Preparation method of magnetic photonic crystal film and application of magnetic photonic crystal film in visual detection of heavy metal Ni < 2 + >
Through the preparation of magnetophoton crystal thin films, the combination of magnetic nanoparticles and thiourea-containing functional copolymers is used to achieve high sensitivity and visual detection of heavy metal ion Ni2+, and solve the problems of high detection cost and complex operation in the prior art. , provides a low-cost and simple detection method.
Patent Information
- Application Number
- CN202411255145.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-09
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-09-09
AI Technical Summary
In the prior art, the detection of heavy metal ion Ni2+ relies on large precision instruments, resulting in high detection cost, complex operation and poor universality, and lack of low-cost, convenient detection methods without large-scale equipment.
The preparation method of magnetophoton crystal film is adopted to prepare Fe3O4 magnetic nanoparticles by solvothermal method, and the multi-layer magnetophoton crystal film is prepared by spin coating method under the combination of silicon oxide core-shell structure and sulfhydrourea-containing functional copolymer. , the nanoparticles are arranged in an orderly manner under the action of magnetic fields to achieve high sensitivity and visual detection of Ni2+.
A low-cost and simple Ni2+ detection method is realized. Through visual inspection of color changes, it has high sensitivity and low detection cost. It does not rely on large equipment. It can quickly and accurately determine whether the Ni2+ concentration exceeds the standard.
Smart Images

Figure CN118994993A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of magnetic assembly nanomaterial photonic crystal film and heavy metal ion detection, and specifically relates to a preparation method of a magnetic photonic crystal film and a method for visually detecting heavy metal Ni 2+ Purpose. Background Art
[0002] Heavy metal ion Ni 2+ Pollution can seriously harm the environment. 2+ Excessive accumulation in the environment can cause contact dermatitis, damage the digestive system, irritate the respiratory system, lead to neurasthenia and even cause cancer. 2+ The concentration can determine the degree of environmental pollution, assess human health risks, monitor environmental pollution sources and governance effects, and provide a scientific basis for the formulation of environmental protection policies and regulations.
[0003] At present, the heavy metal ion Ni 2+ The detection of Ni mainly relies on large precision instruments, which have extremely high accuracy and sensitivity (i.e. very low detection limit), but precision instruments are expensive and require skilled operators to operate the instruments. The detection process requires complex sample preparation. 2+ The detection universality is poor, and there is an urgent need for a low-cost, convenient, intuitive and readable Ni 2+ Detection method.
[0004] Magnetophotonic crystals are composed of two or more materials with different refractive indices arranged periodically. They have wavelength selection function and can selectively allow light of a certain wavelength to pass through while blocking light of other wavelengths. The light that does not pass through is reflected. When the lattice spacing and refractive index of the material are within a certain range, it can reflect light in the visible light region, thereby showing structural color. Thiourea-containing functional copolymers can adsorb Ni 2+ As the chemical structure of the copolymer changes, the functional copolymer layer of the photonic material expands rapidly in water, and the infiltrated Ni 2+ By chelating with the copolymer ligands on the polymer layer, the polymer layer shrinks in volume, which eventually leads to a blue shift in the diffraction wavelength of the photonic structure, which is automatically converted into a visually perceptible color change. Combining the advantages of both, and taking advantage of the conjugated heavy metal ions of the magneto-photonic crystal and the copolymer, the Ni 2+ Highly sensitive, visual and selective detection. Summary of the invention
[0005] The present invention provides a method for preparing a magneto-photonic crystal film and a method for visually detecting heavy metal Ni 2+ The purpose is to detect Ni by magnetoluminescent particles 2+, to reduce the existing Ni 2+ Detection requires reliance on large equipment.
