrosion materials. This may be because: nano zinc oxide can increase the cross-linking density of the coating, which helps to form a denser and stronger coating structure. This structure can more effectively block the penetration of corrosive media such as salt spray, thereby improving the corrosion resistance of the coating; it may also be because nano zinc oxide has adsorption and surface activity, which can significantly improve the barrier properties of the coating and effectively reduce the erosion of corrosive substances such as chloride ions in salt spray on the coating and substrate, thereby extending the service life of the coating.

[0093] Using cyclo(tyrosine-proline) alone can also improve the salt spray corrosion resistance of new water-based anti-corrosion materials to varying degrees. This may be because: cyclo(tyrosine-proline) itself has anti-corrosion properties; it may also be because cyclo(tyrosine-proline) can improve the density of the coating and improve the corrosion resistance of new water-based anti-corrosion materials.

[0094] The use of cyclo(tyrosine-proline) and nano zinc oxide dispersion in the ratio of the present invention can significantly improve the salt spray corrosion resistance of the new water-based anticorrosive material to produce a synergistic effect, and the change in the ratio of the two will also affect its performance. This may be because: when the cyclo(tyrosine-proline) and nano zinc oxide dispersion in the ratio of the present invention are used, the dense protective layer formed by the nano zinc oxide is combined with the coating adhesion enhanced by the cyclo(tyrosine-proline), providing the coating with a dual effect of physical barrier and chemical protection.

[0095] Nano zinc oxide dispersion has a better effect than nano zinc oxide. This may be because: Nano zinc oxide dispersion avoids the agglomeration of nanoparticles, improves the uniformity of nano zinc oxide in the new water-based anticorrosion material, and ensures the stability of the quality of the new water-based anticorrosion material;

[0096] Experiment 2 Bacterial attachment experiment

[0097] The nine paint film samples prepared in Experiment 1 were sterilized to prevent initial contamination, and then suspended and immersed in a beaker filled with fresh seawater to ensure that the paint film samples were completely immersed in the seawater. The light, temperature, and salinity were controlled to simulate the actual marine environment.

[0098] After 7 days, the coated samples were removed and the surfaces were rinsed with sterile seawater to remove non-resident organisms. The bacterial attachment on the paint film samples was counted (the number of bacterial attachments was rounded to an integer), as shown in Table 2.

[0099] Table 2 Bacterial adhesion test results

[0100]

[0101]

[0102] It can be seen from Table 2 that the number of bacteria attached to the paint film sample prepared by the technical solution of the present invention is only 40-45 CFU / cm 2 , the number of bacteria attached is small, the distribution is sparse, and the shape is irregular, while the amount of bacteria attached in comparative examples 1-6 is large, forming a layer of biofilm.

[0103] Comparative Example 1 did not add cyclo(tyrosine-proline), Comparative Example 2 did not add nano zinc oxide, and Comparative Example 3 did not add nano zinc oxide and cyclo(tyrosine-proline). The number of bacteria attached was 480 CFU / cm 2 、500CFU / cm 2 、800CFU / cm 2 In contrast, in Examples 5-6, the change in the ratio of cyclo(tyrosine-proline) and nano zinc oxide will eventually affect the antibacterial properties of the new water-based antiseptic material, with the number of bacteria attached being 170 CFU / cm2 、180CFU / cm 2 ; It can be proved that: the use of nano zinc oxide / cyclo (tyrosine-proline) alone can enhance the antibacterial ability of the sample, but when the two are combined in the ratio of the present invention, the effect is significantly enhanced. The joint use of nano zinc oxide and cyclo (tyrosine-proline) synergistically enhances the antibacterial ability of the paint film sample. This may be because: under the preparation ratio of the present invention, the photocatalytic bactericidal effect of nano zinc oxide is combined with the antibacterial effect of the natural antibacterial agent cyclo (tyrosine-proline), which may form a stronger antibacterial barrier and effectively inhibit the attachment and growth of various marine organisms; it may also be because the high specific surface area and nano effect of nano zinc oxide can increase the contact area with bacteria and increase the release rate of zinc ions.

[0104] In Comparative Example 4, since nano zinc oxide solid was directly used without preparing dispersion liquid of nano zinc oxide, the antibacterial property of the new water-based antiseptic material was also affected. The number of bacteria attached was 400 CFU / cm 2 This may be because: nano zinc oxide itself has antibacterial properties, and the dispersion form allows this antibacterial property to be fully utilized in the new water-based anti-corrosion material, thereby improving the antibacterial and anti-mildew ability of the new water-based anti-corrosion material.

