High-strength aluminum alloy section bar easy to absorb energy as well as processing technology and application thereof
By optimizing the composition and heat treatment process of aluminum alloy materials, the problems of low extrusion efficiency and insufficient mechanical properties in the existing technology are solved, and high-strength, easy energy absorption and lightweight automobile threshold beam profiles are realized, reducing production costs and meeting the Car safety and lightweight requirements.
Patent Information
- Application Number
- CN202411185050.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-27
AI Technical Summary
When producing automobile threshold beam profiles, the existing 6082 aluminum alloy material has low extrusion efficiency, low tensile strength and yield strength, which cannot meet the requirements of automobile lightweight and has high material cost.
By optimizing the composition and heat treatment process of aluminum alloy materials, adjusting the content of elements such as Mg, Si, Cu, Fe, Mn, La, Ce, etc., improving the homogeneous heat treatment and extrusion process, improving the strength and plasticity of the material, and reducing extrusion resistance , improve production efficiency.
It achieves high strength, easy energy absorption and good formability, meets the safety requirements of automobiles, improves extrusion efficiency, reduces material and production costs, and realizes lightweighting of threshold beams.
Smart Images

Figure CN118996296A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of aluminum alloy processing and preparation, and in particular to a high-strength and energy-absorbing aluminum alloy profile and a processing technology and application thereof. Background Art
[0002] The automobile threshold beam is an important safety component of the automobile. It connects the bottom structure and the side structure of the car body and bears the load from the road and the side. Therefore, the automobile threshold beam needs to have high strength, easy energy absorption and good formability. Aluminum alloy materials have become an ideal choice for automobile threshold beams due to their light weight, high strength and good formability. In the prior art, automobile threshold beams usually use 6082 aluminum alloy materials. 6082 aluminum alloy material is a commonly used aluminum alloy material with good comprehensive properties. In the production process, the aluminum alloy material must first be cast, then heat treated, and finally extruded into an automobile threshold beam profile. The heat treatment process mainly includes homogenization heat treatment, extrusion online solution and artificial aging. Through a reasonable heat treatment process, the microstructure of the aluminum alloy material can be improved, thereby improving its mechanical properties.
[0003] However, there are still some problems in the existing technology when producing automobile threshold beam profiles: 1. The existing 6082 aluminum alloy material has a large resistance when extruded and deformed, resulting in low extrusion efficiency, and the thinnest wall thickness of the produced profile is limited, which is not conducive to achieving lightweighting of the threshold beam. 2. When the existing 6082 alloy is used to produce automobile threshold beam profiles, the tensile strength and yield strength are low, the material bending angle is small, and it cannot meet the requirements of automobile lightweighting, and the material cost is also high.
[0004] Therefore, the prior art has the problems of low production efficiency, high material cost and insufficient mechanical properties when producing automobile door sill beam profiles. Summary of the invention
[0005] The purpose of the present invention is to provide a high-strength, energy-absorbing aluminum alloy profile processing technology with low extrusion resistance and high strength, so as to at least provide a beneficial choice or create conditions for solving one or more technical problems existing in the prior art.
[0006] To achieve the above objectives, the present invention adopts the following technical solutions.
[0007] A high-strength and energy-absorbing aluminum alloy profile processing technology, the steps of which are as follows.
[0008] 1) Optimize the composition of aluminum alloy materials: by adjusting the content of Mg, Si, Cu, Fe, Mn, La, Ce and other elements, the Mg content is 0.7%-1.0%, the Si content is 0.7%-1.0%, and the Cu content is 0.05%-0.35%; the Mg / Si ratio is controlled in the range of 0.8-1.3 to avoid excessive Si causing more silicon particles, which will affect the plasticity of the profile, reduce the bending angle, and cause column pressure to break; the sum of the Mg, Si, and Cu contents Mg+Si+Cu is controlled in the range of 1.6%-1.9% to ensure sufficient strengthening phase elements, avoid the strength loss caused by too little strengthening phase, and avoid the increase of material quenching sensitivity and the decrease of material plasticity caused by too many strengthening phase elements; Fe content 0.05%-0.25%, Mn content 0.1%-0.3%; the difference between Si and Fe content Si-Fe is controlled at 0.6%-0.8%, ensuring that there is enough Si element to participate in strengthening, avoiding the situation of strength reduction due to too little effective Si element content; Mn / Fe range is 0.8-1.4, ensuring that there is enough Mn element to promote the transformation of Fe phase to α phase, avoiding the adverse effect of β-Fe phase on plasticity; La content is 0.05%-0.15%, Ce content is 0.05%-0.15%; the sum of Mn, La, and Ce content Mn+La+Ce is controlled at 0.20%-0.40%, ensuring sufficient refinement effect on the material grain structure, but avoiding excessive element content affecting the quenching sensitivity of the material. The above element ratio makes the aluminum alloy material have low extrusion deformation resistance, and the extrusion efficiency can be increased by more than 20% compared with the conventional 6082 alloy, while maintaining high material strength and plasticity. The above contents are all mass percentages.
