Catalyst slurry spraying method and circular membrane electrode CCM preparation method
By forming concentric circles through unidirectional segmented spraying along a circular spraying path, the problem of low catalyst utilization is solved, achieving efficient catalyst utilization and cost savings.
Patent Information
- Application Number
- CN202410968854.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-07-18
AI Technical Summary
Existing spraying processes have low catalyst utilization rates when preparing circular membrane electrodes, leading to increased costs.
A circular spraying path is used for unidirectional segmented spraying to form concentric circles. The spraying starts from the farthest point from or near the center of the concentric circles and sprays sequentially. The spraying parameters are a flow rate of 0.6-1.5 ml/min and a speed of 60-100 mm/s.
It significantly improved catalyst utilization, reduced membrane electrode costs, and increased precious metal loading by 38%-45%.
Smart Images

Figure CN118996465A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of hydrogen energy, and relates to a method for spraying a catalyst slurry and a method for preparing a circular membrane electrode CCM. Background Art
[0002] Hydrogen energy is a secondary energy source that is abundant in sources, green, low-carbon and widely used. It can help to absorb renewable energy on a large scale, achieve large-scale peak regulation of the power grid and cross-seasonal and cross-regional energy storage, and accelerate the low-carbonization of industries such as industry, construction, and transportation.
[0003] The membrane electrode is the core of the PEM water electrolysis hydrogen production reaction, which determines the performance, life and cost of the final membrane electrode product. Its preparation method and structural design are closely related to the PEM water electrolysis performance. At present, the PEM membrane electrode generally adopts the CCM structure (catalyst coated membrane), that is, the catalyst slurry is coated on both sides of the proton exchange membrane.
[0004] At present, there are related studies on the spraying process. For example, the patent application with publication number CN116264284A discloses a spraying process for catalyst slurry and a method for preparing fuel cell CCM. The spraying path includes an interdigitated serpentine path I and a serpentine path II, and the serpentine path I and the serpentine path II both include a straight path and a turning path. This patent application controls the spraying speed and slurry flow rate of the catalyst layer spraying process, adopts an interdigitated serpentine path for spraying, and controls the temperature of the drying platform in different zones, so that the speed of the turning path spraying is 1.1-2 times faster than that of the straight path spraying, and the flow rate of the turning path spraying is 0.1-0.9 times that of the straight path spraying. A blank area is left between the two straight paths sprayed in sequence to avoid the accumulation of slurry during the turning path spraying, and solve the problem of high thickness of the catalyst layer at the edge of the catalyst layer caused by traditional uniform speed / uniform flow rate spraying.
[0005] And the invention patent with authorization number CN112599793B discloses a CCM coating process that uses a protective backing film to achieve anti-swelling, wherein the catalyst slurry is coated on the first surface of the proton exchange membrane, and the first catalyst layer is formed after drying; a protective membrane with a flexible carrier layer is prepared, and a protective membrane with a flexible carrier layer is attached to the first surface of the proton exchange membrane containing the first catalyst layer, and the protective membrane and the proton exchange membrane are pressed together; the catalyst slurry is coated on the second surface of the proton exchange membrane, and the second catalyst layer is dried to obtain a membrane electrode with a temporary protective membrane; finally, the membrane electrode with a temporary protective membrane is subjected to heat treatment or ultraviolet (UV) irradiation, and the temporary protective layer is peeled off to obtain a membrane electrode; if heat treatment is selected, a nano oxide solution needs to be sprayed on the surface of the first catalyst layer before the first catalyst layer is dried. The invention effectively avoids the swelling of the proton exchange membrane during the preparation of the membrane electrode.
[0006] When preparing circular membrane electrodes by spraying, it is usually necessary to position a square surface spraying area, and then use a circular spraying tool to cover it on the proton membrane, and then use the coating line to alternately fill it in one or two directions to form a circular membrane electrode, and finally heat and dry to remove the solvent to form a catalyst layer. However, this spraying method will cause serious waste of catalyst slurry, low catalyst utilization, and increased membrane electrode costs.
[0007] Therefore, more spraying processes are needed to adapt to more membrane electrode processing technologies. Summary of the invention
[0008] In order to solve the above technical problems, the present invention proposes to use a circular spray path to perform unidirectional segmented spraying on the proton membrane, and finally solve the problem of severe catalyst loss in a concentric circle manner, so as to achieve the purpose of improving catalyst utilization and saving membrane electrode costs.
[0009] To achieve the above purpose, the specific technical solutions of the present invention are as follows:
[0010] The present invention provides a method for spraying catalyst slurry, wherein the catalyst slurry is sprayed on a proton exchange membrane, and the catalyst slurry is sprayed on both sides of the proton exchange membrane in a circular path. The spraying path adopts unidirectional segmented spraying, and concentric circles are formed after spraying in sequence.