[0006] To this end, the present invention adopts the following technical solutions: A method for preparing a magneto-photonic crystal film comprises the following steps: 1) Obtain or prepare Fe 3 O 4 Magnetic nanoparticles were prepared by solvothermal method; 2) Preparation of silicon oxide core-shell structure magnetic nanoparticles: Fe 3 O 4 Magnetic nanoparticles are mixed with tetraethyl orthosilicate (TEOS), liquid alcohol and concentrated ammonia water in proportion and reacted under ultrasonic conditions to prepare magnetic nanoparticles with a silicon oxide core-shell structure. On the one hand, the silicon oxide coating can stabilize the dispersion in the solution, and on the other hand, as a magneto-photonic crystal material, it has good light reflection effect after orderly arrangement under the action of a magnetic field. 3) Preparation of polymer P (AM-ATU) nanoparticles: AM (acrylamide), ATU (N-allylthiourea), surfactant AOT (sodium docusate), toluene, and AIBN (azobisisobutyronitrile) were mixed successively, and the hot reaction liquid was condensed, refluxed, and stirred. After the reaction, ethanol was used for precipitation to obtain polymer P (AM-ATU) nanoparticles; the copolymer has a high swelling property in water, thus providing Ni 2+ The shrinkage of the polymer layer during handling provides sufficient space; 4) Preparation of magneto-photonic crystal film: Take the polymer P(AM-ATU) nanoparticle dispersion prepared in step 3) and prepare the first film by spin coating; Take the silicon oxide core-shell structure magnetic nanoparticle dispersion prepared in step 2) and prepare a second film layer on top of the first film layer by spin coating; immediately apply a magnetic field after the spin coating is completed, so that the silicon oxide core-shell structure magnetic nanoparticles are orderly arranged under the action of the magnetic field; repeat this step to prepare a total of 2 to 5 layers of film, thereby preparing a magneto-photonic crystal film.
[0007] Furthermore, the silicon oxide core-shell structure magnetic nanoparticles prepared in step 2) have a PDI (aggregation index) < 0.1 and are monodispersed; Further, the mixing reaction steps in step 3) are as follows: 1) Prepare the reaction solution Dissolve AM (acrylamide) and ATU (N-allylthiourea) in a mass ratio of 1:1-5:1 in 1 ml-5 ml of deionized water to form a monomer solution A; Dissolve 5 mg to 15 mg of AIBN (azobisisobutyronitrile) in 1 ml to 5 ml of toluene to form solution B; Dissolve 1 g to 5 g of AOT (docusate sodium) in 50 ml of toluene solution to form solution C; 2) Reaction process Solution C was heated to 50°C-90°C under nitrogen protection and condensation reflux conditions to form a hot reaction liquid; then solution B was added to the hot reaction liquid; finally, solution A was stirred at 0.5 ml·min -1 —2ml·min -1 The mixture is injected into the hot reaction liquid at a rate of and reacted for 0.5h-2h.
[0008] Furthermore, the mass concentration of the polymer P(AM-ATU) nanoparticles prepared in step 3) dispersed in water is 2%-10%.
[0009] Furthermore, the substrate for preparing the magneto-photonic crystal film in step 4) is a silicon wafer having a crystal plane-oriented silicon oxide layer on the surface ( <111> , <100> ).
[0010] Furthermore, the magneto-photonic crystal film prepared in step 4) has 2 to 5 layers, wherein the first layer is a dispersion of polymer P (AM-ATU) nanoparticles, which is used to improve the bonding of the magneto-photonic crystal film; the second layer is a dispersion of silicon oxide core-shell structure magnetic nanoparticles; and the third to fifth layers are analogous in sequence.
[0011] Furthermore, in the preparation of the first layer, the rotation speed of the spin coater is 2000rpm-5000rpm, the time is 20s-80s, and it is dried at 100℃-200℃ for 1min-5min; the dispersion of the second layer is a dispersion of water, ethanol, ethylene glycol, and polymer P (AM-ATU) nanoparticles, the rotation speed of the spin coater is 1000rpm-4000rpm, the time is 20s-80s, and it is cured for 3min-10min at a magnetic field strength of 20mT-60mT, and dried at 100℃-200℃ for 1min-5min; the preparation conditions of the third to fifth layers are similar.
[0012] A magneto-photonic crystal film for rapid visual detection of heavy metal Ni 2+ The method comprises the following steps: 1) Prepare different concentrations of Ni 2+ The aqueous solution of different concentrations of Ni 2+ The aqueous solution was dripped onto the magneto-photonic crystal film, and the reaction time was 1-20 minutes. The color change was observed. With the increase of concentration, the color change trend was gradually blue shift. 2) Use Haiyang optical spectrometer to measure the reflectance spectrum and establish a standard curve to detect Ni 2+ The linear range is 1×10 -7 mol / L—2×10 -1 mol / L.