[0009] 2) Improve the heat treatment process: By improving the heat treatment process, the production efficiency is improved, and the microstructure of the aluminum alloy material is improved, and its mechanical properties are improved. Specifically, the aluminum rod is first subjected to homogenization heat treatment, the homogenization heat treatment temperature is 540℃-560℃, the homogenization holding time is 8h-12h, and the homogenization is quickly cooled after homogenization, and the cooling rate needs to reach 300℃ / h. Then, according to different types of profiles, different extruded rod gentle discharge speeds are selected, and water cooling or water spray cooling is performed. Finally, pre-aging and secondary aging are performed, the pre-aging temperature is 100℃-120℃, the pre-aging holding time is 1h-2h, the secondary aging temperature is 160℃-180℃, and the aging time is 4h-10h.
[0010] In some implementations, the aluminum alloy profile in the shape of a letter "C" is obtained by extrusion, the extrusion rod temperature is 480-500°C, the profile discharge speed is 7-12m / min, and the discharge port temperature is 540-550°C.
[0011] In some embodiments, a multi-grid integrated aluminum alloy profile is obtained by extrusion, the extrusion rod temperature is 480-500°C, the profile discharge speed is 6-8m / min, and the discharge port temperature is 540-550°C.
[0012] The present invention optimizes the composition and heat treatment process of the aluminum alloy material so that the tensile strength of the produced profile is greater than 340MPa, the yield strength is greater than 300MPa, the elongation after fracture is greater than 10%, and the bending angle of the material is greater than 80°, thereby meeting the requirements of automobile safety.
[0013] The present invention optimizes the composition and heat treatment process of the aluminum alloy material so that the thinnest wall thickness of the produced profile can be as low as 1.5 mm, which helps to achieve lightweighting of the threshold beam and greatly reduces the material and extrusion production costs.
[0014] On the other hand, the present invention further provides a high-strength and energy-absorbing aluminum alloy profile, which is manufactured using the high-strength and energy-absorbing aluminum alloy profile processing technology as described above.
[0015] On the other hand, the present invention also provides the use of the high-strength and energy-absorbing aluminum alloy profile as described above in the production of automobile door sill beams.
[0016] Compared with the prior art, the present invention mainly solves the following technical problems.
[0017] 1) The problem of the existing 6082 aluminum alloy material having large resistance during extrusion deformation, resulting in low extrusion efficiency, is solved. By optimizing the composition and heat treatment process of the aluminum alloy material, the material's resistance to extrusion deformation is reduced, and the extrusion efficiency can be increased by more than 20% compared with conventional 6082 alloy.
[0018] 2) The problem that the existing technology has low tensile strength and yield strength, small material bending angle, and cannot meet the safety requirements of lightweight automobiles when producing automobile door sill beam profiles is solved. By optimizing the composition and heat treatment process of aluminum alloy materials, the tensile strength of the produced profile is greater than 340MPa, the yield strength is greater than 300MPa, the elongation after fracture is greater than 10%, and the material bending angle is greater than 80°, which meets the safety requirements of automobiles.
[0019] 3) The problem of high material cost in the existing technology for producing automobile door sill beam profiles is solved. By optimizing the composition of aluminum alloy materials and the heat treatment process, the thinnest wall thickness of the produced profile can be as low as 1.5mm, which helps to achieve lightweight door sill beams and greatly reduces material and extrusion production costs.
[0020] Compared with the prior art, the present invention has the following advantages and beneficial effects.
[0021] 1. In the aluminum alloy material of the present invention, the content range of Mg, Si, Cu, Fe, Mn, La and Ce is precisely controlled, so that the material has high strength, easy energy absorption and good formability, and can meet the safety requirements of automobile door sill beams. At the same time, the ratio of Mn / Fe is also within a certain range, which helps to further optimize the microstructure of the material and improve its mechanical properties.
