Suspended emulsion for fracturing fluid and preparation method thereof

Through the suspension emulsion for fracturing fluid of specific combination formulas, the problem of insufficient dissolution speed and stability of suspension emulsion in the prior art is solved, rapid dissolution and long-term stability are achieved, damage to the reservoir is reduced, and continuous The demand for mixed and large displacement construction.

CN118995177AActive Publication Date: 2024-11-22SINOPEC OILFIELD SERVICE CORPORATION +2

Patent Information

Application Number
CN202310577908.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-22
Publication Date
2024-11-22
Estimated Expiration
2043-05-22

AI Technical Summary

Technical Problem

The existing suspension emulsions have shortcomings in dissolution speed and stability, which cannot meet the needs of continuous mixing and large displacement construction, and cause great damage to the reservoir.

Method used

Using specific combination formulas, including white oil, polyacrylamide or guanidine gel thickening agent, non-ionic emulsifier, bentonite, polysaccharide suspension and silicate dispersants, the density is prepared by high-speed stirring. Suspended emulsion for fracturing fluid with a viscosity of 0.95-0.97g/cm3 and a viscosity of 350-500mPa·s is used to reduce the amount of bentonite to reduce the damage to the reservoir.

Benefits of technology

The suspension emulsion for fracturing liquid has achieved good suspension stability, with fast dissolution speed, ready-to-use and no residual liquid, reducing transportation and tank cleaning fees, reducing damage to reservoirs, polyacrylamide and plant glue The damage rate of suspension emulsion to reservoirs is less than 10%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_3
    Figure SMS_3
  • Figure SMS_4
    Figure SMS_4
Patent Text Reader

Abstract

The invention provides a suspension emulsion for a fracturing fluid. The suspension emulsion comprises 40-60 parts by weight of white oil; 30-60 parts by weight of a thickening agent; 1-5 parts by weight of a nonionic emulsifier; 1-3 parts by weight of bentonite; 0.5-2 parts by weight of a suspending agent; 0.5-2 parts by weight of a dispersant; and 0.1 to 1.2 parts by weight of a cosolvent. Compared with the prior art, the suspension emulsion for the fracturing fluid, provided by the invention, is good in suspension stability and high in swelling speed, can be prepared and injected immediately on site, is free of residual liquid, avoids waste of the fracturing fluid, and reduces transportation cost, tank cleaning cost and the like at the same time; and the use amount of bentonite is reduced, so that the damage to the reservoir is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of oilfield chemistry, and in particular relates to a suspension emulsion for fracturing fluid and a preparation method thereof. Background Art

[0002] Hydraulic fracturing technology is a conventional measure to increase the production of oil and gas layers. The thickeners that can be used for hydraulic fracturing are divided into three types: powder, invert emulsion and suspended emulsion. However, the dissolution time of powder thickeners (polyacrylamide, plant gum, etc.) is too long, the timeliness is poor, it is easy to produce dust pollution, and it is easy to produce "fish eyes" during the dissolution process, which cannot meet the requirements of continuous mixing and large-volume construction at the fracturing site; although the dissolution time of invert emulsion thickeners is short, the effective content of thickeners (polyacrylamide) is low, and the product quality is difficult to control, resulting in poor stability; the suspended emulsion system has a high solid content, a relatively fast swelling rate, and no waste liquid residue, which can be used for continuous mixing on site, but the existing suspended emulsions generally do not exceed 2 months. The phenomenon of stratification and bottom deposition and hardening has poor stability, and the dissolution rate is about 30 to 60s, and the rapid mixing effect on site is not ideal. Therefore, a suspended emulsion with good stability and fast dissolution rate is needed for continuous mixing and large-volume construction of fracturing fluid thickeners.

[0003] Therefore, how to improve the suspension stability and dissolution rate of the suspension emulsion thickener to meet the requirements of the continuous mixing "ready-to-mix and inject" fracturing process is one of the problems that technicians in this field need to solve urgently. Summary of the invention

[0004] In view of this, the technical problem to be solved by the present invention is to provide a suspension emulsion for fracturing fluid with good suspension stability, quick dissolution performance and low damage to reservoirs and a preparation method thereof.

