Fireproof water-based paint for interior and exterior walls and preparation method of fireproof water-based paint

By forming a crosslinking network structure with polylactic acid-based epoxy resin and aqueous amine curing agent, and combining acrylic modified epoxy resin and nano zinc oxide particles, the problem of fire resistance attenuation of existing fire-retardant coatings in harsh environments is solved, and the fire resistance performance attenuation of existing fire-retardant coatings in harsh environments is achieved. High-performance fire-resistant water-based coatings suitable for high-temperature fire protection in steel and concrete structures.

CN118995004AInactive Publication Date: 2024-11-22GUODING (SUZHOU) MATERIAL TECH CO LTD

Patent Information

Application Number
CN202411130058.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In harsh environments, existing fire-resistant coatings have deteriorated fire-resistant performance due to moisture absorption, migration and precipitation of carbon agents, and are difficult to meet the high-temperature fire protection needs of steel structures and concrete structures.

Method used

The cross-linked network structure is formed with polylactic acid-based epoxy resin and aqueous amine curing agent as the main component of fire-retardant coating, and the mixture of acrylic modified epoxy resin and silica sol-modified acrylic resin is combined with nano zinc oxide particles. A uniform paint film is formed to improve refractory resistance.

Benefits of technology

The excellent adhesion, cohesion strength, durability and corrosion resistance of the coating are achieved, crack resistance and impact resistance are enhanced, fire resistance is extended, fire resistance is improved, and moisture absorption problem of carbon-forming agents is avoided.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004997555960000121
    Figure BDA0004997555960000121
  • Figure BDA0004997555960000131
    Figure BDA0004997555960000131
Patent Text Reader

Abstract

The invention discloses a fireproof water-based paint for interior and exterior walls and a preparation method thereof, and relates to the technical field of paints. A mixture of acrylic acid modified epoxy resin and silicon dioxide sol modified acrylic resin is used as modified resin, acrylic acid groups are introduced into the modified resin, carbon-carbon double bonds in silicon dioxide sol and acrylic acid can be softened and broken in advance when meeting fire, and the expansion degree of a paint film is improved through the synergistic effect with nano-zinc oxide; a heat-insulating carbon layer is formed to improve the fireproof performance of the coating; the silicon dioxide sol is uniformly dispersed in the acrylic resin, so that the corrosion resistance and durability of a paint film are improved. The polylactic acid-based epoxy resin is used as a material, and two interpenetrating network structures are formed between the polylactic acid-based epoxy resin and the modified resin, so that the stress generated during curing of the epoxy resin is reduced, and the overall toughness, cracking resistance and impact resistance are improved. The prepared fireproof water-based paint for the interior and exterior walls is excellent in fireproof performance and corrosion resistance, environmentally friendly and capable of meeting the sustainable development concept.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of coatings, in particular to a fire-retardant water-based coating for interior and exterior walls and a preparation method thereof. Background Art

[0002] With the extensive application of organic synthetic materials, their flammability has become increasingly prominent. Organic polymers containing halogens and other flame retardants often lead to the deterioration of the physical properties of the materials, shortened service life and increased prices. The method of applying fire retardant coatings on their surfaces for fire protection can not only maintain the excellent properties of the original organic synthetic materials, but also be economical and applicable. The application of fire retardant coatings on organic synthetic materials also has broad prospects. In addition, ordinary steel loses its structural strength when heated to about 540°C; concrete structures are also prone to cracking and disintegration under the action of high-temperature flames. Therefore, fire protection of steel structures and concrete structures can prolong the time for deformation and damage when a fire occurs, gain time for fire extinguishing, and reduce fire losses. People attach great importance to it, and the application of fire retardant coatings on steel structures and cement structures is expanding.

[0003] Water-based paint is very popular because of its environmentally friendly characteristics that it can be well dispersed in water and no longer uses organic solvents containing benzene, toluene, xylene, esters, etc. as diluents. Therefore, it is necessary to develop a fire-retardant water-based paint for walls. Summary of the invention

[0004] The object of the present invention is to provide a fire retardant water-based paint for interior and exterior walls and a preparation method thereof, so as to solve the problems existing in the prior art.