[0022] Second, the homogenization heat treatment temperature and time of the present invention are precisely controlled, and the cooling rate of rapid cooling optimizes the microstructure of the aluminum alloy material, thereby improving its mechanical properties. In addition, the pre-aging and secondary aging temperatures and times of the present invention are also precisely controlled, which helps to further improve the mechanical properties of the aluminum alloy material.
[0023] 3. The extrusion process of the present invention is precisely controlled, so that the aluminum alloy material has a smaller resistance during extrusion deformation, thereby improving the extrusion efficiency. The thinnest wall thickness of the produced profile can reach 1.5 mm, which is conducive to lightweighting of the threshold beam and greatly reduces the material and extrusion production costs.
[0024] Fourth, the tensile strength, yield strength, elongation after fracture and bending angle of the produced profile of the present invention are significantly improved, thereby meeting the requirements of automobile safety. In general, the aluminum alloy material and its heat treatment process of the present invention not only improve the mechanical properties of automobile door sill beams, but also improve production efficiency, reduce material costs, and have broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 The figure shows a column pressure test diagram of the aluminum alloy profile for automobile door sill beam prepared in Example 1 of the present invention.
[0026] Figure 2 Shown is a column pressure test diagram of the aluminum alloy profile for automobile door sill beam prepared in Comparative Example 1 of the present invention. DETAILED DESCRIPTION
[0027] The specific implementation of the present invention is further described below to make the technical solution and beneficial effects of the present invention clearer and more specific. The following embodiments are exemplary and intended to explain the present invention, but cannot be construed as limiting the present invention.
[0028] Additional aspects and advantages of the present invention will become apparent in the following description or may be learned by practice of the present invention. Example
[0029] A processing technology for aluminum alloy profiles for automobile door sill beams has the following steps.
[0030] Step 1: Material preparation. First, prepare an aluminum rod with a diameter of 228 mm, whose composition by weight percentage is as follows: Mg content 0.74%, Si content 0.80%, Cu content 0.15%, Mg / Si ratio controlled to 0.95, Mg+Si+Cu content 1.69%, Fe content 0.15%, Mn content 0.18%, Si-Fe content 0.65%, Mn / Fe 1.2, La content 0.08%, Ce content 0.10%, Mn+La+Ce content 0.36%, and the rest is Al.
[0031] Step 2: Homogenization heat treatment. Put the aluminum rod into the homogenization furnace for homogenization heat treatment. The homogenization heat treatment temperature is 550℃, and the homogenization heat preservation time is 10h. After homogenization treatment, cool quickly, and the cooling rate needs to reach 300℃ / h.
[0032] Step 3: Extrusion molding. According to different types of profiles, different extrusion rod temperatures and discharge speeds are selected. In this embodiment, the extrusion rod temperature is 480°C, the profile discharge speed is 10m / min, the discharge port temperature is 550°C, and water cooling is performed.
[0033] Step 4: Pre-aging treatment: The extruded profile is pre-aged at 100°C for 1 hour.
[0034] Step 5: Secondary aging treatment: The pre-aged profile is subjected to secondary aging treatment at 180°C for 6 hours.
[0035] The aluminum alloy profile for automobile threshold beam prepared in this embodiment was subjected to column pressure test, and the results are as follows: Figure 1 As shown. Figure 1 It can be seen that the aluminum alloy profile for automobile sill beams produced in this embodiment passes the column pressure test and meets the high-strength and easy-energy-absorbing use requirements of the aluminum alloy profile for automobile sill beams. Example
[0036] A processing technology for aluminum alloy profiles for automobile door sill beams has the following steps.
[0037] Step 1: Material preparation. First, prepare an aluminum rod with a diameter of 228 mm, whose composition by weight percentage is as follows: Mg content 0.89%, Si content 0.80%, Cu content 0.17%, Mg / Si ratio controlled to 1.11, Mg+Si+Cu content to 1.86, Fe content 0.19%, Mn content 0.20%, Si-Fe content 0.61%, Mn / Fe 1.05, La content 0.08%, Ce content 0.10%, Mn+La+Ce content 0.38%, and the rest is Al.
[0038] Step 2: Homogenization heat treatment. Put the aluminum rod into the homogenization furnace for homogenization heat treatment. The homogenization heat treatment temperature is 560℃, and the homogenization heat preservation time is 10h. After homogenization, cool quickly, and the cooling rate needs to reach 300℃ / h.
[0039] Step 3: Extrusion molding. Extrusion category letter-shaped interior door sill beam profile, extrusion rod temperature is 500℃, profile discharge speed is 10m / min, discharge port temperature is 550℃, and water cooling is performed.