[0005] The present invention provides a suspension emulsion for fracturing fluid, comprising:

[0006]

[0007]

[0008] Preferably, the particle size of the thickener is 100-150 μm; and the dispersant is a single-layer flaky structure.

[0009] Preferably, the thickener is selected from polyacrylamide thickeners and / or guar gum thickeners;

[0010] The nonionic emulsifier is a polyoxyethylene ether emulsifier;

[0011] The suspending agent is a polysaccharide suspending agent;

[0012] The dispersant is selected from silicate dispersants and / or aluminosilicate dispersants;

[0013] The cosolvent is a small molecule alcohol.

[0014] Preferably, the white oil is selected from one or more of 3# white oil, 5# white oil, 7# white oil, 10# white oil, 15# white oil, 20# white oil, 22# white oil, 26# white oil and 32# white oil;

[0015] The thickener is selected from one or more of polyacrylamide thickeners, carboxymethyl guar gum, hydroxypropyl guar gum and carboxymethyl hydroxypropyl guar gum;

[0016] The nonionic emulsifier is selected from one or more of fatty alcohol polyoxyethylene ether, cocamide polyoxyethylene ether, Tween 80, coconut oil polyoxyethylene ether, isomeric tridecyl alcohol polyoxyethylene ether and polyoxypropylene polyoxyethylene propylene glycol ether;

[0017] The bentonite is selected from sodium bentonite and / or calcium bentonite;

[0018] The suspending agent is selected from one or more of carboxymethyl cellulose, hydroxypropyl cellulose, sodium hydroxypropyl methyl cellulose and maltodextrin;

[0019] The dispersant is selected from one or more of sodium aluminosilicate, sodium silicate, magnesium aluminum silicate, magnesium hexasilicate and sodium metasilicate pentahydrate;

[0020] The co-solvent is selected from one or more of methanol, ethanol, ethylene glycol, propylene glycol, glycerol and isopropanol.

[0021] Preferably, including:

[0022]

[0023] Preferably, the density of the suspension emulsion for fracturing fluid is 0.95-0.97 g / cm 3 .

[0024] Preferably, the bulk viscosity of the suspension emulsion for fracturing fluid is 350-500 mPa·s.

[0025] Preferably, the viscosity of the fracturing fluid suspension emulsion after stirring for 15 to 30 seconds is more than 80% of the final viscosity.

[0026] The present invention also provides a method for preparing a suspension emulsion for fracturing fluid, comprising:

[0027] The white oil, thickener, nonionic emulsifier, bentonite, suspending agent, dispersant and co-solvent are mixed and stirred at high speed to obtain a suspension emulsion for fracturing fluid.

[0028] Preferably, the mixing speed is 200-2000 r / min; the high-speed stirring speed is 2000-8000 r / min; the high-speed stirring time is 20-100 min; and the high-speed stirring temperature is 10°C-80°C.

[0029] The present invention provides a suspension emulsion for fracturing fluid, comprising: 40-60 parts by weight of white oil; 30-60 parts by weight of thickener; 1-5 parts by weight of nonionic emulsifier; 1-3 parts by weight of bentonite; 0.5-2 parts by weight of suspending agent; 0.5-2 parts by weight of dispersant; and 0.1-1.2 parts by weight of cosolvent. Compared with the prior art, the suspension emulsion for fracturing fluid provided by the present invention has good suspension stability and fast swelling speed, can be prepared and injected on site, has no residual liquid, avoids waste of fracturing fluid, and reduces transportation costs, tank cleaning costs, etc.; and reduces damage to reservoirs by reducing the amount of bentonite used.

[0030] Experimental results show that the suspension emulsion for fracturing fluid provided by the present invention is left to stand for 6 months without stratification, sedimentation or hardening, and the performance of the suspension emulsion is not affected; the viscosity of the polyacrylamide suspension emulsion can reach more than 80% of the final viscosity after stirring for 15 seconds and the plant gum emulsion for 30 seconds, and the mixture can be prepared and injected immediately on site without residual liquid, thereby avoiding waste of fracturing fluid and reducing transportation costs, tank cleaning costs, etc.; by reducing the amount of bentonite used, the damage of the suspension emulsion to the reservoir is reduced, and the damage rates of the polyacrylamide suspension emulsion and the plant gum suspension emulsion to the reservoir are both less than 10%. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 This is a state diagram of the suspension emulsion prepared in Examples 1 to 3 of the present invention after being placed for 6 months;