[0005] In order to solve the above problems, the present invention provides the following technical solution: a method for preparing a fire retardant water-based coating for interior and exterior walls, characterized in that it comprises the following preparation steps:

[0006] (1) Weighing ethyl orthosilicate and ethanol in a container according to the mass ratio, stirring, adding deionized water to dissolve, keeping the temperature in a water bath, adding a catalyst and an organic silane coupling agent, continuously stirring and mixing, condensing and refluxing, and obtaining a uniform nano-silica sol;

[0007] (2) uniformly mixing an acrylic prepolymer and dibutyl phthalate according to a mass ratio, adding an organic solvent to dissolve, adding nano zinc oxide, continuing to stir, keeping the temperature in a water bath, slowly dropping nano silica sol, raising the temperature after the reaction is complete, performing reduced pressure distillation, removing the organic solvent and water, and obtaining a silica sol-modified acrylic resin;

[0008] (3) reacting low molecular weight polylactic acid and maleic anhydride in an inert gas atmosphere, controlling the temperature and reaction time, to obtain polylactic acid terminated with carboxyl groups at both ends;

[0009] (4) dissolving the polylactic acid terminated with carboxyl groups obtained in the previous step in water and an organic solvent, keeping the temperature constant in a water bath, adding a halogenated epoxy compound and an alkaline metal catalyst with stirring, reacting completely, filtering, separating the aqueous phase, adding an alkaline metal catalyst again, and distilling after sufficient reaction to obtain a polylactic acid-based epoxy resin;

[0010] (5) adding polylactic acid-based epoxy resin, acrylic acid-modified epoxy resin, silica sol-modified acrylic resin and modified flame retardant to a reaction kettle in sequence, stirring them thoroughly to make the components uniform, then adding ammonium polyphosphate and melamine cyanurate, heating and stirring them uniformly, and then adding reinforcing filler and continuing to stir to obtain component A;

[0011] (6) Add cyanuric acid melamine salt, talcum powder and water-based modified amine curing agent to the reaction container in sequence, keep the temperature in a water bath, stir evenly, add reinforcing fiber, and after the reaction is complete, move to a three-roll mill, grind, and refine the particles to obtain component B;

[0012] (7) Component A and component B are mixed in a certain mass ratio to prepare a fire retardant water-based coating for interior and exterior walls.

[0013] Furthermore, in the step (1), the mass ratio of tetraethyl orthosilicate, ethanol, catalyst, and organic silane coupling agent is 10-12:20-25:0.1-0.2:0.5-1; the catalyst in the step (1) is hydrochloric acid with a concentration of 0.01M-0.1M; the organic silane coupling agent in the step (1) is KH-570; the water bath temperature in the step (1) is 70-80°C, and the condensation reflux is carried out for 3-5h.

[0014] Furthermore, the acrylic prepolymer in step (2) is obtained by adding azobisisobutyronitrile as an initiator to a mixture of methyl methacrylate and ethyl acrylate; the mass ratio of the acrylic prepolymer, dibutyl phthalate, zinc oxide and silica sol in step (2) is 30-50:20-40:3-5:10-20; the water bath temperature in step (2) is 80°C-100°C, the silica sol is slowly added dropwise, the reaction is carried out for 18h-24h, and then the temperature is raised to 100-120°C and maintained for 2-4h.

[0015] Furthermore, the molecular weight of the polylactic acid is 10,000 to 100,000; the molar ratio of the polylactic acid to maleic anhydride is 1 to 3:2 to 4; the reaction temperature of the step (3) is 110 to 130° C., and the reaction time is 3 to 5 hours.

[0016] Furthermore, the halogenated epoxy compound is epichlorohydrin, and the alkaline metal catalyst is a mixture of sodium hydroxide and potassium hydroxide; the molar ratio of the carboxyl-terminated polylactic acid, the alkali metal catalyst, and the halogenated epoxy compound is 3-5:0.6-1.2:8-25; and the reaction temperature of step (4) is 30-80°C and the reaction time is 1-4h.