[0040] Step 4: Pre-aging treatment: The extruded profile is pre-aged at 100°C for 1.5 hours.
[0041] Step 5: Secondary aging treatment: The pre-aged profile is subjected to secondary aging treatment at 170°C for 6 hours. Example
[0042] A processing technology for aluminum alloy profiles for automobile door sill beams has the following steps.
[0043] Step 1: Material preparation. First, prepare an aluminum rod with a diameter of 381 mm, whose composition by weight percentage is as follows: Mg content 0.93%, Si content 0.82%, Cu content 0.10%, Mg / Si ratio controlled to 1.1, Mg+Si+Cu content 1.85%, Fe content 0.12%, Mn content 0.12%, Si-Fe content 0.70%, Mn / Fe 1.0, La content 0.07%, Ce content 0.08%, Mn+La+Ce content 0.27%, and the rest is Al.
[0044] Step 2: Homogenization heat treatment. Put the aluminum rod into the homogenization furnace for homogenization heat treatment. The homogenization heat treatment temperature is 560℃, and the homogenization heat preservation time is 10h. After homogenization, cool quickly, and the cooling rate needs to reach 300℃ / h.
[0045] Step 3: Extrusion molding. According to different types of profiles, different extrusion rod temperatures and discharge speeds are selected. In this embodiment, a multi-grid integrated threshold beam profile is extruded, the extrusion rod temperature is 500°C, the profile discharge speed is 6m / min, the discharge port temperature is 545°C, and water spray cooling is used.
[0046] Step 4: Pre-aging treatment: The extruded profile is pre-aged at 110°C for 1.5 hours.
[0047] Step 5: Secondary aging treatment: The pre-aged profile is subjected to secondary aging treatment at 165°C for 10 hours. Example
[0048] A processing technology for aluminum alloy profiles for automobile door sill beams has the following steps.
[0049] Step 1: Material preparation. First, prepare an aluminum rod with a diameter of 381 mm, whose composition by weight percentage is as follows: Mg content 0.72%, Si content 0.73%, Cu content 0.30%, Mg / Si ratio controlled to 0.99, Mg+Si+Cu content 1.65%, Fe content 0.12%, Mn content 0.12%, Si-Fe content 0.61%, Mn / Fe 1, La content 0.06%, Ce content 0.07%, Mn+La+Ce content 0.25%, and the rest is Al.
[0050] Step 2: Homogenization heat treatment. Put the aluminum rod into the homogenization furnace for homogenization heat treatment. The homogenization heat treatment temperature is 550℃, and the homogenization heat preservation time is 12h. After homogenization, cool quickly, and the cooling rate needs to reach 300℃ / h.
[0051] Step 3: Extrusion molding. According to different types of profiles, different extrusion rod temperatures and discharge speeds are selected. In this embodiment, a multi-grid integrated threshold beam profile is extruded, the extrusion rod temperature is 490°C, the profile discharge speed is 8m / min, the discharge port temperature is 545°C, and water spray cooling is used.
[0052] Step 4: Pre-aging treatment: The extruded profile is pre-aged at 110°C for 2 hours.
[0053] Step 5: Secondary aging treatment: The pre-aged profile is subjected to secondary aging treatment at 170°C for 8 hours.
[0054] Comparative example 1.
[0055] A processing technology for aluminum alloy profiles for automobile door sill beams is basically the same as that of embodiment 1, except that:
[0056] 1) Step 1: In the material preparation step, the composition of the aluminum rod is as follows by weight percentage: Mg content 0.65%, Si content 0.86%, Cu content 0.32%, Mg / Si ratio controlled at 0.76, Mg+Si+Cu content 1.83%, Fe content 0.2%, Mn content 0.22%, Si-Fe content 0.64%, Mn / Fe 1.1, La content 0.06%, Ce content 0.08%, Mn+La+Ce content 0.36%, and the rest is Al.
[0057] 2) During the extrusion step, the profile discharge speed is 12 m / min.
[0058] The aluminum alloy profile for automobile threshold beam prepared in this comparative example was subjected to column pressure test, and the results are as follows: Figure 2 As shown. Figure 2It can be seen that the aluminum alloy profile for automobile threshold beams prepared in this comparative example fails the column pressure test and cannot meet the high-strength and easy-energy-absorbing use requirements of the aluminum alloy profile for automobile threshold beams.
[0059] In order to better reflect the progress of the present invention, the present invention also conducted comparative tests of Comparative Examples 2 to 6. The process parameters of Comparative Examples 2 to 6 are shown in Tables 1 and 2.