[0011] Preferably, the interval of the unidirectional segmented spraying is 6-7 mm. The flow rate of the spraying is 0.6-1.5 ml / min, and the spraying speed is 60-100 mm / s. Under this parameter range, the problem of proton membrane swelling caused by the slurry not drying in time can be avoided.
[0012] Specifically, during unidirectional segmented spraying, the spraying starting point is sprayed from a position away from the center of the concentric circle to the center of the circle, or sprayed from the center of the circle to a position away from the center of the concentric circle.
[0013] Wherein, the catalyst in the catalyst slurry is a platinum-carbon catalyst.
[0014] The present invention also provides application of the spraying method in preparing a circular membrane electrode CCM.
[0015] The present invention also provides a method for preparing a circular membrane electrode CCM, preparing a catalyst slurry, spraying the catalyst slurry onto a proton exchange membrane to prepare a membrane electrode, obtaining the circular membrane electrode CCM, and spraying the catalyst slurry onto both sides of the proton exchange membrane using the spraying method.
[0016] Specifically, the method for preparing the catalyst slurry comprises the following steps:
[0017] The catalyst, perfluorosulfonic acid resin and solvent are mixed and dispersed uniformly to obtain catalyst slurry.
[0018] The solvent is water and organic alcohol; the mass ratio of water to organic alcohol is 1-2:1;
[0019] The mass ratio of the perfluorosulfonic acid resin to the catalyst is 10:1.
[0020] The dispersion is firstly carried out by ultrasonic dispersion and then shearing by a high-speed homogenizer.
[0021] Beneficial effects of the present invention:
[0022] The present invention can avoid catalyst slurry loss caused by excessive spraying by forming concentric circles; this method is simple and quick, and only needs to determine a circular path, and the next circular path can be set by corresponding interval displacement to finally form concentric circles; in addition, the spraying starting point can be sprayed from the outside to the inside (from the point far away from the center of the concentric circle to the center of the circle) in sequence, and can also be sprayed from the inside to the outside (from the center of the circle to the point far away from the center of the concentric circle) in sequence.
[0023] That is, the present invention adopts a circular spraying path to spray the proton membrane in a unidirectional segmented manner, and finally forms a concentric circle process, which can increase the precious metal loading by 38%-45%. The process of the present invention can significantly improve the catalyst utilization rate. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 It is a schematic diagram of the spraying process of the present invention.
[0025] Figure 2 This is a spraying effect diagram in Example 1.
[0026] Figure 3 This is a spraying effect diagram in Example 2.
[0027] Figure 4 This is a spraying effect diagram in Comparative Example 1. DETAILED DESCRIPTION
[0028] Example 1
[0029] Prepare catalyst slurry: weigh 0.029g of platinum-carbon catalyst, 0.29g of perfluorosulfonic acid resin (concentration 5%), 10g of deionized water, and 10g of n-propanol, mix the above components evenly, and then use an ultrasonic machine for ultrasonic dispersion at an ultrasonic frequency of 75Hz for 30min; then use a high-speed homogenizer for shearing at a speed of 14000rpm for 30min to finally form a uniform slurry.
[0030] Spraying setting: The spraying process diagram of the catalyst slurry of the present invention is as follows Figure 1As shown, the specific steps are as follows: lay a proton membrane of size 76mm*76mm flat on the operating table, set the heating temperature to 90℃ and perform vacuum adsorption. The circular size required for spraying is Set a concentric circle path, with the spraying starting point from the outside to the inside. Set the first point (69, 107.2), the second point (104, 72.2), and the third point (69, 37.2) of the first circular path. The interval between two adjacent circular paths is 6 mm. The next circular path can be set in sequence until the number of spraying sections of the circular path is 70 / 2 / 6=6 (rounded off). Set the spray flow rate to 0.6 ml / min and the spray speed to 60 mm / s.
[0031] Spraying effect Figure 2 As shown, the circular spraying area is relatively complete, the catalytic layer is relatively uniform as a whole, and there is no obvious overspray phenomenon at the edge.
[0032] Example 2
[0033] Preparation of slurry: Weigh 0.029g of platinum-carbon catalyst, 0.29g of perfluorosulfonic acid resin (concentration 5%), 5g of deionized water, and 10g of n-propanol, mix the above components evenly, and then use an ultrasonic machine for ultrasonic dispersion, the ultrasonic frequency is 75Hz, and the time is 30min; then use a high-speed homogenizer for shearing, the speed is 14000rpm, and the shearing time is 30min, finally forming a uniform slurry.