[0017] Furthermore, in the step (5), there are 20 to 25 parts of lactic acid epoxy resin; 10 to 20 parts of modified resin; 25 to 30 parts of modified flame retardant; 25 to 30 parts of ammonium polyphosphate; 5 to 8 parts of cyanuric acid melamine salt; 3 to 8 parts of reinforcing filler; and 2 to 3 parts of reinforcing fiber; the modified flame retardant is prepared by mixing polyethylene glycol ether and pentaerythritol phosphate, wherein the mass ratio of polyethylene glycol ether to pentaerythritol phosphate is 1 to 3:4 to 8; the reinforcing filler in the step (5) is basalt, and the particle size of the basalt is 300 to 500 mesh; the reinforcing fiber in the step (5) is one or more of zirconium-containing ceramic fiber, carbon fiber, basalt fiber, glass fiber, and boron fiber.

[0018] Furthermore, in step (6), the water-based modified amine curing agent is 40 to 60 parts; talcum powder is 10 to 15 parts; cyanuric acid melamine salt is 15 to 25 parts; and reinforcing fiber is 5 to 10 parts.

[0019] Furthermore, the mass ratio of component A to component B is 4 to 6:1.

[0020] Furthermore, a fire-retardant water-based paint for interior and exterior walls is provided, characterized in that the paint is prepared by the method described.

[0021] Compared with the prior art, the beneficial effects achieved by the present invention are as follows: a fire-retardant water-based paint for interior and exterior walls of the present invention uses polylactic acid-based epoxy resin as a synthetic material for the fire-retardant water-based paint; the polylactic acid-based epoxy resin material has excellent biodegradability and conforms to the environmental protection concept of sustainable development; and a cross-linked network structure formed after curing with a water-based amine curing agent can be used as the main carbonizing agent in the fire-retardant paint, without the need to add additional polyhydroxy hydrocarbons as carbonizing agents, thereby avoiding the problem of fire-retardant performance attenuation and anti-corrosion performance degradation of traditional fire-retardant paints in harsh environments due to the moisture absorption, migration and precipitation of carbonizing agents; the paint film formed by the polylactic acid-based epoxy resin after curing with the water-based amine curing agent has excellent adhesion, cohesive strength, durability and corrosion resistance, and can meet the requirements of indoor and outdoor environments.

[0022] The present invention uses a mixture of acrylic acid modified epoxy resin and silica sol modified acrylic resin as modified resin. The acrylic acid modified epoxy resin in the modified resin can increase the compatibility between epoxy resin and silica sol modified acrylic resin, so that the film-forming material has a high degree of uniformity. The organic silane coupling agent and silica are copolymerized to generate organic silicon. The surface hydroxyl groups of silica sol and the hydroxyl groups on the organic silicon molecular chain undergo condensation cross-linking reaction, which plays a bridging role between the organic phase and the inorganic phase. This bridging role enables the silica sol to be uniformly dispersed in the acrylic resin, thereby improving the corrosion resistance and durability of the paint film. Secondly, the acrylic acid modified epoxy resin and the silica sol modified acrylic resin Two interpenetrating network structures are formed between the acrylic acid group and the polylactic acid epoxy resin, which are interspersed and entangled with each other, reducing the stress generated when the epoxy resin and the amine curing agent are cured, increasing the toughness of the overall resin, and greatly improving the crack resistance and impact resistance of the coating with high film thickness. In addition, the CC bond energy of the acrylic acid group and the ester group in the modified resin are much lower than the bond energy of the benzene ring structure in the epoxy group. When exposed to fire, they can soften and break in advance, which can increase the early expansion of the paint film and form an insulating carbon layer in advance. Nano zinc oxide particles are introduced to improve the structure of the expanded carbon layer, making the foaming pores small, uniform and dense, extending the fire resistance time, and improving the fire retardant performance of the coating.

[0023] The present invention prepares the coating by preparing component A and component B separately and then mixing them, which facilitates the chemical reaction of the coating in advance, facilitates the storage of the coating, and can control the mixed mass ratio to achieve the best performance requirements. DETAILED DESCRIPTION

[0024] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0025] In order to more clearly illustrate the method provided by the present invention, the following examples are used to describe in detail the various index testing methods of the fire retardant water-based coatings for interior and exterior walls prepared in the following examples are as follows:

[0026] Salt spray resistance: Use 150mm×75mm×3mm steel plate, paint film thickness 6mm, test according to ASTM B117 standard;

[0027] Fire resistance: Use a steel plate of 150mm×150mm×6mm and a paint film thickness of 6mm. Test according to GA / T714-2007 standard. The time when the back temperature of the steel plate reaches 450℃ is taken as the fire resistance limit.

