Concrete anti-freezing and anti-carbonization protective layer of sandwich-like structure and preparation method of concrete anti-freezing and anti-carbonization protective layer
Through the concrete protective layer with a sandwich-like structure and the multi-layer design of silane functionalization treatment, the shortcomings of the concrete protective layer in the existing technology in complex environments are solved, and more efficient anti-freeze-thaw and carbonization properties are achieved, and the performance of simplification is achieved. The construction process has significantly extended the service life of the concrete structure.
Patent Information
- Application Number
- CN202411331741.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-24
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-09-24
AI Technical Summary
Existing concrete protective layers are insufficient in dealing with complex environmental erosion, especially in improving freeze-thaw and carbonization resistance, as well as ensuring long-term stability and simplifying construction processes.
Concrete anti-freeze-thaw and carbonization-resistant protective layer using sandwich-like structure, including poly(dimethylsiloxane)urea resin modified with silane functionalized fluorinated carbon, and intermediate layer modified with silane functionalized montmorillonite. Poly(dimethylsiloxane)urea resin and the bottom layer are polyol modified poly(dimethylsiloxane)urea resin. The interface bonding performance is optimized through the multi-layer functional structure design, so as to achieve surface waterproofing, middle layer barrier and bottom layer enhancement. The synergistic effect of bonding.
It significantly improves the anti-freeze and thaw properties of concrete and the resistance to carbonization, extends the service life of the structure, provides multiple protection mechanisms, is suitable for new construction and repair structures, and simplifies construction processes and reduces costs and energy consumption.
Smart Images

Figure CN118995037A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a concrete anti-freezing and anti-carbonization protective layer with a sandwich structure and a preparation method thereof, belonging to the technical field of concrete protection. Background Art
[0002] As one of the most widely used building materials, the durability of concrete has always been the focus of attention in the engineering community. In harsh environments, concrete structures face severe challenges such as freeze-thaw cycles and carbonization, which can cause a sharp decline in concrete performance and seriously affect the service life and safety of the structure. At present, the commonly used concrete protection methods mainly include surface coating, impregnation, and admixture addition. However, these methods often have many technical difficulties, such as the difficulty of a single coating protection mechanism in coping with complex environmental erosion, and the serious lack of interfacial bonding between the existing protective layer and the concrete substrate. In addition, the compatibility and long-term stability between the components of the multi-level protective layer are greatly limited, and the construction process is extremely complicated. Therefore, in view of these technical difficulties, it is urgent to develop a new type of concrete protective layer with multiple protection mechanisms, good interface bonding, high component compatibility, long-term stability and easy construction. Summary of the invention
[0003] Technical problem: The present invention aims to address the shortcomings of existing concrete protective layers in dealing with complex environmental erosion, especially in improving the freeze-thaw and carbonation resistance of concrete structures, ensuring long-term stability and simplifying construction processes. The present invention aims to provide a concrete freeze-thaw and carbonation resistance layer with a sandwich-like structure. The protective layer achieves comprehensive protection through a multi-layer functional structural design, optimizes interface bonding performance, achieves a synergistic effect of surface waterproofing, middle layer barrier and bottom layer enhanced bonding, ensures the long-term stability of the concrete protective layer, and at the same time develops a simple and efficient construction process for concrete protection technology, significantly improving the freeze-thaw resistance and carbonation resistance of concrete foundation structures, and providing a new technical solution for the protection of concrete structures.
[0004] Technical solution:
[0005] The present invention aims to address the shortcomings of existing concrete surface protection technology under conditions where freeze-thaw and carbonization coexist, and proposes a concrete anti-freeze-thaw and anti-carbonization protective layer with a sandwich-like structure and a preparation method thereof. The characteristic of the present invention is that the sandwich structure of the concrete anti-freeze-thaw and anti-carbonization protective layer comprises the following three layers: a surface layer is a silane-functionalized fluorinated carbon modified poly (dimethylsiloxane) urea resin layer, a middle layer is a silane-functionalized montmorillonite modified poly (dimethylsiloxane) urea resin layer, and a bottom layer is a polyol-modified poly (dimethylsiloxane) urea resin layer.