[0060] Table 1. Aluminum alloy material composition of Examples 1-4 and Comparative Examples 1-6 .
[0061] Table 2. Comparison of heat treatment processes for Examples 1-4 and Comparative Examples 1-6 .
[0062] It should be noted that Table 1 and Table 2 are used to show the differences between different embodiments and different comparative examples, and the parts not shown in Table 1 and Table 2 are the same.
[0063] Performance testing.
[0064] The performance tests were conducted on the aluminum alloy profiles for automobile door sill beams prepared in Examples 1-4 and Comparative Examples 1-6. The results are shown in Table 3.
[0065] Table 3. Performance test comparison table of Examples 1-4 and Comparative Examples 1-6 .
[0066] It can be seen from Table 3 that when one or more of the aluminum alloy material composition and the heat treatment process changes, one or more of the strength and energy absorption performance of the obtained aluminum alloy profile will deteriorate. It can be seen that the technical effect of the present invention is the result of the combined effect of the optimization of the aluminum alloy material composition and the optimization of the heat treatment process.
[0067] In addition, due to the advanced nature of the present invention, it can be widely used in application fields such as the automotive engineering field, the material science field and the heat treatment process field. In the automotive engineering field, the high-strength and energy-absorbing aluminum alloy material for automobile threshold beams and its heat treatment process of the present invention can effectively solve the problems existing in the prior art when producing automobile threshold beam profiles. First, the aluminum alloy material of the present invention has a small resistance during extrusion deformation, which can improve the extrusion efficiency and reduce the material cost. At the same time, the threshold beam can be lightweight, meeting the demand for lightweighting of automobiles. Secondly, when the aluminum alloy material of the present invention is used to produce profiles, the tensile strength and yield strength are high, the elongation after fracture is large, and the material bending angle is large, which can meet the requirements of automobile safety. Therefore, the present invention has broad application prospects in the automotive engineering field. In the field of materials science, the aluminum alloy material of the present invention and its heat treatment process can be used as a new type of high-strength and energy-absorbing aluminum alloy material, which is applied to various materials requiring high strength, easy energy absorption and good formability. Due to its unique alloy composition and heat treatment process, the aluminum alloy material of the present invention has excellent mechanical properties and formability, which can meet the needs of various applications. Therefore, the present invention has broad application prospects in the field of materials science. In the field of heat treatment technology, the heat treatment process of the present invention can be used as a new type of high-efficiency and energy-saving heat treatment process for aluminum alloy materials, and can be applied to various aluminum alloy materials that require high strength, easy energy absorption and good formability. Due to its simple and efficient heat treatment process, the heat treatment process of the present invention can improve production efficiency, and at the same time can avoid defects inside the aluminum alloy material and improve its mechanical properties. Therefore, the present invention has broad application prospects in the field of heat treatment technology.
[0068] In general, the high-strength and energy-absorbing aluminum alloy material for automobile door sill beams and the heat treatment process thereof of the present invention have excellent mechanical properties and forming properties due to their unique alloy composition and heat treatment process, can meet the needs of the fields of automobiles, materials and heat treatment, and have broad application prospects and market demands.
[0069] It should be noted that the technical features of the above embodiments can be combined arbitrarily. In order to make the description concise, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0070] The above embodiments only express several implementation methods of the present invention, and the description is relatively specific and detailed, but it cannot be understood as limiting the scope of the invention patent. It should be pointed out that for ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. The parts not described in the specific embodiments are all prior art or common knowledge.
[0071] It should be noted that, in the description of the present invention, the content of the present invention can be more easily understood by referring to the detailed description of the preferred implementation method of the present invention above and the embodiments included. Unless otherwise specified, all technical and scientific terms used in the present invention have the same meanings as those of ordinary skill in the art to which the present invention belongs. When there is a conflict, the definitions in this specification shall prevail.
[0072] In the present invention, the term "prepared from..." is used synonymously with "comprising". The terms "comprising", "including", "having", "containing" or any other variation thereof, as used in the present invention, are intended to cover a non-exclusive inclusion. For example, a composition, process, method, article, or apparatus comprising the listed elements is not necessarily limited to only those elements, but may include other elements not expressly listed or inherent to such composition, process, method, article, or apparatus.
