Modified radix asparagi polyurea resin anticorrosive paint and preparation method thereof
Through the chemical bonding of isocyanate-modified silicone and asparagus polyurea resin, the problem of poor corrosion resistance of asparagus polyurea resin is solved, and the water resistance, salt spray resistance and impact performance of the coating is improved, which significantly improves its Application effects in anticorrosion coatings.
Patent Information
- Application Number
- CN202411205087.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Asparagus polyurea resin has poor anti-corrosion performance and insufficient wear and impact resistance, which limits its application in anti-corrosion coatings.
Isocyanate modified silicone is used as a curing agent, and hydrogen-addition reaction with hydrogen-containing silicone oil is introduced to form an isocyanate modified silicone curing agent, and chemically bonded with asparagus polyurea resin to improve the The water, salt spray and impact resistance of the paint.
It significantly reduces the surface drying and hard work time of the paint, improves water resistance and salt spray resistance, enhances impact performance, flexibility and wear resistance, and enables the paint to exhibit excellent corrosion resistance.
Smart Images

Figure CN118995015A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of coatings, in particular to a modified asparagine polyurea resin anticorrosive coating and a preparation method thereof. Background Art
[0002] Polyurea has excellent mechanical properties, corrosion resistance, aging resistance and other properties, and is widely used in the field of anticorrosive coatings; among them, polyaspartic acid ester polyurea is called the third generation of new polyurea, which has the characteristics of high gloss, good fullness, excellent surface decoration effect, etc., and has a wide range of application prospects. It is of great significance to improve the wear resistance, softness, impact resistance and other properties of aspartic acid ester polyurea materials. Chinese patent CN111848950B discloses a silicon-modified aspartic acid ester polyurea and its preparation method and application. A primary amine compound is reacted with a maleate compound to obtain an aspartic acid resin, which is then reacted with an organic siloxane to obtain a silicon-modified aspartic acid ester polyurea, which has the advantages of short surface drying time, excellent impact resistance and aging resistance at room temperature and low temperature. However, the preparation method of the silicon-modified aspartic acid ester polyurea of the patent is relatively complicated, and does not show good anticorrosive properties such as water resistance and salt spray resistance, which is not conducive to the practical application of aspartic acid ester polyurea in anticorrosive coatings. The invention uses isocyanate-modified organic silicon as a curing agent for aspartame polyurea, aiming to improve the anti-corrosion, wear resistance, impact resistance and other properties of the aspartame polyurea coating. Summary of the invention
[0003] Technical problem to be solved: The present invention provides a modified asparagus polyurea resin anti-corrosion coating, which solves the problems of poor anti-corrosion performance, poor wear resistance and poor impact resistance of asparagus polyurea resin.
[0004] Technical solution: A modified asparagus polyurea resin anti-corrosion coating, consisting of component A and component B; component A includes 50-60 parts by weight of modified third-generation asparagus polyurea resin, 4-6 parts by weight of active diluent, 1.5-2 parts by weight of additives, 6-9 parts by weight of anti-rust pigments, 15-20 parts by weight of fillers, 0.5-1 parts by weight of polyamide wax thixotropic agent, 8-12 parts by weight of titanium dioxide, and 0.2-0.5 parts by weight of coupling agent.
[0005] Component B is 34-44 parts by weight of isocyanate modified silicone curing agent.
[0006] Furthermore, the auxiliary agent is any one or a combination of a dispersant, a defoamer, and a leveling agent.
[0007] Furthermore, the anti-rust pigment is any one of aluminum tripolyphosphate and strontium chrome yellow.
[0008] Furthermore, the coupling agent is a multi-chain phosphate resin.
[0009] Furthermore, the filler is any one of talc, mica iron oxide, and precipitated barium sulfate.
[0010] Furthermore, the preparation method of the isocyanate-modified silicone curing agent is as follows: 3-isopropenyl-α,α-dimethylbenzyl isocyanate is added to the hydrogen-containing silicone oil, mixed well, and then an isopropanol solution containing chloroplatinic acid is added under a nitrogen atmosphere, and after the reaction, low-boiling substances are removed by reduced pressure distillation to obtain the isocyanate-modified silicone curing agent.
[0011] Furthermore, the mass of 3-isopropenyl-α,α-dimethylbenzyl isocyanate is 20-50% of the mass of the hydrogen-containing silicone oil.