[0006] The preparation method of the poly(dimethylsiloxane)urea resin comprises: the preparation method of the poly(dimethylsiloxane)urea resin comprises: mixing amino-terminated polydimethylsiloxane and dicyclohexylmethane 4,4'-diisocyanate in an N'N-dimethylformamide solvent at a molar ratio of 1:2, and keeping the mixed system stirred at 0°C for 1-2 hours, then slowly adding an equal amount of polyether diamine chain extender to the mixture, continuing the reaction for 1-2 hours, then adding an appropriate amount of end-capping agent and continuing stirring for 30 minutes, and after the reaction is completed, pouring the product into a preheated mold, curing at 80-90°C for 6-8 hours, and then post-curing at room temperature for 48-72 hours to obtain a poly(dimethylsiloxane)urea resin, the molecular structure of which is as follows:
[0007]
[0008] Wherein R represents a polyether segment.
[0009] The surface layer is a poly(dimethylsiloxane)urea resin layer modified by silane functionalized fluorinated carbon, which is prepared by mixing and compounding silane functionalized nano-fluorinated carbon and poly(dimethylsiloxane)urea resin, and the mass ratio of the two is set in the range of 1% to 6%, preferably 3%.
[0010] The preparation method of silane-functionalized nano-carbon fluoride comprises: dispersing carbon fluoride in an organic solvent at a weight percentage of 0.1 to 1, and ultrasonically treating for 30 to 60 minutes to form a uniform dispersion; then adding 3 to 5 weight percentages of silane to the dispersion, and then stirring the mixture at 60±5° C. for 4 to 6 hours; centrifuging the reaction product, and washing it three times with ethanol and deionized water; and finally vacuum drying the washed product at 60° C. for 12 hours to obtain silane-functionalized nano-carbon fluoride;
[0011] Preferably, the nano-carbon fluoride includes one or a combination of two or more of nano-carbon tetrafluoride, nano-carbon hexafluoride or nano-carbon octafluoride; preferably, the organic solvent is one or a combination of two or more of ethanol, isopropanol, tetrahydrofuran or toluene; preferably, the silane coupling agent is one or a combination of two or more of γ-aminopropyltriethoxysilane, γ-glycidyloxypropyltrimethoxysilane or vinyltrimethoxysilane.
[0012] The intermediate layer is a poly(dimethylsiloxane)urea resin layer modified by silane functionalized montmorillonite, which is prepared by mixing and compounding silane functionalized montmorillonite and poly(dimethylsiloxane)urea resin, and the mass ratio of the two is set in the range of 1% to 6%, preferably 3%; the preparation method of the silane functionalized montmorillonite comprises: dispersing 5 to 10 parts by weight of montmorillonite powder in 95 to 90 parts by weight of anhydrous ethanol, and ultrasonically treating for 30 to 60 minutes to form a uniform dispersion; adding 1 to 3 parts by weight of γ-aminopropyltriethoxysilane to the dispersion, and stirring and reacting at 60±5°C for 4 to 6 hours; centrifuging the reaction product, washing it with anhydrous ethanol for 3 to 5 times, and centrifuging it after each washing; and vacuum drying the washed product at 80°C for 12 to 24 hours to obtain the silane functionalized montmorillonite.
[0013] The bottom layer is a polyol-modified poly(dimethylsiloxane) urea resin layer prepared by stirring and mixing a polyol and a poly(dimethylsiloxane) urea resin at 60-70° C. for 2-3 hours; the mass percentage of the polyol and the poly(dimethylsiloxane) urea resin is 2%-5%; the polyol is one or a combination of two or more of glycerol, pentaerythritol and sorbitol.
[0014] The method for preparing the concrete anti-freezing and anti-carbonization protective layer is characterized in that the preparation steps include:
[0015] The polyol-modified poly(dimethylsiloxane) urea resin is sprayed on the pretreated concrete surface with a thickness of 100-150 μm, and pre-cured at room temperature for 2-4 hours. Then, the silane-functionalized montmorillonite-modified poly(dimethylsiloxane) urea resin composite is sprayed on the bottom layer with a thickness of 150-200 μm, and pre-cured at room temperature for 2-4 hours. Subsequently, the silane-functionalized fluorinated carbon-modified poly(dimethylsiloxane) urea resin composite is sprayed on the middle layer with a thickness of 150-200 μm. Finally, the coated three-layer structure is cured at room temperature for 24 hours, thereby obtaining a concrete anti-freeze-thaw and anti-carbonization protective layer with a sandwich-like structure. The total thickness of the concrete anti-freeze-thaw and anti-carbonization protective layer is 300-550 μm.