[0028] Carbon layer strength: Use a compression bending tester to select a 60mm×60mm carbon layer after the fire resistance test, and test it and record the strength value;

[0029] Corrosion rate: Use a steel plate of 150mm×150mm×6mm, with a paint film thickness of 6mm, and use the GB / T19746-2005 method for testing, taking the average of three times;

[0030] Example 1

[0031] (1) Weigh 110 parts of ethyl orthosilicate and 220 parts of ethanol into a container, stir, add deionized water to dissolve, keep the water bath temperature at 70°C, add 1 part of 0.1M hydrochloric acid as a catalyst and 3 parts of an organic silane coupling agent KH-570, continue to stir and mix evenly, condense and reflux for 3 hours to obtain a uniform nano-silica sol.

[0032] (2) 30 parts of acrylic prepolymer and 20 parts of dibutyl phthalate were mixed evenly, 30 parts of ethanol was added to dissolve, 10 parts of nano zinc oxide was added, stirring was continued, the temperature was kept constant at 85°C in a water bath, nano silica sol was slowly added dropwise, the reaction was continued for 21 hours, the temperature was then raised to 110°C, and the organic solvent and water were removed by vacuum distillation to obtain silica sol modified acrylic resin.

[0033] (3) reacting 35 parts of low molecular weight polylactic acid and 30 parts of maleic anhydride under an inert gas atmosphere at 120° C. for 4 hours to obtain polylactic acid terminated with carboxyl groups at both ends;

[0034] (4) 30 parts of the polylactic acid with carboxyl groups terminated at both ends obtained in the previous step were dissolved in water and an organic solvent, and the mixture was kept in a water bath at a constant temperature of 55° C., 120 parts of epichlorohydrin and 4 parts of sodium hydroxide were added with stirring, and the mixture was reacted for 1.5 hours, filtered, and the aqueous phase was separated, and 4 parts of potassium hydroxide was added again. After sufficient reaction for 1 hour, the mixture was distilled to obtain a polylactic acid-based epoxy resin;

[0035] (5) Add 20 parts of polylactic acid-based epoxy resin, 10 parts of acrylic modified epoxy resin, 5 parts of silica sol modified acrylic resin, and 30 parts of modified flame retardant in the reaction kettle in sequence, stir them thoroughly to make the ingredients uniform, then add 25 parts of ammonium polyphosphate and 5 parts of cyanuric acid melamine salt, disperse at high speed for 60 minutes at 55° C., then add 5 parts of basalt, 2 parts of carbon fiber, and 1 part of zirconium-containing ceramic fiber, stir at low speed for 50 minutes to obtain component A;

[0036] (6) Add 25 parts of melamine cyanurate salt, 15 parts of talc, and 50 parts of water-based modified amine curing agent to a reaction container in sequence, keep the temperature in a water bath at 60° C., stir evenly, add 10 parts of glass fiber and 3 parts of boron fiber, and after the reaction is complete, move the mixture into a three-roll mill, grind, and refine the particles to obtain component B;

[0037] (7) Component A and component B are mixed evenly in a ratio of 5:1 to prepare a fire retardant water-based coating for interior and exterior walls.

[0038] Example 2

[0039] (1) Weigh 100 parts of ethyl orthosilicate and 200 parts of ethanol into a container, stir, add deionized water to dissolve, keep the temperature in a water bath at 80°C, add 1 part of 0.1M hydrochloric acid as a catalyst and 1 part of an organic silane coupling agent KH-570, continue to stir and mix evenly, condense and reflux for 5 hours, and obtain a uniform nano-silica sol.