[0012] Furthermore, the reaction temperature is 85-100° C., and the reaction time is 3-6 h.
[0013] Further, the preparation method of the modified asparagus polyurea resin anticorrosive coating is characterized in that 25-30 parts by weight of the modified third generation asparagus polyurea resin, 4-6 parts by weight of active diluent, and 1.5-2 parts by weight of auxiliary agent are added to a container, dispersed at a speed of 800-1000 rpm for 5-10 minutes, and then 8-12 parts by weight of titanium dioxide, 6-9 parts by weight of antirust pigment, 15-20 parts by weight of filler, 0.5-1 parts by weight of polyamide wax thixotropic agent, 1200- Disperse at a speed of 1500rmp for 20-30min; then grind to control the fineness ≦30um, finally add 25-30 parts by weight of modified third-generation asparagus polyurea resin and 0.2-0.5 parts by weight of coupling agent, and disperse at a speed of 800-1000rmp for 5-10min to obtain component A; finally, add 34-44 parts by weight of isocyanate modified silicone curing agent as component B to component A, stir and mix to obtain modified asparagus polyurea resin anti-corrosion coating.
[0014] Technical Effects
[0015] The invention utilizes hydrogen-containing silicone oil and 3-isopropenyl-α,α-dimethylbenzyl isocyanate to undergo a hydrosilylation reaction, thereby introducing an isocyanate group into the side chain of the hydrogen-containing silicone oil to obtain an isocyanate-modified organic silicon curing agent.
[0016] The present invention utilizes isocyanate-modified silicone as a curing agent. The isocyanate-modified silicone has a relatively long molecular chain, and the molecular side chain contains a plurality of isocyanate groups, which can enable the isocyanate groups to quickly come into contact with the asparagine polyurea resin, accelerate the curing reaction, and thus reduce the surface-drying and actual-drying time.
[0017] The present invention uses isocyanate modified silicone as a curing agent to chemically bond the silicone molecular chain to the asparagus polyurea resin cured product. The silicone has strong chemical stability, excellent water resistance, acid and alkali resistance and chemical resistance, which is beneficial to improving the water resistance and salt spray resistance of the coating, so that the coating exhibits good anti-corrosion performance. In addition, the silicone has the characteristics of good toughness and strong wear resistance. Chemically bonding to the asparagus polyurea resin cured product can significantly improve the impact performance, flexibility, tensile performance and wear resistance of the coating. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 This is the preparation reaction mechanism of isocyanate-modified silicone curing agent.
[0019] Figure 2 This is the infrared spectrum of isocyanate modified silicone curing agent. DETAILED DESCRIPTION
[0020] The technical solution of the present invention will be clearly and completely described below in conjunction with specific implementation methods. However, those skilled in the art will understand that the embodiments described below are only part of the embodiments of the present invention, rather than all of the embodiments, and are only used to illustrate the present invention, and should not be regarded as limiting the scope of the present invention.
[0021] The modified third-generation asparagus polyurea resin of the present invention is branded as Covestro NH1520.
[0022] The active diluent is AGE epoxy resin active diluent.
[0023] The titanium dioxide is Meililian 595 rutile titanium dioxide.
[0024] The polyamide wax thixotropic agent is Hemmings 8056 polyamide wax powder.
[0025] The dispersant brand is BYK-346.
[0026] The defoamer brand is RP-6053.
[0027] The leveling agent brand is BYK-306
[0028] The brand of hydrogen-containing silicone oil is TD-2.
[0029] Example 1
[0030] Add 4g of 3-isopropenyl-α,α-dimethylbenzyl isocyanate to 20g of hydrogenated silicone oil, mix well, add 3mL of isopropanol solution containing 4mg of chloroplatinic acid under nitrogen atmosphere, heat to 90℃, react for 6h, remove low-boiling substances by vacuum distillation after the reaction, and obtain isocyanate-modified organosilicon curing agent. Figure 1 Instructions Figure 2In the infrared spectrum, 1169cm -1 It is the characteristic peak of Si-O-Si in hydrogenated silicone oil; 2243cm -1 It is the characteristic peak of -NCO group, 1569cm -1 It is a characteristic peak of the benzene ring, indicating that 3-isopropenyl-α,α-dimethylbenzyl isocyanate is grafted into the hydrogen-containing silicone oil and an isocyanate group is introduced into the side chain of the hydrogen-containing silicone oil.