[0016] The present invention provides a concrete anti-freezing and anti-carbonization protective layer with a sandwich-like structure prepared by the above method and its application in the technical field of improving concrete durability.
[0017] Compared with the prior art, the present invention has the following beneficial effects:
[0018] 1) A sandwich-like structure design is adopted, in which each layer has different functions, and the synergistic effect improves the overall performance of the protective layer; Silane functionalization treatment improves the compatibility of fluorinated carbon and montmorillonite with poly (dimethylsiloxane) urea resin, and enhances the overall performance of the composite material;
[0019] 2) The silane-functionalized fluorinated carbon and poly (dimethylsiloxane) urea resin are compounded to design the concrete protective surface layer, which improves the hydrophobicity and weather resistance of the surface resin and can effectively prevent the penetration of moisture and harmful substances;
[0020] 3) Using silane-functionalized montmorillonite and poly(dimethylsiloxane) urea resin as the middle layer of the sandwich structure improves the sealing barrier performance of the coating and further enhances the barrier effect against harmful substances such as carbon dioxide and chloride ions;
[0021] 4) Based on the polyol-modified poly(dimethylsiloxane) urea resin as the bottom layer of the sandwich structure, the hydroxyl groups inside the resin network coordinate with the metal ions of the concrete matrix, thereby enhancing the adhesion between the coating and the concrete, and improving the adhesion and durability of the entire protective layer;
[0022] 5) All three layers use poly (dimethylsiloxane) urea resin as the matrix, which ensures the compatibility and bonding between the layers and avoids the problem of interlayer peeling.
[0023] 6) The protective layer has excellent freeze-thaw resistance and good anti-carbonation performance, which can effectively reduce the damage of freeze-thaw cycles to concrete, significantly delay the carbonization process of concrete, and extend the service life of the structure.
[0024] 7) The multi-layer structure design provides multiple protections. Even if the surface layer is partially damaged, the lower layer can continue to play a protective role. This protective layer is not only suitable for new concrete structures, but can also be used for the repair and reinforcement of existing structures. This method is simple to construct, low in cost, low in energy consumption, and green and environmentally friendly, and has broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 Schematic diagram of the sandwich structure of the interface between the concrete anti-freeze-thaw and anti-carbonation protective layers. DETAILED DESCRIPTION
[0026] Embodiment 1:
[0027] The steps for preparing a concrete anti-freezing and anti-carbonization protective layer with a sandwich-like structure are as follows:
[0028] Preparation of poly(dimethylsiloxane) urea resin: 100 g of amino-terminated polydimethylsiloxane (molecular weight of about 2000) was mixed with 84 g of dicyclohexylmethane 4,4'-diisocyanate in 200 mL of N'N-dimethylformamide solvent, and the mixed system was stirred at 0°C for 1.5 h, and then 100 g of polyetherdiamine (molecular weight of about 1000) was slowly added to the mixture, and the reaction was continued for 1.5 h, and then 10 g of n-butanol capping agent was added and stirred for 30 min. After the reaction was completed, the product was poured into a preheated mold, cured at 85°C for 7 h, and then post-cured at room temperature for 60 h to obtain poly(dimethylsiloxane) urea resin.
