Control process for trace elements of tire cord steel
By strictly controlling raw materials and smelting parameters in cord steel production and using impurity removal and additive technology, the problem of trace elements control is solved, and the element content in cord steel is effectively reduced and product quality is improved.
Patent Information
- Application Number
- CN202311797055.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-25
- Publication Date
- 2024-11-22
AI Technical Summary
During the production process of cord steel, it is difficult to effectively control the content of trace elements, resulting in the presence of inclusions affecting product quality.
By strictly selecting and screening raw materials, controlling the smelting temperature and atmosphere, using impurity removal processes and additives to adsorb, separate or convert trace elements, including alkaline flux desulfurization, deoxygenation and degassing of steel slag and adding sodium borate or sodium chloride, etc. , ensure effective removal of trace elements.
It realizes effective control of trace elements in cord steel, ensures product quality, achieves low content of sulfur, oxygen, vanadium, aluminum and other elements, and improves the purity and service life of the product.
Smart Images

Figure CN118996230A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of cord steel smelting, in particular to a cord steel trace element control process. Background Art
[0002] Steel cord is a special-purpose fine steel strand or rope made of high-quality high-carbon steel with brass coating on the surface. It is mainly used for car tires, light truck tires, heavy truck tires, construction machinery tires, aircraft tires and other rubber product skeleton materials. The radial tire made of steel cord as reinforcement material has the advantages of long service life, high driving speed, puncture resistance, good elasticity, safety and comfort, and fuel saving.
[0003] When the cord steel is drawn into 100km filaments, breakage is not allowed. Therefore, all production processes of cord steel have strict requirements, among which the control of inclusions is the key. The main source of inclusions is the harmful elements in the steel. Therefore, every link in the production and smelting process must be controlled and no mistakes are allowed. The control of harmful elements has become the key to smelting cord steel. For this reason, we propose a trace element control process for cord steel. Summary of the invention
[0004] The object of the present invention is to provide a trace element control process for cord steel to solve the problems raised in the above background technology.
[0005] To achieve the above object, the present invention provides the following technical solution: a cord steel trace element control process, the cord steel trace element control process comprising the following steps:
[0006] Step 1: Raw material selection. Before smelting, the raw materials are strictly screened and controlled to ensure that the trace element content in the raw materials is low. This can be achieved by carefully selecting raw materials such as ore and scrap steel, and using chemical analysis instruments to test the raw materials.
[0007] Step 2: Put the raw materials into the smelting furnace, control the smelting temperature, atmosphere and material addition parameters, so as to minimize the content of trace elements. Higher temperature helps to reduce the solid solubility of elements, so that trace elements are easier to separate. By controlling the smelting temperature, the trace elements can be fully dissolved and evenly distributed;
[0008] Step 3: Impurity removal: During the smelting process, an impurity removal process is required to remove trace elements to ensure the quality of the cord steel after forming;
[0009] Step 4: Adding additives: During the smelting process, some special additives are added to the raw materials to adsorb, separate or convert trace elements.
[0010] Preferably, in step 2, the amount of oxygen blown in is controlled to increase so as to increase the oxidation reaction rate during the smelting process, thereby achieving the effect of reducing the content of trace elements.
[0011] Preferably, the impurity removal process in step 3 comprises the following steps:
[0012] S1. Reduce sulfur content by alkaline flux desulfurization, prepare alkaline flux, determine suitable alkaline flux, such as calcium, magnesium, etc., calculate and prepare enough flux according to furnace capacity and desulfurization requirements, add flux to the furnace, and evenly add the pre-prepared alkaline flux to the furnace during smelting;
[0013] S2. Use a stirring device or gas stirring to mix and stir them, which can ensure that the flux and the molten metal in the furnace are fully mixed and contacted;
[0014] S3. In molten metal, alkaline flux will react with sulfide to generate sulfide that is insoluble in metal. Sulfide will precipitate or float on the metal surface and then be removed or fished out, thereby reducing the sulfur content in the metal.
[0015] S4. Monitor the desulfurization reaction in real time and determine the desulfurization effect through chemical analysis or online monitoring instruments.
[0016] 6. Preferably, the impurity removal process in step 3 further comprises: using steelmaking slag for deoxidation and degassing, and using steelmaking slag for deoxidation and degassing comprises the following steps:
[0017] S1. Prepare steelmaking slag. Steelmaking slag is usually obtained from limestone and other auxiliary materials (such as coke, etc.) through a smelting process. Prepare enough steelmaking slag and ensure that it meets the deoxidation requirements.