[0031] Add 250g of modified third-generation asparagus polyurea resin, 4g of active diluent, 5g of dispersant, 8g of defoamer, and 2g of leveling agent into a container, disperse at a speed of 1000rmp for 5min, then add 120g of titanium dioxide, 70g of rust-proof pigment aluminum tripolyphosphate, 200g of filler precipitated barium sulfate, and 7g of polyamide wax thixotropic agent, and disperse at a speed of 1500rmp for 20min; then grind to control the fineness to ≦30um, finally add 250g of modified third-generation asparagus polyurea resin and 5g of coupling agent, disperse at a speed of 800rmp for 8min to obtain component A; finally, add 340g of isocyanate-modified silicone curing agent as component B to component A, stir and mix to obtain a modified asparagus polyurea resin anticorrosive coating.
[0032] Example 2
[0033] To 20 g of hydrogenated silicone oil, add 7 g of 3-isopropenyl-α,α-dimethylbenzyl isocyanate, mix well, add 3 mL of isopropanol solution containing 5 mg of chloroplatinic acid under a nitrogen atmosphere, heat to 100 ° C, react for 3 h, and after the reaction, remove low-boiling substances by reduced pressure distillation to obtain an isocyanate-modified silicone curing agent.
[0034] Add 300g of modified third-generation asparagus polyurea resin, 6g of active diluent, 6g of dispersant, 10g of defoamer, 2g of leveling agent into a container, disperse at a speed of 800rmp for 10min, then add 100g of titanium dioxide, 60g of antirust pigment strontium chrome yellow, 150g of filler talcum powder, 10g of polyamide wax thixotropic agent, and disperse at a speed of 1500rmp for 20min; then grind to control the fineness ≦30um, finally add 300g of modified third-generation asparagus polyurea resin and 5g of coupling agent, disperse at a speed of 800rmp for 10min to obtain component A; finally, add 400g of isocyanate-modified silicone curing agent as component B to component A, stir and mix to obtain a modified asparagus polyurea resin anticorrosive coating.
[0035] Example 3
[0036] To 20 g of hydrogenated silicone oil, add 10 g of 3-isopropenyl-α,α-dimethylbenzyl isocyanate, mix well, add 3 mL of isopropanol solution containing 6 mg of chloroplatinic acid under a nitrogen atmosphere, heat to 85 ° C, react for 4 hours, and after the reaction, remove low-boiling substances by reduced pressure distillation to obtain an isocyanate-modified silicone curing agent.
[0037] Add 300g of modified third-generation asparagus polyurea resin, 6g of active diluent, 7g of dispersant, 10g of defoamer, 3g of leveling agent into a container, disperse at a speed of 800rmp for 10min, then add 80g of titanium dioxide, 90g of antirust pigment strontium chrome yellow, 180g of filler mica iron oxide, 5g of polyamide wax thixotropic agent, and disperse at a speed of 1200rmp for 30min; then grind to control the fineness ≦30um, finally add 300g of modified third-generation asparagus polyurea resin and 2g of coupling agent, disperse at a speed of 800rmp for 10min to obtain component A; finally, add 440g of isocyanate-modified silicone curing agent as component B to component A, stir and mix to obtain a modified asparagus polyurea resin anticorrosive coating.
[0038] Comparative Example 1
[0039] Add 250g of modified third-generation asparagus polyurea resin, 4g of active diluent, 5g of dispersant, 8g of defoamer, and 2g of leveling agent into a container, disperse at a speed of 1000rmp for 5min, then add 120g of titanium dioxide, 70g of rust-proof pigment aluminum tripolyphosphate, 200g of filler precipitated barium sulfate, and 7g of polyamide wax thixotropic agent, and disperse at a speed of 1500rmp for 20min; then grind to control the fineness to ≦30um, finally add 250g of modified third-generation asparagus polyurea resin and 5g of coupling agent, and disperse at a speed of 800rmp for 8min to obtain component A; finally, add 340g of toluene diisocyanate trimer as component B to component A, stir and mix to obtain a modified asparagus polyurea resin anticorrosive coating.
[0040] Comparative Example 2
[0041] 10 g of toluene diisocyanate trimer was added to 20 g of hydrogen-containing silicone oil, and the mixture was blended evenly to obtain a silicone-isocyanate trimer blend.