[0029] Preparation of silane-functionalized nano-carbon tetrafluoride: 1 g of nano-carbon tetrafluoride (particle size of about 50 nm) was dispersed in 100 ml of anhydrous ethanol and ultrasonically treated for 45 min to form a uniform dispersion; 4 g of γ-aminopropyltriethoxysilane was then added to the dispersion, and the mixture was stirred and reacted at 65° C. for 5 h; the reaction product was centrifuged and washed with ethanol and deionized water for 3 times; finally, the washed product was vacuum dried at 60° C. for 12 h to obtain silane-functionalized nano-carbon fluoride;
[0030] Preparation of silane functionalized montmorillonite: 7 g of montmorillonite powder was dispersed in 93 g of anhydrous ethanol and ultrasonically treated for 45 min to form a uniform dispersion; 2 g of γ-aminopropyltriethoxysilane was added to the dispersion and stirred for reaction at 65° C. for 5 h; the reaction product was centrifuged and washed with anhydrous ethanol for 4 times, and centrifuged after each washing; the washed product was vacuum dried at 80° C. for 18 h to obtain silane functionalized montmorillonite.
[0031] Preparation of each layer of resin: 1) Bottom layer: 3g glycerol and 97g poly(dimethylsiloxane) urea resin were stirred and mixed at 65°C for 2.5h. 2) Middle layer: 3g silane-functionalized montmorillonite and 97g poly(dimethylsiloxane) urea resin were stirred and mixed at room temperature for 4h. 3) Surface layer: 0.5g silane-functionalized nano-tetrafluorocarbon and 99.5g poly(dimethylsiloxane) urea resin were stirred and mixed at room temperature for 4h.
[0032] Preparation of protective layer: 1) Grind the surface of the concrete test block (100mm×100mm×100mm), clean it with acetone, and dry it for 24 hours; 2) Use high-pressure airless spraying equipment to spray the base layer resin on the concrete surface and pre-cure it at room temperature for 3 hours; 3) Spray the middle layer resin on the base layer and pre-cure it at room temperature for 3 hours; 4) Spray the surface layer resin on the middle layer; 5) Cure the coated three-layer structure at room temperature for 24 hours to obtain a protective layer with a total thickness of 400μm.
[0033] Performance test: 1) Compression strength test: According to GB / T 50081-2002. 2) Dynamic elastic modulus test: According to ASTM C215-14. 3) Freeze-thaw cycle test: According to GB / T 50082-2009, a total of 300 cycles. 4) Carbonization test: Accelerated carbonization for 60 days in an environment of 20±2℃, relative humidity 65±5%, CO2 concentration 20±3%.
[0034] The test results are as follows:
[0035] ① Compressive strength: decreased by 7.5% after freeze-thaw cycles and decreased by 5.8% after carbonization;
[0036] ② Dynamic elastic modulus: decreased by 11% after freeze-thaw cycles and decreased by 8.5% after carbonization;
[0037] ③Mass loss: 0.7% after freeze-thaw cycle, 0.3% after carbonization;
[0038] ④Surface hardness (Shore hardness): decreased by 5.5% after freeze-thaw cycles and decreased by 4% after carbonization.
[0039] Embodiment 2:
[0040] The steps for preparing a concrete anti-freezing and anti-carbonization protective layer with a sandwich-like structure are as follows:
[0041] The preparation steps of poly(dimethylsiloxane) urea resin are the same as those in Example 1.
[0042] Preparation of silane-functionalized nano carbon hexafluoride: 1.6 g of nano carbon hexafluoride (particle size of about 40 nm) was dispersed in 100 mL of anhydrous ethanol and ultrasonically treated for 50 min to form a uniform dispersion; 4.5 g of γ-aminopropyltriethoxysilane was then added to the dispersion, and the mixture was stirred and reacted at 65° C. for 5 h; the reaction product was centrifuged and washed with ethanol and deionized water for 3 times; finally, the washed product was vacuum dried at 60° C. for 12 h to obtain silane-functionalized nano carbon hexafluoride;
[0043] Preparation of silane functionalized montmorillonite: 8 g of montmorillonite powder was dispersed in 92 g of anhydrous ethanol and ultrasonically treated for 45 min to form a uniform dispersion; 2.5 g of γ-aminopropyltriethoxysilane was added to the dispersion and stirred for reaction at 65° C. for 5 h; the reaction product was centrifuged and washed with anhydrous ethanol for 4 times, and centrifuged after each washing; the washed product was vacuum dried at 80° C. for 18 h to obtain silane functionalized montmorillonite.