[0034] Spraying setting: Lay the proton membrane of size 76mm*76mm flat on the operating table, set the heating temperature to 90℃ and perform vacuum adsorption. The circular size required for spraying is Set a concentric circle path, with the spraying starting point from the inside to the outside. Set the first point (69, 79.2), the second point (76, 72.2), and the third point (69, 65.2) of the first circular path. The interval between two adjacent circular paths is 7 mm. The next path can be set in sequence until the number of spraying sections of the circular path is set to 70 / 2 / 7=5. Set the spray flow rate to 1.5 ml / min and the spray speed to 100 mm / s.
[0035] Spraying effect Figure 3 As shown, the circular spraying area is relatively complete, the catalytic layer is relatively uniform as a whole, and there is no obvious overspray phenomenon at the edge.
[0036] Comparative Example 1
[0037] Preparation of slurry: Weigh 0.029g of platinum-carbon catalyst, 0.29g of perfluorosulfonic acid resin (concentration 5%), 10g of deionized water, and 10g of n-propanol, mix the above components evenly, and then use an ultrasonic machine for ultrasonic dispersion, the ultrasonic frequency is 75Hz, and the time is 30min; then use a high-speed homogenizer for shearing, the speed is 14000rpm, and the shearing time is 30min, finally forming a uniform slurry.
[0038] Spraying setup: Lay the 76mm*76mm proton membrane flat on the operating table, set the heating temperature to 90℃ and perform vacuum adsorption, and place the circular spray tooling The first spraying coordinate point (44, 101) and the second spraying coordinate point (101, 55) are set to alternately fill in a tic-tac-toe pattern in the form of coating lines. The spraying interval is set to 6 mm, the spraying flow rate is 0.6 ml / min, and the spraying speed is 60 mm / s.
[0039] Spraying effect Figure 4 As shown, the circular spraying area in the middle is relatively complete and the catalytic layer is relatively uniform overall, but there is obvious overspray at the edge.
[0040] The catalyst layer sprayed in the present invention was tested for platinum content using an XRF detector, and the data are shown in Table 1.
[0041] Table 1
[0042]
[0043] From the table data, it can be seen that the precious metal loading of Examples 1 and 2 is improved compared with Comparative Example 1, and the improvement range is 38%-45%. The specific reason is that the circular membrane electrode formed by filling in the form of coating lines will have the problem of overspraying, and the spraying area formed by the coating lines is larger than the circular spraying area, so the process of the present invention can significantly improve the catalyst utilization rate.
Claims
1. A method for spraying a catalyst slurry, spraying the catalyst slurry on a proton exchange membrane, It is characterized in that The catalyst slurry is sprayed onto both sides of the proton exchange membrane in a circular path. The spraying path adopts unidirectional segmented spraying, and concentric circles are formed after spraying in sequence.
2. The method for spraying the catalyst slurry according to claim 1, It is characterized in that The interval of the unidirectional segmented spraying is 6-7 mm.
3. The method for spraying the catalyst slurry according to claim 1, It is characterized in that The spraying flow rate is 0.6-1.5 ml / min, and the spraying speed is 60-100 mm / s.
4. The method for spraying the catalyst slurry according to claim 1, It is characterized in that During unidirectional segmented spraying, the spraying starting point is sprayed from a point away from the center of the concentric circle to the center of the circle, or sprayed from the center of the circle to a point away from the center of the concentric circle.
5. The method for spraying the catalyst slurry according to claim 1, It is characterized in that The catalyst in the catalyst slurry is a platinum-carbon catalyst.
6. Use of the spraying method according to any one of claims 1 to 5 in the preparation of circular membrane electrode CCM.
7. A method for preparing a circular membrane electrode CCM, comprising preparing a catalyst slurry, spraying the catalyst slurry onto a proton exchange membrane to prepare a membrane electrode, and obtaining the circular membrane electrode CCM. It is characterized in that The catalyst slurry is sprayed onto both sides of the proton exchange membrane using the spraying method described in any one of claims 1 to 5.
8. The preparation method according to claim 7, It is characterized in that The method for preparing the catalyst slurry comprises the following steps: The catalyst, perfluorosulfonic acid resin and solvent are mixed and dispersed uniformly to obtain catalyst slurry.
9. The preparation method according to claim 8, It is characterized in that The solvent is water and organic alcohol; the mass ratio of water to organic alcohol is 1-2:1; The mass ratio of the perfluorosulfonic acid resin to the catalyst is 10:
1.
10. The preparation method according to claim 8, It is characterized in that The dispersion is firstly carried out by ultrasonic dispersion and then shearing by a high-speed homogenizer.
Citation Information
Patent Citations
Implementation method of photoresist coating track
CN104570609A
Direct-writing preparation method of high-flexibility organic electrode
CN109130168A
Preparation method of copper-based conductive ceramic coating electrode material
CN109338269A
Automatic spraying device
CN111530679A
Preparation method of fuel cell CCM
CN116264284A