[0040] (2) 35 parts of acrylic prepolymer and 25 parts of dibutyl phthalate were mixed evenly, 40 parts of ethanol was added to dissolve, 15 parts of nano zinc oxide was added, stirring was continued, the temperature was kept constant at 95°C in a water bath, nano silica sol was slowly added dropwise, the reaction was carried out for 24 hours, the temperature was then raised to 120°C, and the organic solvent and water were removed by vacuum distillation to obtain silica sol modified acrylic resin.

[0041] (3) reacting 40 parts of low molecular weight polylactic acid and 50 parts of maleic anhydride in an inert gas atmosphere at 130° C. for 5 hours to obtain polylactic acid terminated with carboxyl groups at both ends;

[0042] (4) 35 parts of the polylactic acid with carboxyl groups terminated at both ends obtained in the previous step were dissolved in water and an organic solvent, and the mixture was kept at a constant temperature of 80° C. in a water bath, and 170 parts of epichlorohydrin and 5 parts of sodium hydroxide were added with stirring, and the mixture was reacted for 2 hours, filtered, and the aqueous phase was separated, and 5 parts of potassium hydroxide was added again. After sufficient reaction for 2 hours, the mixture was distilled to obtain a polylactic acid-based epoxy resin;

[0043] (5) Add 25 parts of polylactic acid-based epoxy resin, 10 parts of acrylic acid-modified epoxy resin, 10 parts of silica sol-modified acrylic resin, and 40 parts of modified flame retardant in the reaction kettle in sequence, stir them thoroughly to make the ingredients uniform, then add 30 parts of ammonium polyphosphate and 5 parts of cyanuric acid melamine salt, disperse at high speed for 60 minutes at 55° C., then add 5 parts of basalt, 2 parts of carbon fiber, and 1 part of zirconium-containing ceramic fiber, stir at low speed for 50 minutes to obtain component A;

[0044] (6) 30 parts of melamine cyanurate salt, 20 parts of talcum powder, and 50 parts of water-based modified amine curing agent were added to a reaction container in sequence, the temperature was kept constant at 60° C. in a water bath, and the mixture was stirred evenly. 10 parts of glass fiber and 3 parts of boron fiber were added. After the reaction was complete, the mixture was moved to a three-roll mill, ground, and the particles were refined to obtain component B;

[0045] (7) Component A and component B are mixed evenly in a ratio of 6:1 to prepare a fire retardant water-based coating for interior and exterior walls.

[0046] Example 3

[0047] (1) Weigh 120 parts of ethyl orthosilicate and 250 parts of ethanol into a container, stir, add deionized water to dissolve, keep the water bath temperature at 70°C, add 2 parts of 0.1M hydrochloric acid as a catalyst and 5 parts of an organic silane coupling agent KH-570, continue to stir and mix evenly, condense and reflux for 5 hours, and obtain a uniform nano-silica sol.

[0048] (2) 25 parts of acrylic prepolymer and 15 parts of dibutyl phthalate were mixed evenly, 25 parts of ethanol were added to dissolve, 10 parts of nano zinc oxide were added, stirring was continued, the temperature was kept constant at 80°C in a water bath, nano silica sol was slowly added dropwise, the reaction was continued for 18 hours, the temperature was then raised to 105°C, and the organic solvent and water were removed by vacuum distillation to obtain silica sol modified acrylic resin.

[0049] (3) reacting 25 parts of low molecular weight polylactic acid and 30 parts of maleic anhydride under an inert gas atmosphere at 110° C. for 3 hours to obtain polylactic acid terminated with carboxyl groups at both ends;

[0050] (4) Dissolve 25 parts of the polylactic acid terminated with carboxyl groups obtained in the previous step in water and an organic solvent, keep the temperature in a water bath at 30° C., add 70 parts of epichlorohydrin and 2.5 parts of sodium hydroxide with stirring, react for 0.5 h, filter, separate the aqueous phase, add 2.5 parts of potassium hydroxide again, react for 0.5 h, and then distill to obtain a polylactic acid-based epoxy resin;

[0051] (5) Add 20 parts of polylactic acid-based epoxy resin, 10 parts of acrylic modified epoxy resin, 5 parts of silica sol modified acrylic resin, and 30 parts of modified flame retardant in the reaction kettle in sequence, stir them thoroughly to make the ingredients uniform, then add 25 parts of ammonium polyphosphate and 5 parts of cyanuric acid melamine salt, disperse at high speed for 60 minutes at 55° C., then add 5 parts of basalt, 2 parts of carbon fiber, and 1 part of zirconium-containing ceramic fiber, stir at low speed for 50 minutes to obtain component A;