[0018] S2, adding steelmaking slag, and evenly putting the steelmaking slag on the surface of the molten steel to make it fully contact with the molten steel;
[0019] S3, reaction and deoxidation. At high temperature, steelmaking slag will react with oxygen in molten steel to form gas (such as CO, CO2, etc.) and discharge it. At the same time, oxygen in steelmaking slag will also react with other non-metallic elements (such as silicon, manganese, etc.) in molten steel to achieve the effect of deoxidation and degassing.
[0020] S4. Stirring and mixing: Use stirring devices or gas stirring to ensure that the steelmaking slag and molten steel are fully mixed and in contact.
[0021] S5. Monitoring and adjustment: monitor the deoxidation and degassing process in real time, determine the deoxidation effect through chemical analysis or online monitoring instruments, and adjust the amount of steelmaking slag added, stirring intensity, etc. according to the monitoring results to achieve the expected deoxidation effect.
[0022] Preferably, the additive in step 4 is sodium borate to reduce the vanadium content, and the specific steps are as follows:
[0023] S1. Prepare sodium borate by dissolving an appropriate amount of sodium borate solid in sufficient water to prepare a sodium borate solution;
[0024] S2. Prepare steel materials: prepare the cord steel sample to be processed, which may be powdered steel materials or block steel materials;
[0025] S3, adding sodium borate solution, slowly adding the sodium borate solution into the cord steel sample, and ensuring sufficient mixing by stirring or other means;
[0026] S4, smelting: the mixed cord steel sample is smelted, and a suitable smelting method can be selected, such as electric arc furnace smelting;
[0027] S5, filtering and cooling, filtering and cooling the smelted molten liquid to separate the solid residue and the cooled liquid;
[0028] S6, separating the waste residue, and treating the separated solid waste residue, which can be recycled or incinerated;
[0029] S7. Extracting pure cord steel. Extracting pure cord steel from the cooled liquid can be purified by filtering, precipitation, concentration, etc.
[0030] S8. Detect the vanadium content. Detect the vanadium content of the extracted pure cord steel sample. Appropriate chemical analysis methods or instruments can be used for determination.
[0031] Preferably, the additive in step 4 is sodium chloride added during the smelting of cord steel to adsorb and remove alumina, and the specific steps are as follows:
[0032] S1. Prepare a sodium chloride solution by dissolving an appropriate amount of sodium chloride solid in sufficient water to prepare a sodium chloride solution;
[0033] S2. Prepare steel materials, and prepare the cord steel samples to be processed;
[0034] S3, adding sodium chloride solution, and slowly adding the sodium chloride solution into the cord steel sample;
[0035] S4. Smelting: Smelting the mixed cord steel sample. A suitable smelting method may be selected, such as electric arc furnace smelting or other methods;
[0036] S5, filtering and cooling, filtering and cooling the smelted molten liquid to separate the solid residue and the cooled liquid;
[0037] S6, separating the waste residue, and treating the separated solid waste residue, which can be recycled or incinerated;
[0038] S7. Extracting pure cord steel. Extracting pure cord steel from the cooled liquid can be purified by filtering, precipitation, concentration, etc.
[0039] S8. Detect the alumina content. Detect the alumina content of the extracted pure cord steel sample. Appropriate chemical analysis methods or instruments can be used for determination.
[0040] Preferably, the additive is added in step 4, and after the addition is completed, it needs to be stirred continuously. Stirring can ensure sufficient mixing and improve the mixing effect.
[0041] Preferably, after the additives are added in step 4, stirring is required for 15 min-20 min.
[0042] Preferably, in step 2, the combustion speed can be reduced or increased by increasing or decreasing the temperature in the furnace.
[0043] Preferably, during the smelting process, the content of trace elements in the steel needs to be closely monitored by monitoring instruments so that it can be regulated and controlled in a timely manner.
[0044] Compared with the prior art, the present invention provides a cord steel trace element control process, which has the following beneficial effects:
[0045] 1. The trace element control process of the cord steel achieves the purpose of production demand through the design of cord steel composition, process technology plan, and optimization of production organization plan. The converter achieves the goal of controlling P+S ≤ 0.025% through molten iron KR pre-desulfurization and optimization of converter slag basicity. The Al content in the molten steel is stably controlled by optimizing the addition sequence of steelmaking alloys and deoxidation alloys. By optimizing the production organization plan, strictly controlling the types of furnace materials and the types of alloys entering the ladle, controlling the slag and combining deoxidation and alloying to achieve Ti ≤ 0.0015%, Cu ≤ 0.05%, and oxygen content O ≤ 30ppm in the molten steel, thereby achieving effective control of trace elements.