[0032] Figure 2 The state diagram of the suspension emulsion prepared in Examples 4 and 5 of the present invention after being placed for 6 months. DETAILED DESCRIPTION

[0033] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0034] The present invention provides a suspension emulsion for fracturing fluid, comprising:

[0035]

[0036] The present invention uses white oil as a dispersing medium of a thickener; the content of the white oil in the suspension emulsion for fracturing fluid is preferably 40 to 55 parts by weight, more preferably 43 to 53 parts by weight; in the embodiment provided by the present invention, the content of white oil in the suspension emulsion for fracturing fluid is specifically 52.8 parts by weight, 48 parts by weight or 43.4 parts by weight; the type of the white oil is preferably one or more of 3# white oil, 5# white oil, 7# white oil, 10# white oil, 15# white oil, 20# white oil, 22# white oil, 26# white oil and 32# white oil, more preferably two of 3# white oil, 5# white oil, 26# white oil and 32# white oil or one of 7# white oil, 10# white oil and 15# white oil. The present invention selects a specific white oil to increase the density of the white oil (solvent) as much as possible while ensuring that the viscosity of the emulsion is moderate, thereby achieving a better suspension stability effect.

[0037] The thickener is an effective component of the suspension emulsion for fracturing fluid, which is used to increase the viscosity of the fracturing fluid and bring the proppant into the formation during the fracturing construction process; the thickener is preferably a polyacrylamide thickener and / or a guar gum thickener, and more preferably one or more of a polyacrylamide thickener, carboxymethyl guar gum, hydroxypropyl guar gum and carboxymethyl hydroxypropyl guar gum; in the present invention, the suspension emulsion for fracturing fluid can be divided into polyacrylamide suspension emulsion and plant gum suspension emulsion according to the type of thickener; the thickener is a dry powder thickener with a particle size of 100 to 150 μm; the content of the thickener in the suspension emulsion for fracturing fluid is preferably 35 to 55 parts by weight, and more preferably 40 to 50 parts by weight.

[0038] The fracturing fluid suspension emulsion provided by the present invention is added with a non-ionic emulsifier, which can be adsorbed on the surface of the thickener dry powder particles to form a layer of emulsifier molecules, so that each small particle can be stably dispersed and suspended in the medium; the type of the non-ionic emulsifier is preferably a polyoxyethylene ether emulsifier, and more preferably one or more of fatty alcohol polyoxyethylene ether, coconut acid amide polyoxyethylene ether, Tween 80, coconut oil polyoxyethylene ether, isomeric tridecyl alcohol polyoxyethylene ether and polyoxypropylene polyoxyethylene glycol ether; the content of the non-ionic emulsifier in the fracturing fluid suspension emulsion is preferably 1.5 to 4 parts by weight, more preferably 2 to 4 parts by weight, and more preferably 2 to 3 parts by weight; in the embodiments provided by the present invention, the content of the fracturing fluid suspension emulsion is specifically 3 parts by weight, 2.6 parts by weight or 2 parts by weight.

[0039] Bentonite can enhance the thixotropy and suspension of the suspension emulsion system for fracturing fluid, making the system more stable in temperature resistance, shear resistance and suspension performance; the bentonite is preferably sodium-based bentonite and / or calcium-based bentonite; the content of the bentonite in the suspension emulsion for fracturing fluid is preferably 1.5 to 2.5 parts by weight, more preferably 1.8 to 2 parts by weight; in the embodiment provided by the present invention, the content of the bentonite in the suspension emulsion for fracturing fluid is specifically 1.8 parts by weight.

[0040] The suspending agent in the suspoemulsion for fracturing fluid provided by the present invention is preferably a polysaccharide suspending agent, more preferably one or more of carboxymethyl cellulose, hydroxypropyl cellulose, sodium hydroxypropyl methylcellulose and maltodextrin; the content of the suspending agent in the suspoemulsion for fracturing fluid is preferably 0.5 to 1.5 parts by weight, more preferably 0.8 to 1.2 parts by weight, and even more preferably 1 part by weight.