[0052] (6) Add 20 parts of melamine cyanurate salt, 1 part of talcum powder, and 40 parts of water-based modified amine curing agent to a reaction container in sequence, keep the temperature in a water bath at 60° C., stir evenly, add 10 parts of glass fiber and 3 parts of boron fiber, and after the reaction is complete, move to a three-roll mill, grind, and refine the particles to obtain component B;

[0053] (7) Component A and component B are mixed evenly in a ratio of 4:1 to prepare a fire retardant water-based coating for interior and exterior walls.

[0054] Comparative Example 1

[0055] The difference between Comparative Example 1 and Example 1 is that steps (1) and (2) are deleted, and step (5) is changed to sequentially add 20 parts of polylactic acid-based epoxy resin, 15 parts of acrylic modified epoxy resin, and 30 parts of modified flame retardant into a reaction kettle, stir them thoroughly to make the components uniform, then add 25 parts of ammonium polyphosphate and 5 parts of cyanuric acid melamine salt, and disperse at high speed for 60 minutes at 55° C., then add 5 parts of basalt, 2 parts of carbon fiber, and 1 part of zirconium-containing ceramic fiber, and stir at low speed for 50 minutes to obtain component A;

[0056] Comparative Example 2

[0057] The difference between Comparative Example 2 and Example 1 is that steps (1) and (2) are deleted, and step (5) is changed to sequentially add 20 parts of polylactic acid-based epoxy resin, 10 parts of acrylic acid-modified epoxy resin, 5 parts of commercially available silica sol-modified acrylic resin, and 30 parts of modified flame retardant into a reaction kettle, stir them thoroughly to make the ingredients uniform, then add 25 parts of ammonium polyphosphate and 5 parts of cyanuric acid melamine salt, disperse at high speed for 60 minutes at 55° C., then add 5 parts of basalt, 2 parts of carbon fiber, and 1 part of zirconium-containing ceramic fiber, stir at low speed for 50 minutes, and obtain component A;

[0058] Comparative Example 3

[0059] The difference between Comparative Example 3 and Example 1 is that step (2) is changed to (2): 30 parts of acrylic prepolymer and 20 parts of dibutyl phthalate are mixed evenly, 30 parts of ethanol are added to dissolve, and stirring is continued. The temperature is kept constant at 85° C. in a water bath, and nano-silica sol is slowly added dropwise. The reaction is carried out for 21 hours, and then the temperature is raised to 110° C. and distilled under reduced pressure to remove the organic solvent and water to obtain a silica sol-modified acrylic resin.

[0060] Comparative Example 4

[0061] The difference between Comparative Example 4 and Example 1 is that steps (3) and (4) are deleted, and step (5) is changed to sequentially add 20 parts of cyclopentadiene epoxy resin, 10 parts of acrylic acid modified epoxy resin, 5 parts of silica sol modified acrylic resin, and 30 parts of modified flame retardant into the reaction kettle, stir them thoroughly to make the components uniform, then add 25 parts of ammonium polyphosphate and 5 parts of cyanuric acid melamine salt, 55° C., high-speed dispersion for 60 minutes, then add 5 parts of basalt, 2 parts of carbon fiber, and 1 part of zirconium-containing ceramic fiber, and stir them at low speed for 50 minutes to obtain component A;

[0062] Comparative Example 5

[0063] The difference between Comparative Example 5 and Example 1 is that step (7) is deleted, and steps (5) and (6) are changed to add 20 parts of polylactic acid-based epoxy resin, 10 parts of acrylic acid-modified epoxy resin, 5 parts of silica sol-modified acrylic resin, and 30 parts of modified flame retardant in the reaction kettle in sequence, stir them thoroughly to make the components uniform, then add 25 parts of ammonium polyphosphate and 5 parts of cyanuric acid melamine salt, disperse at high speed at 55° C. for 60 minutes, then add 5 parts of basalt, 2 parts of carbon fiber, and 1 part of zirconium-containing ceramic fiber, and stir at low speed for 50 minutes; then continue to add 20 parts of cyanuric acid melamine salt, 1 part of talcum powder, and 40 parts of water-based modified amine curing agent in the reaction kettle, keep the water bath temperature at 60° C., stir evenly, add 10 parts of glass fiber and 3 parts of boron fiber, and disperse at high speed for 60 minutes to obtain a fire-retardant water-based coating for interior and exterior walls.