[0046] 2. The trace element control process of the cord steel can minimize the content of trace elements by real-time control of the smelting temperature. Higher temperature helps to reduce the solid solubility of elements, making it easier to separate trace elements. By controlling the smelting temperature, the trace elements can be fully dissolved and evenly distributed.
[0047] 3. The trace element control process of the cord steel monitors the deoxidation and degassing process in real time, determines the deoxidation effect through chemical analysis or online monitoring instruments, and adjusts the amount of steelmaking slag added, stirring intensity, etc. according to the monitoring results to achieve the expected deoxidation effect. BRIEF DESCRIPTION OF THE DRAWINGS
[0048] Figure 1 It is a schematic diagram of the structure of the present invention. DETAILED DESCRIPTION
[0049] like Figure 1 As shown, the present invention provides a technical solution: a trace element control process for cord steel, the trace element control process for cord steel comprising the following steps:
[0050] Step 1: Raw material selection. Before smelting, the raw materials are strictly screened and controlled to ensure that the trace element content in the raw materials is low. This can be achieved by carefully selecting raw materials such as ore and scrap steel, and using chemical analysis instruments to test the raw materials.
[0051] Step 2: Put the raw materials into the smelting furnace, control the smelting temperature, atmosphere and material addition parameters, so as to minimize the content of trace elements. Higher temperature helps to reduce the solid solubility of elements, so that trace elements are easier to separate. By controlling the smelting temperature, the trace elements can be fully dissolved and evenly distributed;
[0052] Step 3: Impurity removal: During the smelting process, an impurity removal process is required to remove trace elements to ensure the quality of the cord steel after forming;
[0053] Step 4: Adding additives: During the smelting process, some special additives are added to the raw materials to adsorb, separate or convert trace elements.
[0054] In step 2, the amount of oxygen blown in is controlled to increase the oxidation reaction rate during the smelting process, thereby reducing the content of trace elements.
[0055] The impurity removal process in step 3 includes the following steps:
[0056] S1. Reduce sulfur content by alkaline flux desulfurization, prepare alkaline flux, determine suitable alkaline flux, such as calcium, magnesium, etc., calculate and prepare enough flux according to furnace capacity and desulfurization requirements, add flux to the furnace, and evenly add the pre-prepared alkaline flux to the furnace during smelting;
[0057] S2. Use a stirring device or gas stirring to mix and stir them, which can ensure that the flux and the molten metal in the furnace are fully mixed and contacted;
[0058] S3. In molten metal, alkaline flux will react with sulfide to generate sulfide that is insoluble in metal. Sulfide will precipitate or float on the metal surface and then be removed or fished out, thereby reducing the sulfur content in the metal.
[0059] S4. Monitor the desulfurization reaction in real time and determine the desulfurization effect through chemical analysis or online monitoring instruments.
[0060] The impurity removal process in step 3 also includes: using steelmaking slag for deoxidation and degassing, and using steelmaking slag for deoxidation and degassing includes the following steps:
[0061] S1. Prepare steelmaking slag. Steelmaking slag is usually obtained from limestone and other auxiliary materials (such as coke, etc.) through a smelting process. Prepare enough steelmaking slag and ensure that it meets the deoxidation requirements.
[0062] S2, adding steelmaking slag, and evenly putting the steelmaking slag on the surface of the molten steel to make it fully contact with the molten steel;
[0063] S3, reaction and deoxidation. At high temperature, steelmaking slag will react with oxygen in molten steel to form gas (such as CO, CO2, etc.) and discharge it. At the same time, oxygen in steelmaking slag will also react with other non-metallic elements (such as silicon, manganese, etc.) in molten steel to achieve the effect of deoxidation and degassing.
[0064] S4. Stirring and mixing: Use stirring devices or gas stirring to ensure that the steelmaking slag and molten steel are fully mixed and in contact.
[0065] S5. Monitoring and adjustment: monitor the deoxidation and degassing process in real time, determine the deoxidation effect through chemical analysis or online monitoring instruments, and adjust the amount of steelmaking slag added, stirring intensity, etc. according to the monitoring results to achieve the expected deoxidation effect.