[0041] The dispersant in the suspension emulsion for fracturing fluid provided by the present invention is preferably a single-layer flaky structure. Compared with the curled or overlapping structure, the spread-out single-layer structure has the characteristic of larger interlayer spacing, which can separate the suspended particles layer by layer, so that the thickener dry powder is evenly dispersed in the white oil solvent, effectively inhibiting the thickener from settling and agglomerating, and achieving a better suspension stabilization effect. In the present invention, the type of the dispersant is preferably a silicate dispersant and / or an aluminosilicate dispersant, more preferably one or more of sodium aluminosilicate, sodium silicate, magnesium aluminum silicate, magnesium hexasilicate and sodium metasilicate pentahydrate; the content of the dispersant in the suspension emulsion for fracturing fluid is preferably 0.5 to 1.5 parts by weight, more preferably 0.8 to 1.2 parts by weight, and more preferably 1 part by weight.

[0042] The cosolvent in the suspension emulsion for fracturing fluid provided by the present invention is preferably a small molecule alcohol. The addition of the small molecule alcohol can make the thickener dry powder slightly swell, prepare for dissolution in the later preparation of fracturing fluid, accelerate the dissolution rate of the suspension emulsion, and also increase / adjust the viscosity of the emulsion to achieve a better suspension effect. The cosolvent is more preferably one or more of methanol, ethanol, ethylene glycol, propylene glycol, glycerol and isopropanol; the content of the cosolvent in the suspension emulsion for fracturing fluid is preferably 0.2 to 1 parts by weight, more preferably 0.4 to 0.8 parts by weight.

[0043] According to the present invention, further preferably, the suspension emulsion for fracturing fluid comprises:

[0044]

[0045]

[0046] The density of the suspension emulsion for fracturing fluid provided by the present invention is preferably 0.95 to 0.97 g / cm 3Its density and state vary slightly depending on the type and content of the thickener. When the thickener is 40% polyacrylamide thickener, the fracturing fluid suspension emulsion is a milky white viscous liquid with a density of 0.957 g / cm 3 When the thickener is 40% guar gum thickener, the fracturing fluid suspension emulsion is a khaki viscous liquid with a density of preferably 0.966 g / cm 3 .

[0047] The bulk viscosity of the suspension emulsion for fracturing fluid provided by the present invention is preferably 350 to 500 mPa·s, and can be adjusted within this range.

[0048] The viscosity of the suspension emulsion for fracturing fluid provided by the present invention after stirring for 15 to 30 seconds is preferably more than 80% of the final viscosity.

[0049] The suspension emulsion for fracturing fluid provided by the present invention has good suspension stability and fast swelling speed, can be prepared and injected immediately on site, has no residual liquid, avoids waste of fracturing fluid, and reduces transportation costs, tank cleaning costs, etc.; and reduces damage to reservoirs by reducing the amount of bentonite used.

[0050] The present invention also provides a method for preparing the above-mentioned suspension emulsion for fracturing fluid, comprising: mixing white oil, thickener, nonionic emulsifier, bentonite, suspending agent, dispersant and co-solvent and stirring at high speed to obtain the suspension emulsion for fracturing fluid.

[0051] The present invention has no special restrictions on the sources of all raw materials, and any raw materials available on the market can be used; the white oil, thickener, nonionic emulsifier, bentonite, suspending agent, dispersant and cosolvent are the same as those described above and will not be described in detail here.

[0052] The white oil, thickener, nonionic emulsifier, bentonite, suspending agent, dispersant and co-solvent are mixed; the mixing speed is preferably 200-2000 r / min, more preferably 500-1500 r / min, and even more preferably 700-1100 r / min; the mixing is preferably carried out in a reactor.

[0053] After mixing, high-speed stirring is performed to obtain a suspended emulsion for fracturing fluid; the rotation speed of the high-speed stirring is preferably 2000-8000 r / min, more preferably 2000-7000 r / min, and more preferably 3000-6000 r / min; the time of the high-speed stirring is preferably 20-100 min, more preferably 30-70 min, and more preferably 30-60 min; the temperature of the high-speed stirring is preferably 10°C-80°C, more preferably 20°C-70°C, and more preferably 25°C-50°C.