[0042] Add 250g of modified third-generation asparagus polyurea resin, 4g of active diluent, 5g of dispersant, 8g of defoamer, and 2g of leveling agent into a container, disperse at a speed of 1000rmp for 5min, then add 120g of titanium dioxide, 70g of rust-proof pigment aluminum tripolyphosphate, 200g of filler precipitated barium sulfate, and 7g of polyamide wax thixotropic agent, and disperse at a speed of 1500rmp for 20min; then grind to control the fineness to be ≦30um, finally add 250g of modified third-generation asparagus polyurea resin and 5g of coupling agent, and disperse at a speed of 800rmp for 8min to obtain component A; finally, add 340g of component B silicone-isocyanate trimer blend to component A, stir and mix to obtain a modified asparagus polyurea resin anticorrosive coating.
[0043] Using tinplate as the substrate, the paint was sprayed on the surface of the tinplate by high-pressure airless spraying method and cured at room temperature. The surface drying and through drying time of the paint film were tested according to the method of GB / T 1728-2020.
[0044] The abrasive properties of the paint film were tested according to the method of GB / T 1768-2006, with a grinding wheel load of 1kg and a wear time of 1000h to measure the mass loss. The lower the mass loss, the better the wear resistance.
[0045] The water resistance of the paint film was tested according to the method of GB / T 9274-1988 (Method A).
[0046] The salt spray resistance of the paint film was tested according to the method of GB / T 1771-2007 (scratch method).
[0047] The impact performance of the paint film is tested according to the method of GB / T 1732-2020.
[0048] The flexibility of the paint film was tested according to the method of GB / T 1731-2020.
[0049] The tensile properties were tested according to the method of GBT 16777-2008.
[0050] Table 1 Test of surface drying and through drying time of coatings.
[0051] Surface drying time (min) Drying time (min) Example 1 40 435 Example 2 35 420 Example 3 35 425 Comparative Example 1 45 460 Comparative Example 2 50 475
[0052] After testing, in Comparative Example 1, conventional toluene diisocyanate trimer was used as a curing agent, and the surface drying and thorough drying times of the coating were 45 minutes and 460 minutes.
[0053] In Examples 1-3, isocyanate-modified silicone is used as a curing agent, and the surface-drying and through-drying time of the coating are significantly reduced to only 35-45 minutes and 420-435 minutes. This is because the isocyanate-modified silicone has a longer molecular chain and the molecular side chain contains multiple isocyanate groups, which can make the isocyanate groups quickly contact with the asparagine polyurea resin, accelerate the curing reaction, and thus reduce the surface-drying and through-drying time.
[0054] In Comparative Example 2, hydrogen-containing silicone oil and toluene diisocyanate trimer are physically blended, and no isocyanate group is introduced into the side chain of the hydrogen-containing silicone oil. The curing reaction is only carried out by toluene diisocyanate trimer and asparagine polyurea resin, which does not accelerate the curing reaction and does not reduce the surface drying and actual drying time.
[0055] Table 2 Water resistance and salt spray resistance test of coatings
[0056] Water resistance (360h) Salt spray resistance (7200h) Example 1 No blistering, no peeling, no cracks No blistering, no peeling, no cracks Example 2 No blistering, no peeling, no cracks No blistering, no peeling, no cracks Example 3 No blistering, no peeling, no cracks No blistering, no peeling, no cracks Comparative Example 1 No blistering, no peeling, no cracks No blistering, peeling or cracking Comparative Example 2 No blistering, no peeling, no cracks No blistering, no peeling, no cracks
[0057] Table 3 Mechanical properties test of coatings
[0058]
[0059] After testing, Examples 1-3 use isocyanate-modified silicone as a curing agent to chemically bond silicone molecular chains to the asparagus polyurea resin cured product. Silicone has strong chemical stability, excellent water resistance, acid and alkali resistance, and chemical resistance, which is beneficial to improving the water resistance and salt spray resistance of the coating, and making the coating exhibit good anti-corrosion performance. In addition, silicone has the characteristics of good toughness and strong wear resistance. Chemical bonding to the asparagus polyurea resin cured product can significantly improve the impact performance, flexibility, tensile performance, and wear resistance of the coating.
[0060] Comparative Example 1 uses toluene diisocyanate trimer as a curing agent and does not contain a silicone molecular chain. The coating has poor water resistance and salt spray resistance. At the same time, the coating has poor flexibility, tensile strength, wear resistance and other properties.