[0066] In step 4, the additive is sodium borate to reduce the vanadium content, and the specific steps are as follows:
[0067] S1. Prepare sodium borate by dissolving an appropriate amount of sodium borate solid in sufficient water to prepare a sodium borate solution;
[0068] S2. Prepare steel materials: prepare the cord steel sample to be processed, which may be powdered steel materials or block steel materials;
[0069] S3, adding sodium borate solution, slowly adding the sodium borate solution into the cord steel sample, and ensuring sufficient mixing by stirring or other means;
[0070] S4, smelting: the mixed cord steel sample is smelted, and a suitable smelting method can be selected, such as electric arc furnace smelting;
[0071] S5, filtering and cooling, filtering and cooling the smelted molten liquid to separate the solid residue and the cooled liquid;
[0072] S6, separating the waste residue, and treating the separated solid waste residue, which can be recycled or incinerated;
[0073] S7. Extracting pure cord steel. Extracting pure cord steel from the cooled liquid can be purified by filtering, precipitation, concentration, etc.
[0074] S8. Detect the vanadium content. Detect the vanadium content of the extracted pure cord steel sample. Appropriate chemical analysis methods or instruments can be used for determination.
[0075] The additive in step 4 is to add sodium chloride to the smelting cord steel to adsorb and remove alumina, and the specific steps are as follows:
[0076] S1. Prepare a sodium chloride solution by dissolving an appropriate amount of sodium chloride solid in sufficient water to prepare a sodium chloride solution;
[0077] S2. Prepare steel materials, and prepare the cord steel samples to be processed;
[0078] S3, adding sodium chloride solution, and slowly adding the sodium chloride solution into the cord steel sample;
[0079] S4. Smelting: Smelting the mixed cord steel sample. A suitable smelting method may be selected, such as electric arc furnace smelting or other methods;
[0080] S5, filtering and cooling, filtering and cooling the smelted molten liquid to separate the solid residue and the cooled liquid;
[0081] S6, separating the waste residue, and treating the separated solid waste residue, which can be recycled or incinerated;
[0082] S7. Extracting pure cord steel. Extracting pure cord steel from the cooled liquid can be purified by filtering, precipitation, concentration, etc.
[0083] S8. Detect the alumina content. Detect the alumina content of the extracted pure cord steel sample. Appropriate chemical analysis methods or instruments can be used for determination.
[0084] In step 4, the additives are added and stirred continuously after the addition is completed. Stirring can ensure sufficient mixing and improve the mixing effect.
[0085] After adding the additives in step 4, stir for 15-20 minutes.
[0086] In step 2, the combustion speed can be reduced or increased by increasing or decreasing the temperature in the furnace.
[0087] During the smelting process, the content of trace elements in the steel needs to be closely monitored through monitoring instruments so that it can be adjusted and controlled in time.
[0088] The above generally describes the present invention in detail, but it is obvious to a person skilled in the art that some modifications or improvements can be made to the present invention. Therefore, modifications or improvements that do not depart from the spirit of the present invention are within the scope of protection of the present invention.
Claims
1. A cord steel trace element control process, characterized in that: The cord steel trace element control process includes the following steps: Step 1: Raw material selection. Before smelting, the raw materials are strictly screened and controlled to ensure that the trace element content in the raw materials is low. This can be achieved by carefully selecting raw materials such as ore and scrap steel, and using chemical analysis instruments to test the raw materials. Step 2: Put the raw materials into the smelting furnace and control the smelting temperature, atmosphere and material addition parameters; Step 3: impurity removal: during the smelting process, an impurity removal process is required to remove trace elements; Step 4: Adding additives: During the smelting process, some special additives are added to the raw materials to adsorb, separate or convert trace elements.
2. A cord steel trace element control process according to claim 1, characterized in that: In the step 2, the oxidation reaction rate in the smelting process is increased by controlling and increasing the amount of oxygen blown in.
3. A cord steel trace element control process according to claim 1, characterized in that: The impurity removal process in step 3 comprises the following steps: S1. Reduce sulfur content by alkaline flux desulfurization, prepare alkaline flux, determine suitable alkaline flux, such as calcium, magnesium, etc., calculate and prepare enough flux according to furnace capacity and desulfurization requirements, add flux to the furnace, and evenly add the pre-prepared alkaline flux to the furnace during smelting; S2, mixing and stirring the mixture by using a stirring device or gas stirring; S3. In molten metal, alkaline flux will react with sulfide to generate sulfide that is insoluble in metal. Sulfide will precipitate or float on the metal surface and then be removed or fished out, thereby reducing the sulfur content in the metal. S4. Monitor the desulfurization reaction in real time and determine the desulfurization effect through chemical analysis or online monitoring instruments.