[0013] The beneficial effects of the present invention are: 1. The present invention uses monodisperse (PDI < 0.1) silicon oxide core-shell magnetic nanoparticles as magnetic responsive photonic crystal materials, which have the characteristics of fast response rate, high sensitivity, rapid migration along the magnetic field direction under the action of an external magnetic field, and self-assembly arrangement to form a stable chain structure. Its magnetic response band gap can cover the entire visible spectrum, and has fast, bright and reversible diffraction changes.
[0014] 2. A thiourea-functional polymer P(AM-ATU) was prepared as an indicator of Ni in aqueous solution. 2+ As the chemical structure of the copolymer changes, the functional copolymer layer of the photonic material in water expands sharply, causing a large volume contraction of the polymer layer, which ultimately causes the diffraction wavelength of the photonic structure to blue shift and automatically convert into a visually perceptible color change. 2+ The exclusion of water due to binding and polymer shrinkage changes the refractive index, which also contributes to the photosensing signal.
[0015] 3. The transition of magnetic nanoparticles from ordered arrangement to disordered arrangement at a certain concentration will also cause the diffraction wavelength of the photonic structure to change. Therefore, the ordered magnetic nanoparticles in the magneto-photonic crystal film gradually become disordered in the solution, which will change the color. Combining functional polymers and magnetic nanoparticles can make the reflected color change more obviously.
[0016] 4. The present invention indicates different concentrations of Ni by using different reaction colors of the magneto-photonic crystal film 2+ Whether the standard is exceeded can be judged by naked eyes without any instrument, so the detection cost is low and the operation is simple. A highly sensitive, low-cost and simple detection method for Ni 2+ method. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 The schematic diagram of the preparation and visual detection of magneto-photonic crystal film; Figure 2 TEM image and particle size distribution of monodispersed silicon oxide core-shell structure nanoparticles; Figure 3 This is a SEM image of spin-coated magnetic nanoparticles and solidified under a magnetic field; Figure 4 Photos of different numbers of layers of spin-coated magneto-photonic crystal films; Figure 5 Three layers of magneto-photonic crystal films with different concentrations of Ni 2+ Reflectance spectrum after reaction. DETAILED DESCRIPTION
[0018] The present invention will be further described below in conjunction with the accompanying drawings and specific embodiments: The preparation steps of magneto-photonic crystal thin film are as follows: 1) Obtain Fe 3 O 4 Nano magnetic particles 1.7 g FeCl 3 6H 2 O and 4.5 g NaAc·3H 2 O was dissolved in 300ml ethylene glycol, and 1ml deionized water was added. After it was completely dissolved, the brown solution was transferred to a 500ml high-temperature and high-pressure reactor, and the speed was controlled at 300r / min. Two-stage heating was performed; the first stage was heated at 160℃ for 3h, and the second stage was heated at 200℃ for 5h. After natural cooling, it was washed with anhydrous ethanol for 3-5 times, and finally dispersed in anhydrous ethanol.
[0019] 2) Preparation of silicon oxide core-shell structured nanomagnetic particles The Fe prepared in step 1) was 3 O 4 The nano-magnetic particles were dispersed in 2L of alcohol solution, which included 750ml of deionized water and 1250ml of anhydrous ethanol; ultrasonic dispersion was performed for 20 minutes, and 6.25ml of tetraethyl orthosilicate (TEOS) was added dropwise after adding 125ml of ammonia water, and ultrasonic reaction was performed for 40 minutes; after the reaction, magnetic separation was performed and the particles were washed with anhydrous ethanol for 3-5 times to obtain magnetic nano-particles with a silicon oxide core-shell structure; and then magnetic nano-particle dispersions with three concentration levels of 10mg / ml, 20mg / ml and 30mg / ml were prepared; Figure 2 It can be seen that the silica core-shell magnetic nanoparticles have good dispersibility, and their PDI index is less than 0.1.