[0064]

[0065]

[0066] From the data comparison of the embodiment and the comparative example, it can be found that the acrylic modified epoxy resin in the modified resin can increase the compatibility of the epoxy resin and the silica sol modified acrylic resin, so that the film-forming material has a high degree of uniformity; the surface hydroxyl groups of the SiO2 sol in the hybrid sol undergo condensation cross-linking reaction with the hydroxyl groups on the organic silicon molecular chain, playing a bridging role between the organic phase and the inorganic phase. This bridging effect enables the silica sol to be evenly dispersed in the acrylic resin, thereby improving the corrosion resistance and durability of the paint film; at the same time, the acrylic group in the modified resin The bond energy of CC and ester groups is much lower than that of the benzene ring structure in the epoxy group. They can soften and break in advance when exposed to fire, which can increase the early expansion of the paint film and form an insulating carbon layer in advance. The introduction of nano-Zn particles can improve the structure of the expanded carbon layer, make the foaming pores small, uniform and dense, extend the fire resistance time, and improve the fire retardant performance of the coating. In addition, the coating is prepared by preparing component A and component B separately and then mixing them, which can avoid premature chemical reactions of the coating and control the mixed mass ratio to achieve the best performance requirements.

[0067] It is obvious to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above, and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be regarded as exemplary and non-restrictive from any point of view, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims are included in the present invention, and no mark in the claims should be regarded as limiting the claims involved.

Claims

1. A method for preparing a fire retardant water-based coating for interior and exterior walls, characterized in that: The method comprises the following preparation steps: (1) Weighing ethyl orthosilicate and ethanol in a container according to the mass ratio, stirring, adding deionized water to dissolve, keeping the temperature in a water bath, adding a catalyst and an organic silane coupling agent, continuously stirring and mixing, condensing and refluxing, and obtaining a uniform nano-silica sol; (2) uniformly mixing an acrylic prepolymer and dibutyl phthalate according to a mass ratio, adding an organic solvent to dissolve, adding nano zinc oxide, continuing to stir, keeping the temperature in a water bath, slowly dropping nano silica sol, raising the temperature after the reaction is complete, performing reduced pressure distillation, removing the organic solvent and water, and obtaining a silica sol-modified acrylic resin; (3) reacting low molecular weight polylactic acid and maleic anhydride in an inert gas atmosphere, controlling the temperature and reaction time, to obtain polylactic acid terminated with carboxyl groups at both ends; (4) dissolving the polylactic acid terminated with carboxyl groups obtained in the previous step in water and an organic solvent, keeping the temperature constant in a water bath, adding a halogenated epoxy compound and an alkaline metal catalyst with stirring, reacting completely, filtering, separating the aqueous phase, adding an alkaline metal catalyst again, and distilling after sufficient reaction to obtain a polylactic acid-based epoxy resin; (5) adding polylactic acid-based epoxy resin, acrylic acid-modified epoxy resin, silica sol-modified acrylic resin and modified flame retardant to a reaction kettle in sequence, stirring them thoroughly to make the components uniform, then adding ammonium polyphosphate and melamine cyanurate, heating and stirring them uniformly, and then adding reinforcing filler and continuing to stir to obtain component A; (6) Add cyanuric acid melamine salt, talcum powder and water-based modified amine curing agent to the reaction container in sequence, keep the temperature in a water bath, stir evenly, add reinforcing fiber, and after the reaction is complete, move to a three-roll mill, grind, and refine the particles to obtain component B; (7) Component A and component B are mixed in a certain mass ratio to prepare a fire retardant water-based coating for interior and exterior walls.