4. A cord steel trace element control process according to claim 3, characterized in that: The impurity removal process in step 3 further includes: using steelmaking slag for deoxidation and degassing, and using steelmaking slag for deoxidation and degassing includes the following steps: S1. Prepare steelmaking slag. Steelmaking slag is usually obtained from limestone and other auxiliary materials (such as coke, etc.) through a smelting process. Prepare enough steelmaking slag and ensure that it meets the deoxidation requirements. S2, adding steelmaking slag, and evenly putting the steelmaking slag on the surface of the molten steel to make it fully contact with the molten steel; S3, reaction and deoxidation, at high temperature, steelmaking slag will react with oxygen in molten steel to form gas (such as CO, CO2, etc.) and discharge it. At the same time, oxygen in steelmaking slag will also react with other non-metallic elements (such as silicon, manganese, etc.) in molten steel; S4. Stirring and mixing: Use stirring devices or gas stirring to ensure that the steelmaking slag and molten steel are fully mixed and in contact. S5. Monitoring and adjustment: monitor the deoxidation and degassing process in real time, determine the deoxidation effect through chemical analysis or online monitoring instruments, and adjust the amount of steelmaking slag added, stirring intensity, etc. based on the monitoring results.
5. A cord steel trace element control process according to claim 1, characterized in that: The additive in step 4 is sodium borate to reduce the vanadium content, and the specific steps are as follows: S1. Prepare sodium borate by dissolving an appropriate amount of sodium borate solid in sufficient water to prepare a sodium borate solution; S2. Prepare steel materials: prepare the cord steel sample to be processed, which may be powdered steel materials or block steel materials; S3, adding sodium borate solution, slowly adding the sodium borate solution into the cord steel sample, and ensuring sufficient mixing by stirring or other means; S4, smelting: the mixed cord steel sample is smelted, and a suitable smelting method can be selected, such as electric arc furnace smelting; S5, filtering and cooling, filtering and cooling the smelted molten liquid to separate the solid residue and the cooled liquid; S6, separating the waste residue, and treating the separated solid waste residue, which can be recycled or incinerated; S7. Extracting pure cord steel. Extracting pure cord steel from the cooled liquid can be purified by filtering, precipitation, concentration, etc. S8. Detect the vanadium content. The vanadium content of the extracted pure cord steel sample can be detected by using appropriate chemical analysis methods or instruments.
6. A cord steel trace element control process according to claim 1, characterized in that: The additive in step 4 is to add sodium chloride to the smelting of cord steel to adsorb and remove alumina, and the specific steps are as follows: S1. Prepare a sodium chloride solution by dissolving an appropriate amount of sodium chloride solid in sufficient water to prepare a sodium chloride solution; S2. Prepare steel materials, and prepare the cord steel samples to be processed; S3, adding sodium chloride solution, and slowly adding the sodium chloride solution into the cord steel sample; S4. Smelting: Smelting the mixed cord steel sample. A suitable smelting method may be selected, such as electric arc furnace smelting or other methods; S5, filtering and cooling, filtering and cooling the smelted molten liquid to separate the solid residue and the cooled liquid; S6, separating the waste residue, and treating the separated solid waste residue, which can be recycled or incinerated; S7. Extracting pure cord steel. Extracting pure cord steel from the cooled liquid can be purified by filtering, precipitation, concentration, etc. S8. Detect the alumina content. Detect the alumina content of the extracted pure cord steel sample. Appropriate chemical analysis methods or instruments may be used for determination.
7. A cord steel trace element control process according to claim 6, characterized in that: In the step 4, the additive is added and it needs to be stirred continuously after the addition is completed.
8. A cord steel trace element control process according to claim 7, characterized in that: After the additives are added in step 4, stirring is required for 15-20 minutes.
9. A cord steel trace element control process according to claim 1, characterized in that: In the step 2, the combustion speed can be reduced or increased by increasing or decreasing the temperature in the furnace.
10. A cord steel trace element control process according to claim 1, characterized in that: During the smelting process, the content of trace elements in the steel needs to be closely monitored by monitoring instruments.