[0020] 3) Preparation of polymer P(AM-ATU) nanoparticles AM (acrylamide) and ATU (N-allylthiourea) were dissolved in 1 ml of deionized water at a mass ratio of 1:1 to form solution A; 5 mg of AIBN (azobisisobutyronitrile) was dissolved in 1 ml of toluene to form solution B; 1 g of AOT (docusate sodium) was dissolved in 50 ml of toluene solution to form solution C. Solution C was heated to 50°C under nitrogen protection and condensation reflux, and solution B was added to the hot reaction solution; finally, solution A was stirred at 0.1 ml·min -1The mixture was injected into the reaction solution at a speed of 1000 μm and reacted for 0.5 h. After the reaction, the mixture was cooled naturally and anhydrous ethanol with a volume twice that of the mixed solution was added for precipitation. After removing the supernatant, a polymer P (AM-ATU) dispersion with a mass concentration of 2% was prepared.
[0021] 4) Preparation of magneto-photonic crystal films Surface Oriented <111> The silicon wafer with silicon oxide layer is used as the substrate, and the polymer P prepared in step 3) is spin-coated at a speed of 2000 rpm for 20 seconds and then dried at 100°C for 1 minute.
[0022] Example 2 The preparation steps of magneto-photonic crystal thin film are as follows: 1) Obtain Fe 3 O 4 Nano magnetic particles 1.7 g FeCl 3 6H 2 O and 4.5 g NaAc·3H 2 O was dissolved in 300ml ethylene glycol, and 1ml deionized water was added. After it was completely dissolved, the brown solution was transferred to a 500ml high-temperature and high-pressure reactor, with a speed of 300r / min and two-stage heating, the first stage was heated at 160℃ for 3h, and the second stage was heated at 200℃ for 5h. After natural cooling, it was washed with anhydrous ethanol for 3-5 times and finally dispersed in anhydrous ethanol.
[0023] 2) Preparation of silicon oxide core-shell structured nanomagnetic particles The Fe prepared three times in step 1) 3 O 4 The nano-magnetic particles are dispersed in 2L of alcohol solution, the alcohol solution includes 750ml of deionized water and 1250ml of anhydrous ethanol; ultrasonic dispersion is performed for 20 minutes, 125ml of ammonia water is added, and then 6.25ml of tetraethyl orthosilicate (TEOS) is added dropwise, and the ultrasonic reaction is performed for 40 minutes. After the reaction is completed, magnetic separation is performed and the particles are washed with anhydrous ethanol for 3-5 times to obtain magnetic nano-particles with a silicon oxide core-shell structure, and the magnetic nano-particle dispersions with three concentrations of 10mg / ml, 20mg / ml and 30mg / ml are prepared; 3) Preparation of polymer P(AM-ATU) nanoparticles AM (acrylamide) and ATU (N-allylthiourea) were dissolved in 1 ml of deionized water at a mass ratio of 1:1 to form solution A; 5 mg of AIBN (azobisisobutyronitrile) was dissolved in 1 ml of toluene to form solution B; 1 g of AOT (docusate sodium) was dissolved in 50 ml of toluene solution to form solution C. Solution C was heated to 50°C under nitrogen protection and condensation reflux, and solution B was added to the hot reaction solution. Finally, solution A was stirred at 0.1 ml·min -1 The reaction mixture was injected into the reaction solution at a speed of 1000 μg / min and reacted for 0.5 h. After the reaction was completed, the mixture was naturally cooled and anhydrous ethanol twice the volume of the solution was added for precipitation. After removing the supernatant, a polymer P (AM-ATU) dispersion with a mass concentration of 2% was prepared.
[0024] 4) Preparation of magneto-photonic crystal films Surface Oriented <111> The silicon wafer with silicon oxide layer is used as the substrate, the polymer P prepared in step 3) is spin-coated at a speed of 2000 rpm for 20 seconds and then dried at 100°C for 1 minute to obtain a first thin film; the magnetic nanoparticle dispersion of silicon oxide core-shell structure in step 2) is spin-coated on the first thin film at a speed of 2000 rpm for 20 seconds and then left to stand in a magnetic field of 20 mT for 1 minute, and then dried at 100°C for 1 minute, from Figure 3 It can be seen that the magnetic nanoparticles are arranged in an orderly manner in the film after applying a magnetic field.