[0044] Preparation of each layer of resin: 1) Bottom layer: 4g of pentaerythritol and 96g of poly(dimethylsiloxane)urea resin were stirred and mixed at 65°C for 2.5h. 2) Middle layer: 4g of silane-functionalized montmorillonite and 96g of poly(dimethylsiloxane)urea resin were stirred and mixed at room temperature for 4h. 3) Surface layer: 0.8g of silane-functionalized nano-carbon hexafluoride and 99.2g of poly(dimethylsiloxane)urea resin were stirred and mixed at room temperature for 4h.
[0045] Preparation of protective layer: 1) Grind the surface of the concrete test block (100mm×100mm×100mm), clean it with acetone, and dry it for 24 hours; 2) Use high-pressure airless spraying equipment to spray the base layer resin on the concrete surface and pre-cure it at room temperature for 3 hours; 3) Spray the middle layer resin on the base layer and pre-cure it at room temperature for 3 hours; 4) Spray the surface layer resin on the middle layer; 5) Cure the coated three-layer structure at room temperature for 24 hours to obtain a protective layer with a total thickness of 450μm.
[0046] Performance test: Same as Example 1.
[0047] The test results are as follows:
[0048] ① Compressive strength: decreased by 6.8% after freeze-thaw cycles and decreased by 5.2% after carbonization;
[0049] ② Dynamic elastic modulus: decreased by 10% after freeze-thaw cycles and decreased by 7.8% after carbonization;
[0050] ③Mass loss: 0.65% after freeze-thaw cycle, 0.28% after carbonization;
[0051] ④Surface hardness (Shore hardness): decreased by 5% after freeze-thaw cycles and decreased by 3.7% after carbonization.
[0052] Embodiment 3:
[0053] The steps for preparing a concrete anti-freezing and anti-carbonization protective layer with a sandwich-like structure are as follows:
[0054] The preparation steps of poly(dimethylsiloxane) urea resin are the same as those in Example 1.
[0055] Preparation of silane-functionalized nano carbon octafluoride: 0.6 g of nano carbon octafluoride (particle size of about 60 nm) was dispersed in 100 mL of anhydrous ethanol and ultrasonically treated for 50 min to form a uniform dispersion; 4.5 g of γ-aminopropyltriethoxysilane was then added to the dispersion, and the mixture was stirred and reacted at 65° C. for 5 h; the reaction product was centrifuged and washed with ethanol and deionized water for 3 times; finally, the washed product was vacuum dried at 60° C. for 12 h to obtain silane-functionalized nano carbon octafluoride;
[0056] Preparation of silane functionalized montmorillonite: 10 g of montmorillonite powder was dispersed in 92 g of anhydrous ethanol and ultrasonically treated for 45 min to form a uniform dispersion; 3 g of γ-aminopropyltriethoxysilane was added to the dispersion and stirred for reaction at 65° C. for 5 h; the reaction product was centrifuged and washed with anhydrous ethanol for 4 times, and centrifuged after each washing; the washed product was vacuum dried at 80° C. for 18 h to obtain silane functionalized montmorillonite.
[0057] Preparation of each layer of resin: 1) Bottom layer: 4g sorbitol and 98g poly(dimethylsiloxane) urea resin were stirred and mixed at 65°C for 2.5h. 2) Middle layer: 5g silane-functionalized montmorillonite and 95g poly(dimethylsiloxane) urea resin were stirred and mixed at room temperature for 4h. 3) Surface layer: 0.3g silane-functionalized nano-octafluorocarbon and 99.7g poly(dimethylsiloxane) urea resin were stirred and mixed at room temperature for 4h.
[0058] Preparation of protective layer: 1) Grind the surface of the concrete test block (100mm×100mm×100mm), clean it with acetone, and dry it for 24 hours; 2) Use high-pressure airless spraying equipment to spray the base layer resin on the concrete surface and pre-cure it at room temperature for 3 hours; 3) Spray the middle layer resin on the base layer and pre-cure it at room temperature for 3 hours; 4) Spray the surface layer resin on the middle layer; 5) Cure the coated three-layer structure at room temperature for 24 hours to obtain a protective layer with a total thickness of 350μm.
[0059] Performance test: Same as Example 1.