[0054] The polymer suspension emulsion and guar gum suspension emulsion provided by the present invention have the characteristics of fast dissolution speed (less than 15 seconds) and long stable period (more than 6 months). In the continuous mixing and large-volume construction, they can be prepared and injected on site as thickeners, effectively avoiding the costs of liquid preparation, transportation, tank cleaning, etc. caused by early liquid preparation.

[0055] In order to further illustrate the present invention, the following describes in detail a suspension emulsion for fracturing fluid and a preparation method thereof in conjunction with embodiments.

[0056] The reagents used in the following examples are all commercially available. The white oil (3#, 5#, 7#, 10#, 15#, 26#, 32#) used in the examples is provided by Shandong Taichang Petrochemical Technology Co., Ltd., bentonite (sodium-based) is provided by Lingshou County Yiran Mineral Products Processing Plant, emulsifier (coconut oil polyoxyethylene ether 26L, isomeric tridecanol polyoxyethylene ether E-1303) is provided by Jiangsu Hai'an Petrochemical Plant, suspending agent (hydroxypropyl methylcellulose sodium HPMC) is provided by North Chemical Co., Ltd., dispersant (sodium silicate, sodium metasilicate pentahydrate) is provided by Shandong Duofeng Chemical Co., Ltd., cosolvent (glycerol, ethylene glycol, ethanol), polyacrylamide powder (anion C powder) is provided by Aisen Aisen (China) Flocculant Co., Ltd.; carboxymethyl hydroxypropyl guar gum powder and hydroxypropyl guar gum powder are provided by Beijing Baofengchun Petroleum Technology Co., Ltd., and the above raw materials are all commercially available industrial products; the particle size of the thickener powder used in the examples is 100 to 200 meshes.

[0057] Example 1

[0058] The components of the polymer suspension emulsion are: in parts by weight, 52.8 parts of white oil, 40 parts of thickener dry powder, 1.8 parts of bentonite, 3 parts of emulsifier, 1 part of suspending agent, 1 part of dispersant, and 0.4 parts of cosolvent; the white oil includes 30 parts of 3# white oil, 22.6 parts of 32# white oil, the thickener dry powder is polyacrylamide, the bentonite is sodium bentonite, the emulsifier is coconut oil polyoxyethylene ether, the suspending agent is sodium hydroxypropyl methylcellulose, the dispersant is sodium silicate, and the cosolvent is glycerol.

[0059] The preparation method is as follows: place 3# white oil and 32# white oil in a beaker, set the speed to 700r / min, add bentonite, emulsifier, suspending agent, dispersant, cosolvent, and dry powder in sequence, continue stirring at 3000r / min and 50°C for 50min, and obtain a polyacrylamide suspension emulsion with an effective content of 40%.

[0060] Example 2

[0061] The components of the polymer suspension emulsion are: in parts by weight, 48 parts of white oil, 45 parts of thickener dry powder, 1.8 parts of bentonite, 2.6 parts of emulsifier, 1 part of suspending agent, 1 part of dispersant, and 0.6 part of cosolvent; the white oil includes 24 parts of 5# white oil, 24 parts of 26# white oil, the thickener dry powder is polyacrylamide, the bentonite is sodium bentonite, the emulsifier is coconut oil polyoxyethylene ether, the suspending agent is sodium hydroxypropyl methylcellulose, the dispersant is sodium silicate, and the cosolvent is ethylene glycol.

[0062] The preparation method is as follows: place 5# white oil and 26# white oil in a beaker, set the speed to 800r / min, add bentonite, emulsifier, suspending agent, dispersant, cosolvent, and dry powder in sequence, continue stirring at 4000r / min and 40°C for 40 minutes, and obtain a polyacrylamide suspension emulsion with an effective content of 45%.

[0063] Example 3

[0064] The components of the polymer suspension emulsion are: in parts by weight, 43.4 parts of white oil, 50 parts of thickener dry powder, 1.8 parts of bentonite, 2 parts of emulsifier, 1 part of suspending agent, 1 part of dispersant, and 0.8 part of cosolvent; the white oil includes 30 parts of 7# white oil, 13.4 parts of 26# white oil, the thickener dry powder is polyacrylamide, the bentonite is sodium bentonite, the emulsifier is isomeric tridecyl alcohol polyoxyethylene ether, the suspending agent is sodium hydroxypropyl methylcellulose, the dispersant is sodium metasilicate pentahydrate, and the cosolvent is ethanol.