[0025] In Examples 3-7, the preparation conditions of silicon oxide core-shell structure magnetic nanoparticles are the same as those of step 1) and step 2) in Example 1, and the steps of step 3) and step 4) are the same. The specific raw materials and reaction conditions are shown in Tables 1 and 2 below: Table 1 Table 2 After consulting the data, it was found that most of the conventional preparation methods of magneto-photonic crystal films choose the mold method, that is, to process a fixture of a certain thickness, mix the magnetic nanoparticles with photon effect with organic matter in proportion, inject them into the fixture and apply a fixed magnetic field. This method prepares magneto-photonic crystal films that are relatively thick, kept at the millimeter level, and cannot achieve the composite superposition of multilayer films. The preparation conditions are relatively complex. Compared with the traditional preparation method, the film thickness prepared by the spin coating method is thin, and it is micron-level after detection. After applying the magnetic field, the magnetic nanoparticles can quickly achieve orderly arrangement, the curing rate is fast, and it has outstanding advantages in realizing the preparation of multilayer films, such as fast, convenient, and simple. At the same time, due to the thin film thickness, the color change time is short when detected in the solution, which can greatly improve the detection efficiency and provide a solution for the subsequent composite processing of multifunctional layers.
[0026] Figure 1 This is the principle diagram of the color change of magneto-photonic crystal film. Figure 4 The color of the film after multi-layer spin coating. The ligands on the film layer of polymer P(AM-ATU) nanoparticle spin coating can react with metal Ni 2+ Chelation causes a large volume shrinkage of the polymer layer, which eventually leads to a blue shift in the diffraction wavelength of the photonic structure, which is automatically converted into a visually perceptible color change. At the same time, the addition of magneto-photonic crystals, after multi-layer spin coating and orderly arrangement of magneto-photonic crystal films under a magnetic field, gradually becomes disordered in the aqueous solution, which also causes changes in the reflected light. Combining the two, the color change before and after the detection will be greatly enhanced compared to the single-layer film, which can improve the Ni in the aqueous solution. 2+ The detection line and specificity, such as Figure 5 The color change before and after the reaction shown has a large span and is easy to distinguish.
[0027] Taking Example 5 as an example, the concentrations of 0µm, 200µm, 400µm, 600µm, and 800µm Ni 2+ The solution reacted for 1 min, and the reaction system had an obvious color change. The reflectance spectrum was tested by a portable spectrometer, such as Figure 5 As shown, then Ni 2+ With the increase of concentration, the color of the reflection peak position shifts significantly to the blue.
Claims
1. A method for preparing a magneto-photonic crystal film, characterized in that: The following steps are involved: 1) Obtaining or preparing Fe3O4 magnetic nanoparticles; 2) Preparation of silicon oxide core-shell structured magnetic nanoparticles: The Fe3O4 magnetic nanoparticles prepared in step 1) are mixed with tetraethyl orthosilicate (TEOS), liquid alcohol and concentrated ammonia water in proportion, and reacted under ultrasonic conditions to prepare silicon oxide core-shell structured magnetic nanoparticles; 3) Preparation of polymer P (AM-ATU) nanoparticles: AM (acrylamide), ATU (N-allylthiourea), surfactant AOT (docusate sodium), toluene, and AIBN (azobisisobutyronitrile) were mixed successively, the hot reaction liquid was condensed and refluxed with stirring, and after the reaction was completed, ethanol was used for precipitation to obtain polymer P (AM-ATU) nanoparticles; 4) Preparation of magneto-photonic crystal film: Take the polymer P(AM-ATU) nanoparticle dispersion prepared in step 3) and prepare the first film by spin coating; Take the silicon oxide core-shell structure magnetic nanoparticle dispersion prepared in step 2) and prepare a second film layer on top of the first film layer by spin coating; immediately apply a magnetic field after the spin coating is completed, so that the silicon oxide core-shell structure magnetic nanoparticles are orderly arranged under the action of the magnetic field; repeat this step to prepare a total of 2 to 5 layers of film, thereby preparing a magneto-photonic crystal film.