[0060] The test results are as follows:
[0061] ① Compressive strength: decreased by 6.8% after freeze-thaw cycles and decreased by 5.2% after carbonization;
[0062] ② Dynamic elastic modulus: decreased by 10% after freeze-thaw cycles and decreased by 7.8% after carbonization;
[0063] ③Mass loss: 0.65% after freeze-thaw cycle, 0.28% after carbonization;
[0064] ④Surface hardness (Shore hardness): decreased by 5% after freeze-thaw cycles and decreased by 3.7% after carbonization.
[0065] Comparative Example:
[0066] Preparation of poly(dimethylsiloxane)urea resin: Same as Example 1.
[0067] Preparation of protective layer: 1) The surface of the concrete specimen (100mm×100mm×100mm) was polished and cleaned with acetone, and dried for 24 hours; 2) Poly(dimethylsiloxane) urea resin was sprayed directly on the concrete surface using high-pressure airless spraying equipment with a thickness of 350μm; 3) The coated structure was cured at room temperature for 24 hours to obtain a single-layer protective layer with a total thickness of 400μm.
[0068] Performance test: Same as Example 1.
[0069] The test results are as follows:
[0070] ① Compressive strength: decreased by 18% after freeze-thaw cycles and decreased by 14% after carbonization;
[0071] ② Dynamic elastic modulus: decreased by 25% after freeze-thaw cycles and decreased by 20% after carbonization;
[0072] ③Mass loss: 2.2% after freeze-thaw cycle, 1.5% after carbonization;
[0073] ④Surface hardness (Shore hardness): decreases by 15% after freeze-thaw cycles and decreases by 12% after carbonization.
[0074] In summary, the concrete anti-freeze-thaw and anti-carbonization protective layer with a sandwich-like structure proposed by the present invention is significantly better than a single-layer poly(dimethylsiloxane) urea resin protective layer. In all test indicators, the sandwich-like protective layer shows better performance, and by adjusting the composition and thickness of each layer, the performance of the protective layer can be further optimized to meet different environmental and application requirements.
[0075] The above-described embodiments are only for the purpose of explaining the technical solution of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may be subject to various modifications and variations. Any modification, equivalent substitution, improvement, etc. made within the spirit and principle of the present invention shall be within the scope of the claims of the present invention.
Claims
1. A sandwich-like concrete anti-freezing and anti-carbonization protective layer, characterized in that: The sandwich structure of the concrete anti-freezing and anti-carbonation protective layer includes the following three layers: the surface layer is a silane-functionalized fluorinated carbon modified poly (dimethylsiloxane) urea resin layer, the middle layer is a silane-functionalized montmorillonite modified poly (dimethylsiloxane) urea resin layer, and the bottom layer is a polyol modified poly (dimethylsiloxane) urea resin layer.
2. The concrete anti-freeze-thaw and anti-carbonization protective layer according to claim 1, characterized in that: The preparation method of the poly(dimethylsiloxane)urea resin comprises: mixing amino-terminated polydimethylsiloxane and dicyclohexylmethane 4,4'-diisocyanate in a N'N-dimethylformamide solvent at a molar ratio of 1:2, and keeping the mixed system stirred at 0°C for 1-2 hours, then adding an equal amount of polyether diamine chain extender to the mixture, continuing the reaction for 1-2 hours, then adding a blocking agent and continuing stirring, and after the reaction is completed, pouring the product into a preheated mold, curing at 80-90°C for 6-8 hours, and then post-curing at room temperature for 48-72 hours to obtain a poly(dimethylsiloxane)urea resin, the molecular structure of which is as follows: Wherein R represents a polyether segment.
3. The concrete anti-freeze-thaw and anti-carbonization protective layer according to claim 1, characterized in that: The surface layer is prepared by mixing and compounding silane-functionalized nano-carbon fluoride and poly(dimethylsiloxane) urea resin; The preparation method of silane-modified nano-carbon fluoride comprises: dispersing carbon fluoride in an organic solvent at a weight percentage of 0.1 to 1, and ultrasonically treating for 30 to 60 minutes to form a uniform dispersion; then adding 3 to 5 weight percentages of a silane coupling agent to the dispersion, and then stirring the mixture at 60±5° C. for 4 to 6 hours; centrifuging the reaction product, and washing it three times with ethanol and deionized water; and finally drying the washed product to obtain the silane-modified nano-carbon fluoride.