[0065] The preparation method is as follows: place white oil in a beaker, set the speed to 900r / min, add bentonite, emulsifier, suspending agent, dispersant, cosolvent, and dry powder in sequence, continue stirring at 6000r / min and 25°C for 30min, and obtain a polyacrylamide suspension emulsion with a 50% effective content.

[0066] Example 4

[0067] Guar gum suspension emulsion components: in parts by weight, 52.8 parts of white oil, 40 parts of thickener dry powder, 1.8 parts of bentonite, 3 parts of emulsifier, 1 part of suspending agent, 1 part of dispersant, and 0.4 parts of cosolvent; the white oil is 10# white oil, the thickener dry powder is carboxymethyl hydroxypropyl guar gum, the bentonite is sodium bentonite, the emulsifier is isomeric tridecyl alcohol polyoxyethylene ether, the suspending agent is sodium hydroxypropyl methylcellulose, the dispersant is sodium silicate, and the cosolvent is ethanol.

[0068] The preparation method is as follows: white oil is placed in a beaker, the rotation speed is set to 1000 r / min, bentonite, emulsifier, suspending agent, dispersant, cosolvent, and thickener dry powder are added in sequence, and stirring is continued at 3500 r / min and 45° C. for 35 minutes to obtain a carboxymethyl hydroxypropyl guar gum suspension emulsion with an effective content of 40%.

[0069] Example 5

[0070] The components of the guar gum suspension emulsion are, in parts by weight, 43.4 parts of white oil, 50 parts of thickener dry powder, 1.8 parts of bentonite, 2 parts of emulsifier, 1 part of suspending agent, 1 part of dispersant, and 0.8 part of cosolvent; the white oil is 15# white oil, the thickener dry powder is hydroxypropyl guar gum, the bentonite is sodium bentonite, the emulsifier is isomeric tridecyl alcohol polyoxyethylene ether, the suspending agent is sodium hydroxypropyl methylcellulose, the dispersant is sodium metasilicate pentahydrate, and the cosolvent is glycerol.

[0071] The preparation method is as follows: white oil is placed in a beaker, the rotation speed is set to 1100 r / min, bentonite, emulsifier, suspending agent, dispersant, cosolvent, and thickener dry powder are added in sequence, and stirring is continued at 4000 r / min and 30° C. for 40 minutes to obtain a hydroxypropyl guar gum suspension emulsion with an effective content of 50%.

[0072] Performance testing:

[0073] (1) Swelling rate test

[0074] Test method: Take 350mL of 20℃ clean water and add it to the mixer measuring cup, adjust the mixer speed to 1700r / min, add the calculated amount of thickener, start timing, stop stirring after 20s, pour the liquid into the six-speed viscosity measuring cup within 10s and put it into the six-speed viscometer for measurement, record the apparent viscosity of the solution at 0.5min, 1min, 2min, and 3min at 100r / min, and compare it with the apparent viscosity at 4h to calculate the swelling rate.

[0075] Table 1 Viscosity and swelling rate test of polyacrylamide suspension emulsion

[0076]

[0077] Table 2 Viscosity and swelling rate test of guar gum suspension emulsion

[0078]

[0079] (2) Suspension stability test: After standing for 6 months, observe whether the suspension emulsion product has delamination ≤5%, and there is no sedimentation or hardening at the bottom, which is considered qualified. Figure 1 , Figure 2 As shown, Figure 1 From left to right in the figure are the states of the suspension emulsions prepared in Examples 1, 2, and 3 after being placed for 6 months. Figure 2 From left to right in the figure are the states of the suspension emulsions prepared in Examples 4 and 5 after being placed for 6 months. It can be seen that the suspension emulsions are still stable after being placed for 6 months, with basically no stratification, and have almost no difference in appearance from the suspension emulsion just prepared, reflecting good suspension stability.

[0080] (3) Harm test: The matrix permeability damage rate of the suspension emulsion was tested according to the standard SY / T 5107-2016 "Water-based fracturing fluid performance evaluation method", and the results are shown in Table 3. It can be seen that the matrix permeability damage rate of the suspension emulsion prepared by this method is low, and it belongs to a low-damage fracturing fluid.