2. The method for preparing a magneto-photonic crystal film according to claim 1, characterized in that: The silicon oxide core-shell structure magnetic nanoparticles prepared in step 2) have a PDI (aggregation index) of <0.1 and are in a monodisperse state.
3. The method for preparing a magneto-photonic crystal film according to claim 1, characterized in that: The mixing reaction steps in step 3) are as follows: 1) Prepare the reaction solution Dissolve AM (acrylamide) and ATU (N-allylthiourea) in a mass ratio of 1:1-5:1 in 1 ml-5 ml of deionized water to form a monomer solution A; Dissolve 5 mg to 15 mg of AIBN (azobisisobutyronitrile) in 1 ml to 5 ml of toluene to form solution B; Dissolve 1 g to 5 g of AOT (docusate sodium) in 50 ml of toluene solution to form solution C; 2) Reaction process Solution C is heated to a temperature of 50°C to 90°C under nitrogen protection and condensation reflux conditions to form a hot reaction liquid; Then add solution B to the hot reaction solution; finally, add solution A at 0.5 ml min -1 —2ml·min -1 The mixture is injected into the hot reaction liquid at a rate of and reacted for 0.5h-2h.
4. The method for preparing a magneto-photonic crystal film according to claim 1, characterized in that: The mass concentration of the polymer P(AM-ATU) nanoparticles prepared in step 3) dispersed in water is 2%-10%.
5. The method for preparing a magneto-photonic crystal film according to claim 1, characterized in that: The substrate for preparing the magneto-photonic crystal film in step 4) is a silicon wafer having a crystal plane-oriented silicon oxide layer on the surface ( <111> , <100> ).
6. The method for preparing a magneto-photonic crystal film according to claim 1, characterized in that: The magneto-photonic crystal film prepared in step 4) has 2 to 5 layers, wherein the first layer is a dispersion of polymer P (AM-ATU) nanoparticles, which is used to improve the bonding of the magneto-photonic crystal film; the second layer is a dispersion of silicon oxide core-shell structure magnetic nanoparticles; and the third to fifth layers are analogous.
7. The method for preparing a magneto-photonic crystal film according to claim 6, characterized in that: In the preparation of the first layer, the speed of the spin coater is 2000rpm-5000rpm, the time is 20s-80s, and it is dried at 100℃-200℃ for 1min-5min; the dispersion of the second layer is a dispersion of water, ethanol, ethylene glycol, and polymer P (AM-ATU) nanoparticles, the speed of the spin coater is 1000rpm-4000rpm, the time is 20s-80s, and it is cured for 3min-10min at a magnetic field strength of 20mT-60mT, and dried at 100℃-200℃ for 1min-5min; the preparation conditions of the third to fifth layers are similar.
8. A method for visually detecting heavy metal Ni using the magneto-photonic crystal film described in any one of claims 1 to 7 2+ The method is characterized in that The steps include: 1) Prepare different concentrations of Ni 2+ The aqueous solution of different concentrations of Ni 2+ The aqueous solution is dripped onto the magneto-photonic crystal film prepared in step 4), the reaction time is 1 min-20 min, and the color change is observed. As the concentration increases, the color change trend is a gradual blue shift; 2) Use Haiyang optical spectrometer to measure the reflectance spectrum and establish a standard curve to detect Ni 2+ The linear range is 1×10 - 7 mol / L—2×10 -1 mol / L.
Citation Information
Patent Citations
Inverse-opal hydrogel photonic crystal sensing film capable of realizing naked-eye detection of concentration of cadmium ion
CN106084123A
Method for preparing magnetic amorphous photonic crystal from ferroferric oxide / silicon dioxide core-shell structure nanoparticles
CN108919386A
Preparation method and application of Ni-NTA modified silicon dioxide coated ferroferric oxide magnetic nano functional assembly
CN111167409A
Nucleic acid probe superparamagnetic photonic crystal sensing material, preparation method and application
CN115452732A
Quick-response photonic crystal heterogeneous gel material as well as preparation method and application thereof
CN116854999A