4. The concrete anti-freeze-thaw and anti-carbonization protective layer according to claim 3 is characterized by: The mass ratio of the silane functionalized nano-carbon fluoride to the poly(dimethylsiloxane)urea resin is 1% to 6%.
5. The concrete anti-freezing and anti-carbonization protective layer according to claim 3 is characterized by: The nano carbon fluoride includes one or a combination of two or more of nano carbon tetrafluoride, nano carbon hexafluoride or nano carbon octafluoride; the organic solvent is one or a combination of two or more of ethanol, isopropanol, tetrahydrofuran or toluene; the silane coupling agent is one or a combination of two or more of γ-aminopropyltriethoxysilane, γ-glycidyloxypropyltrimethoxysilane or vinyltrimethoxysilane.
6. The concrete anti-freezing and anti-carbonization protective layer according to claim 1, characterized in that: The intermediate layer is a poly(dimethylsiloxane)urea resin layer modified by silane functionalized montmorillonite, which is prepared by mixing and compounding silane modified montmorillonite and poly(dimethylsiloxane)urea resin; the preparation method of the silane modified montmorillonite comprises: dispersing 5 to 10 parts by weight of montmorillonite powder in 95 to 90 parts by weight of anhydrous ethanol, ultrasonically treating for 30 to 60 minutes to form a uniform dispersion; adding 1 to 3 parts by weight of γ-aminopropyltriethoxysilane to the dispersion, stirring and reacting at 60±5°C for 4 to 6 hours; centrifuging the reaction product, washing it with anhydrous ethanol for 3 to 5 times, and centrifuging it after each washing; and vacuum drying the washed product at 80°C for 12 to 24 hours to obtain silane functionalized montmorillonite.
7. The concrete anti-freezing and anti-carbonization protective layer according to claim 6, characterized in that: The mass ratio of the silane-modified montmorillonite to the poly(dimethylsiloxane)urea resin is 1% to 6%.
8. The concrete anti-freeze-thaw and anti-carbonization protective layer according to claim 1, characterized in that: The bottom layer is a polyol-modified poly(dimethylsiloxane) urea resin layer prepared by stirring and mixing a polyol and a poly(dimethylsiloxane) urea resin at 60-70° C. for 2-3 hours; the mass percentage of the polyol and the poly(dimethylsiloxane) urea resin is 2%-5%; the polyol is one or a combination of two or more of glycerol, pentaerythritol and sorbitol.
9. The method for preparing a concrete anti-freezing and anti-carbonization protective layer according to claims 1 to 8, characterized in that: The preparation steps include: The polyol-modified poly(dimethylsiloxane) urea resin is sprayed on the pretreated concrete surface with a thickness of 100-150 μm, and pre-cured at room temperature for 2-4 hours. The silane-functionalized montmorillonite-modified poly(dimethylsiloxane) urea resin composite is then sprayed on the bottom layer with a thickness of 150-200 μm, and pre-cured at room temperature for 2-4 hours. Subsequently, the silane-functionalized fluorinated carbon-modified poly(dimethylsiloxane) urea resin composite is sprayed on the middle layer with a thickness of 150-200 μm. Finally, the coated three-layer structure is cured at room temperature to obtain a concrete anti-freeze-thaw and anti-carbonization protective layer with a sandwich-like structure. The total thickness of the concrete anti-freeze-thaw and anti-carbonization protective layer is 300-550 μm.
10. Use of the protective layer with a sandwich-like structure according to any one of claims 1 to 8 in the technical field of improving concrete durability.
Citation Information
Patent Citations
Transparent protective coat for concrete
CN103881496A
Amino-modified nano boron carbide reinforced polyurea composite material as well as preparation method and application thereof
CN117645784A
Anti-freeze-thaw beautified marked polyaspartic protective material applied to pumped storage power station and preparation method of anti-freeze-thaw beautified marked polyaspartic protective material
CN118620501A
A reinforced concrete base member protective coating for villaumite erosion environment
CN204874314U
Corrosion prevention method for concrete and concrete structure prepared by the corrosion prevention method
JP2011020891A