Claims

1. A method for manufacturing a new water-based anticorrosive material. It is characterized in that The steps include: S1. Material preparation: 30-50 parts of inorganic resin, 20-30 parts of deionized water, 5-10 parts of nano zinc oxide, 5-10 parts of cyclo(tyrosine-proline), 0.5-2 parts of 3-aminopropyltrimethoxysilane, 1-3 parts of triphenyl phosphate, 0.5-1 parts of Tinuvin 400, 2-3 parts of polyether-modified dimethyl oxane, 1-3 parts of polydimethylsiloxane, 1-2 parts of sodium polyacrylate, 0.5-1 parts of carboxymethyl cellulose, 2-3 parts of fumed silica, 5-10 parts of polyethylene glycol-400, 1-2 parts of methyl cellulose; S2, preparation of nano zinc oxide dispersion: taking the nano zinc oxide described in step S1 and 1 / 2 of sodium polyacrylate, using sodium polyacrylate as a dispersant and water as a solvent, mixing and dispersing the nano zinc oxide by ultrasonic treatment to obtain a nano zinc oxide dispersion; S3, preparation of resin base material: mixing an inorganic resin and deionized water, and heating under stirring conditions to fully dissolve the resin to obtain a resin base material; S4, primary mixing: adding the nano zinc oxide dispersion and cyclo(tyrosine-proline) to the resin base prepared in step S3, and uniformly dispersing them under stirring to obtain a mixed slurry 1; S5, secondary mixing: after the mixed slurry 1 prepared in step S4 is allowed to stand for 5-10 minutes, 3-aminopropyltrimethoxysilane, triphenyl phosphate and Tinuvin 400 are added in sequence, and stirring is continued until the mixture is uniformly dispersed to obtain mixed slurry 2; S6, three-time mixing: under stirring, adding polyether-modified dimethyl oxane and polydimethylsiloxane to the mixed slurry 2 prepared in S5 in sequence, and continuing to stir until the mixture is evenly dispersed to obtain a mixed slurry 3; S7, mixing for the fourth time: adding the remaining sodium polyacrylate and carboxymethyl cellulose to the mixed slurry three prepared in step S6 under stirring, and continuing to stir until the mixture is evenly dispersed to obtain mixed slurry four; S8, fifth mixing: adding fumed silica, polyethylene glycol-400 and methylcellulose to the mixed slurry 4 prepared in step S7 under stirring, and continuing to stir until the mixture is evenly dispersed to obtain a mixed slurry 5; S9, adjusting pH: under stirring, adding acetic acid to the mixed slurry 5 to adjust the pH value to between 7.0 and 8.5 to obtain a rough material of the water-based anticorrosive new material; S10, impurity removal: remove impurities by filtering to obtain a finished product of the new water-based anticorrosive material.

2. A method for producing a new water-based anticorrosive material as claimed in claim 1, It is characterized in that In the step S1, the prepared materials are: 30 parts of inorganic resin, 20 parts of deionized water, 5 parts of nano zinc oxide, 5 parts of cyclo(tyrosine-proline), 0.5 parts of 3-aminopropyltrimethoxysilane, 1 part of triphenyl phosphate, 0.5 parts of Tinuvin 400, 2 parts of polyether-modified dimethyl oxane, 1 part of polydimethylsiloxane, 1 part of sodium polyacrylate, 0.5 parts of carboxymethyl cellulose, 2 parts of fumed silica, 5 parts of polyethylene glycol-400, and 1 part of methyl cellulose.

3. A method for producing a new water-based anticorrosive material as claimed in claim 1, It is characterized in that In the step S1, the prepared materials are: 50 parts of inorganic resin, 30 parts of deionized water, 10 parts of nano zinc oxide, 10 parts of cyclo(tyrosine-proline), 2 parts of 3-aminopropyltrimethoxysilane, 3 parts of triphenyl phosphate, 1 part of Tinuvin 400, 3 parts of polyether-modified dimethyl oxane, 3 parts of polydimethylsiloxane, 2 parts of sodium polyacrylate, 1 part of carboxymethyl cellulose, 3 parts of fumed silica, 10 parts of polyethylene glycol-400, and 2 parts of methyl cellulose.

4. A method for producing a new water-based anticorrosive material as claimed in claim 1, It is characterized in that In the step S1, the prepared materials are: 40 parts of inorganic resin, 25 parts of deionized water, 8 parts of nano zinc oxide, 8 parts of cyclo(tyrosine-proline), 1 part of 3-aminopropyltrimethoxysilane, 2 parts of triphenyl phosphate, 0.8 parts of Tinuvin 400, 2.5 parts of polyether-modified dimethyl oxane, 2 parts of polydimethylsiloxane, 1.5 parts of sodium polyacrylate, 0.8 parts of carboxymethyl cellulose, 2.5 parts of fumed silica, 8 parts of polyethylene glycol-400, and 1.5 parts of methyl cellulose.

5. A method for producing a new water-based anticorrosive material as claimed in claim 1, It is characterized in that, In the step S2, when preparing the nano zinc oxide dispersion, the frequency of ultrasonic treatment is 30-35 kHz and the treatment time is 15-20 min.

6. A method for producing a new water-based anticorrosive material as claimed in claim 1, It is characterized in that, In the step S2, when the nano zinc oxide dispersion is prepared, the material-liquid ratio is 1:8-10.

7. A method for producing a new water-based anticorrosive material as claimed in claim 1, It is characterized in that, In the step S3, when preparing the resin base material: heating to 50° C.-60° C. to fully dissolve the resin to obtain the resin base material.

8. A new water-based anti-corrosion material prepared by the method for producing a new water-based anti-corrosion material as described in any one of claims 1 to 7.

9. Application of the new water-based anticorrosive material as claimed in claim 8, It is characterized in that Equipment for use in the ocean.

10. Use of the new water-based anticorrosive material as claimed in claim 9, It is characterized in that The device is a ship or a drilling platform.

Citation Information

Patent Citations

  • Nontoxic antifouling paint for oceanographic ship and facilities and method for preparing paint

    CN101967316A

  • Water-based UV anti-corrosive coating and preparation method thereof

    CN108912886A

  • Water-based inorganic mould-proof coating and preparation method thereof

    CN109135358A

  • Acid-resistant and alkali-resistant water-based metal coating for engineering mechanical equipment