2. The method for preparing a fire retardant water-based paint for interior and exterior walls according to claim 1, characterized in that: In the step (1), the mass ratio of tetraethyl orthosilicate, ethanol, catalyst and organosilane coupling agent is 10-12:20-25:0.1-0.2:0.5-1; the catalyst in the step (1) is hydrochloric acid with a concentration of 0.01M-0.1M; the organosilane coupling agent in the step (1) is KH-570; the water bath temperature in the step (1) is 70-80°C, and the condensation reflux is performed for 3-5h.

3. The method for preparing a fire retardant water-based paint for interior and exterior walls according to claim 1, characterized in that: The acrylic prepolymer in step (2) is obtained by adding azobisisobutyronitrile as an initiator to a mixture of methyl methacrylate and ethyl acrylate; the mass ratio of the acrylic prepolymer, dibutyl phthalate, zinc oxide and silica sol in step (2) is 30-50:20-40:3-5:10-20; the water bath temperature in step (2) is 80°C-100°C, the silica sol is slowly added dropwise, the reaction is carried out for 18h-24h, and then the temperature is raised to 100-120°C and maintained for 2-4h.

4. The method for preparing a fire retardant water-based paint for interior and exterior walls according to claim 1, characterized in that: The molecular weight of the polylactic acid is 10,000 to 100,000; the molar ratio of the polylactic acid to maleic anhydride is 1 to 3:2 to 4; the reaction temperature of the step (3) is 110 to 130° C., and the reaction time is 3 to 5 hours.

5. The method for preparing a fire retardant water-based paint for interior and exterior walls according to claim 1, characterized in that: The halogenated epoxy compound is epichlorohydrin, and the alkaline metal catalyst is a mixture of sodium hydroxide and potassium hydroxide; the molar ratio of the carboxyl-terminated polylactic acid, the alkali metal catalyst, and the halogenated epoxy compound is 3-5:0.6-1.2:8-25; the reaction temperature of step (4) is 30-80°C and the reaction time is 1-4h.

6. The method for preparing a fire retardant water-based paint for interior and exterior walls according to claim 1, characterized in that: In the step (5), there are 20 to 25 parts of lactic acid epoxy resin, 10 to 20 parts of modified resin, 25 to 30 parts of modified flame retardant, 25 to 30 parts of ammonium polyphosphate, 5 to 8 parts of cyanuric acid melamine salt, 3 to 8 parts of reinforcing filler, and 2 to 3 parts of reinforcing fiber; the modified flame retardant is prepared by mixing polyethylene glycol ether and pentaerythritol phosphate, wherein the mass ratio of polyethylene glycol ether to pentaerythritol phosphate is 1 to 3:4 to 8; the reinforcing filler in the step (5) is basalt, and the particle size of the basalt is 300 to 500 meshes; the reinforcing fiber in the step (5) is one or more of zirconium-containing ceramic fiber, carbon fiber, basalt fiber, glass fiber, and boron fiber.

7. The method for preparing a fire retardant water-based paint for interior and exterior walls according to claim 1, characterized in that: In the step (6), 40 to 60 parts of water-based modified amine curing agent, 10 to 15 parts of talcum powder, 15 to 25 parts of melamine cyanurate salt, and 5 to 10 parts of reinforcing fiber are used.

8. The method for preparing a fire retardant water-based paint for interior and exterior walls according to claim 1, characterized in that: The mass ratio of component A to component B is 4 to 6:

1.

9. A fire-retardant water-based paint for interior and exterior walls, characterized in that: The coating is prepared by the method according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • Wear resistant fireproof paint for building interior wall

    CN105017891A

  • Preparation method for polylactic acid-based epoxy resin

    CN107474233A

  • Water-based fireproof coating

    CN115368767A

  • Intumescent fireproof coating and preparation method thereof

    CN116004047A

  • Preparation method of acrylic resin / nano SIQ2 composite paint

    CN1657581A

Cited By

  • Preparation method of anti-cracking nano-composite coating for single-piece non-heat-insulation fireproof glass

    CN119371114A

  • Fireproof corrosion-resistant water-based paint and preparation method thereof

    CN119592155A

  • Efficient intumescent fire retardant coating based on bionic multilayer composite structure and preparation method of efficient intumescent fire retardant coating