[0061] Comparative Example 2 physically blends hydrogen-containing silicone oil and toluene diisocyanate trimer, but does not introduce isocyanate groups into the side chains of hydrogen-containing silicone oil, making it impossible to chemically bond the organic silicon molecular chain to the asparagine polyurea resin cured product, and thus failing to improve the water resistance and salt spray resistance of the coating. In addition, the coating has poor flexibility, tensile strength, and wear resistance.
[0062] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A modified asparagus polyurea resin anticorrosive coating, characterized in that: It consists of component A and component B; component A includes 50-60 parts by weight of modified third-generation asparagine polyurea resin, 4-6 parts by weight of active diluent, 1.5-2 parts by weight of auxiliary agent, 6-9 parts by weight of anti-rust pigment, 15-20 parts by weight of filler, 0.5-1 parts by weight of polyamide wax thixotropic agent, 8-12 parts by weight of titanium dioxide, and 0.2-0.5 parts by weight of coupling agent; Component B is 34-44 parts by weight of isocyanate modified silicone curing agent.
2. The modified asparagus polyurea resin anticorrosive coating according to claim 1, characterized in that: The auxiliary agent is any one or a combination of a dispersant, a defoamer and a leveling agent.
3. The modified asparagus polyurea resin anticorrosive coating according to claim 1, characterized in that: The anti-rust pigment is any one of aluminum tripolyphosphate and strontium chrome yellow.
4. The modified asparagus polyurea resin anticorrosive coating according to claim 1, characterized in that: The coupling agent is a multi-chain phosphate resin.
5. The modified asparagus polyurea resin anticorrosive coating according to claim 1, characterized in that: The filler is any one of talc powder, mica iron oxide and precipitated barium sulfate.
6. The modified asparagus polyurea resin anticorrosive coating according to claim 1, characterized in that: The preparation method of the isocyanate-modified organic silicon curing agent comprises the following steps: adding 3-isopropenyl-α,α-dimethylbenzyl isocyanate to hydrogenated silicone oil, mixing well, adding an isopropanol solution containing chloroplatinic acid under a nitrogen atmosphere, and removing low-boiling substances by reduced pressure distillation after the reaction to obtain the isocyanate-modified organic silicon curing agent.
7. The modified asparagus polyurea resin anticorrosive coating according to claim 6, characterized in that: The mass of the 3-isopropenyl-α,α-dimethylbenzyl isocyanate is 20-50% of the mass of the hydrogen-containing silicone oil.
8. The modified asparagus polyurea resin anticorrosive coating according to claim 6, characterized in that: The reaction temperature is 85-100° C., and the reaction time is 3-6 hours.
9. A method for preparing the modified asparagus polyurea resin anticorrosive coating according to any one of claims 1 to 8, characterized in that: Add 25-30 parts by weight of modified third-generation asparagus polyurea resin, 4-6 parts by weight of active diluent, 1.5-2 parts by weight of auxiliary agent into a container, disperse at a speed of 800-1000 rpm for 5-10 min, then add 8-12 parts by weight of titanium dioxide, 6-9 parts by weight of antirust pigment, 15-20 parts by weight of filler, 0.5-1 parts by weight of polyamide wax thixotropic agent, disperse at a speed of 1200-1500 rpm for 20-30 min; then grind to control the fineness to be less than 30 um, finally add 25-30 parts by weight of modified third-generation asparagus polyurea resin and 0.2-0.5 parts by weight of coupling agent, disperse at a speed of 800-1000 rpm for 5-10 min to obtain component A; finally add 34-44 parts by weight of isocyanate-modified silicone curing agent as component A, stir and mix to obtain modified asparagus polyurea resin anticorrosive coating.
Citation Information
Patent Citations
A silicon-modified aspartic acid ester polyurea, its preparation method and application
CN111848950B
Method for synthesizing tri(3-trimethoxy silicon propyl) isocyanurate through addition process
CN109824715A
Method for preparing isocyanate-based silane by hydrosilylation reaction
CN110128465A
Preparation method of self-repairing carbonyl modified thermoplastic polyurea elastomer
CN114853976A
Solvent-free polyaspartate polyurea coating and preparation method thereof
CN115820099A
Cited By
Water-based anticorrosive finish paint, preparation method and application thereof, and oil casing
CN120192700A
A water-based anti-corrosion topcoat and its preparation method and application, oil casing
CN120192700B