[0073] In the present invention, when an amount, concentration, or other value or parameter is expressed as a range, a preferred range, or a range limited by a series of upper preferred values and lower preferred values, this should be understood as specifically disclosing all ranges formed by any pairing of any range upper limit or preferred value with any range lower limit or preferred value, regardless of whether the range is disclosed separately. For example, when a range of "1 to 5" is disclosed, the described range should be interpreted as including a range of "1 to 4", "1 to 3", "1 to 2", "1 to 2 and 4 to 5", "1 to 3 and 5" etc. When a numerical range is described in the present invention, unless otherwise stated, the range is intended to include its end values and all integers and fractions within the range.
[0074] In addition, the indefinite articles "a" and "an" before the elements or components of the present invention have no restrictions on the quantity requirements (i.e. the number of occurrences) of the elements or components. Therefore, "a" or "an" should be interpreted as including one or at least one, and the elements or components in the singular form also include the plural form, unless the number is obviously intended to be in the singular form.
Claims
1. A high-strength and energy-absorbing aluminum alloy profile processing technology, characterized in that: Here are the steps: 1) Material preparation: prepare aluminum bars. The composition of the aluminum bars is as follows by weight percentage: Mg 0.7-10%, Si 0.7-1.0%, Cu 0.05-0.35%, Mg / Si ratio is controlled to be 0.8-1.3, the sum of Mg, Si and Cu contents is controlled to be 1.6-1.9%, Fe content is 0.05-0.25%, Mn content is 0.1-0.3%, the difference between Si and Fe contents is controlled to be 0.6-0.8%, Mn / Fe is 0.8-1.4, La content is 0.05-0.15%, Ce content is 0.05-0.15%, the sum of Mn, La and Ce contents is controlled to be 0.2-0.4%, and the rest is Al; 2) Homogenization heat treatment: put the aluminum rod into a homogenization furnace for homogenization heat treatment; the homogenization heat treatment temperature is 540-560℃, and the homogenization holding time is 8-12h; after homogenization treatment, cool rapidly, with a cooling rate of more than 300℃ / h; 3) Extrusion molding, extruding the aluminum rod after homogenization heat treatment to obtain aluminum alloy profiles; 4) Pre-aging treatment: pre-aging the extruded aluminum alloy profile at a temperature of 100-120°C for 1-2 hours; 5) Secondary aging treatment: the pre-aged profile is subjected to secondary aging treatment at a temperature of 160-180°C for 4-10 hours to obtain a high-strength and energy-absorbing aluminum alloy profile.
2. A high-strength and energy-absorbing aluminum alloy profile processing process according to claim 1, characterized in that: In the extrusion molding step, different gentle discharge speeds of the extruded rod are set according to different types of aluminum alloy profiles obtained by extrusion.
3. The high-strength and energy-absorbing aluminum alloy profile processing technology according to claim 1 is characterized in that: In the extrusion molding step, a type-shaped aluminum alloy profile is extruded, the extrusion rod temperature is 480-500°C, the profile discharge speed is 7-12m / min, and the discharge port temperature is 540-550°C.
4. The high-strength and energy-absorbing aluminum alloy profile processing technology according to claim 1 is characterized in that: In the extrusion molding step, a multi-grid integrated aluminum alloy profile is extruded, the extrusion rod temperature is 480-500°C, the profile discharge speed is 6-8m / min, and the discharge port temperature is 540-550°C.
5. A high-strength and energy-absorbing aluminum alloy profile processing technology according to claim 3 or 4, characterized in that: Aluminum alloy profiles are water cooled after extrusion.
6. A high-strength and energy-absorbing aluminum alloy profile, characterized in that: The high-strength and energy-absorbing aluminum alloy profile is produced by using a processing technology for high-strength and energy-absorbing aluminum alloy profiles as described in any one of claims 1 to 5.
7. The high-strength and energy-absorbing aluminum alloy profile according to claim 6, characterized in that: The thinnest wall thickness of high-strength and energy-absorbing aluminum alloy profiles is 1.5mm.
8. Use of the high-strength and energy-absorbing aluminum alloy profile as described in any one of claims 6 to 7 in the production of automobile door sill beams.
Citation Information
Patent Citations
Cast aluminum alloy components
CN105039798A
High strength products extruded from 6xxx aluminium alloys having excellent crash performance
CN106605004A
Special high-strength and high-toughness aluminum alloy material for automobile and manufacturing technology
CN108660343A
6-series aluminum alloy plate for semiconductor equipment and manufacturing method
CN115679165A
High-strength easy-to-extrude aluminum alloy and profile extrusion method thereof
CN115852217A
Cited By
Integrated machining process for high-strength aluminum alloy mobile phone middle frame
CN119772523A