[0081] Table 3 Test results of matrix permeability damage rate of suspension emulsion

[0082]

[0083] In summary, the present invention provides a new method for preparing a suspension emulsion, which has the advantages of fast dissolution speed, good suspension performance and low cost, and meets the technical requirements of large-volume hydraulic fracturing construction with continuous mixing.

[0084] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A suspension emulsion for fracturing fluid, It is characterized in that include:

2. The suspension emulsion for fracturing fluid according to claim 1, It is characterized in that The particle size of the thickener is 100-150 μm; the dispersant is a single-layer flake structure.

3. The suspension emulsion for fracturing fluid according to claim 1, It is characterized in that The thickener is selected from polyacrylamide thickeners and / or guar gum thickeners; The nonionic emulsifier is a polyoxyethylene ether emulsifier; The suspending agent is a polysaccharide suspending agent; The dispersant is selected from silicate dispersants and / or aluminosilicate dispersants; The cosolvent is a small molecule alcohol.

4. The suspension emulsion for fracturing fluid according to claim 1, It is characterized in that The white oil is selected from one or more of 3# white oil, 5# white oil, 7# white oil, 10# white oil, 15# white oil, 20# white oil, 22# white oil, 26# white oil and 32# white oil; The thickener is selected from one or more of polyacrylamide thickeners, carboxymethyl guar gum, hydroxypropyl guar gum and carboxymethyl hydroxypropyl guar gum; The nonionic emulsifier is selected from one or more of fatty alcohol polyoxyethylene ether, cocamide polyoxyethylene ether, Tween 80, coconut oil polyoxyethylene ether, isomeric tridecyl alcohol polyoxyethylene ether and polyoxypropylene polyoxyethylene propylene glycol ether; The bentonite is selected from sodium bentonite and / or calcium bentonite; The suspending agent is selected from one or more of carboxymethyl cellulose, hydroxypropyl cellulose, sodium hydroxypropyl methyl cellulose and maltodextrin; The dispersant is selected from one or more of sodium aluminosilicate, sodium silicate, magnesium aluminum silicate, magnesium hexasilicate and sodium metasilicate pentahydrate; The co-solvent is selected from one or more of methanol, ethanol, ethylene glycol, propylene glycol, glycerol and isopropanol.

5. The suspension emulsion for fracturing fluid according to claim 1, It is characterized in that include:

6. The suspension emulsion for fracturing fluid according to claim 1, It is characterized in that The density of the suspension emulsion for fracturing fluid is 0.95-0.97 g / cm 3 .

7. The suspension emulsion for fracturing fluid according to claim 1, It is characterized in that The bulk viscosity of the suspension emulsion for fracturing fluid is 350-500 mPa·s.

8. The suspension emulsion for fracturing fluid according to claim 1, It is characterized in that The viscosity of the fracturing fluid suspension emulsion after stirring for 15 to 30 seconds is more than 80% of the final viscosity.

9. A method for preparing a suspension emulsion for fracturing fluid, It is characterized in that include: The white oil, thickener, nonionic emulsifier, bentonite, suspending agent, dispersant and co-solvent are mixed and stirred at high speed to obtain a suspension emulsion for fracturing fluid.

10. The preparation method according to claim 9, It is characterized in that The mixing speed is 200-2000 r / min; the high-speed stirring speed is 2000-8000 r / min; the high-speed stirring time is 20-100 min; the high-speed stirring temperature is 10° C.-80° C.

Citation Information

Patent Citations

  • Biopolymer thickener as well as preparation method and application thereof

    CN111961440A

  • Polymer suspension emulsion for fracturing fluid and preparation method thereof

    CN112175208A

  • Thickening agent suspension emulsion for fracturing fluid and preparation method thereof

    CN113355079A

  • Functional composite thickening agent for integrated fracturing process

    CN113549442A

  • Hydrophobic association polyacrylamide suspension emulsion for fracturing and preparation method thereof

    CN114456795A

Cited By

  • High-salt-tolerance solid-phase-free long-acting suspension drag reducer system and preparation method thereof

    CN122542216A