Test method for measuring characteristic parameters of interface transition zone of asphalt mixture

The modulus and adhesion of the interface transition zone are measured in the asphalt mixture by atomic force microscopy, which solves the problem of inaccurate measurement of the interface transition zone in the prior art, and realizes the precise characterization of the characteristic parameters of the interface transition zone of the asphalt mixture, and improves the improvement of the improvement of the Material properties and durability.

CN119000237APending Publication Date: 2024-11-22HUNAN INST OF INFORMATION TECH +2
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202410967623.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

In the existing method of measuring the characteristic parameters of the interface transition zone of asphalt mixture, the gap between the nanoindentations is large, resulting in the measured interface transition zone inaccurate enough.

Method used

Atomic force microscope is used to conduct micromechanical performance testing, and peak force quantitative nanotesting is carried out at the interface between the aggregate and the slurry in asphalt mixture samples, combined with NanoScope Analysis 3.0 software to analyze the modulus and adhesion distribution maps to accurately quantify the transition zone of the interface. Thickness and adhesion strength.

Benefits of technology

Accurate quantitative characterization of the thickness, mechanical properties and interaction strength of the asphalt mixture interface transition zone is realized, the accuracy and reliability of measurement are improved, and the understanding and optimization of the performance of asphalt mixture is enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119000237A_ABST
    Figure CN119000237A_ABST
Patent Text Reader

Abstract

The invention discloses a test method for measuring characteristic parameters of an interface transition area of an asphalt mixture, relates to the technical field of microstructures and mechanical properties of asphalt mixtures, and aims to solve the problems that gaps between nano-indentation test points are relatively large; and the measured range of the interface transition area is not accurate enough. According to the technical key points, according to the phenomenon of mechanical property change in the interface transition area of the asphalt mixture, an atomic force microscope is used for carrying out a micromechanical property test on the interface of aggregate and asphalt in an asphalt mixture sample, and a selected test area comprises three phases of asphalt, aggregate and the interface transition area; and an experimental result is obtained, and result analysis is carried out by utilizing NanoScope Analysis 3.0 software. By analyzing the modulus and the adhesion distribution diagram, the thickness of the interface transition area can be obtained, the adhesion interaction strength of the aggregate and the asphalt interface transition area can be reflected, and quantitative characterization of the characteristic parameters such as the thickness, the mechanical property and the interaction strength of the asphalt mixture interface transition area can be realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of asphalt mixture microstructure and mechanical properties, and in particular to a test method for measuring characteristic parameters of an asphalt mixture interface transition zone. Background Art

[0002] In composite materials, the characteristics of the interface phase or interface transition zone play a vital role in the performance of the overall material. Asphalt mixture is a commonly used pavement material, and its performance directly affects the service life and safety of the road.

[0003] Asphalt mixture interface transition zone: The interface phase or interface transition zone is an important component of composite multiphase materials and has an important influence on the properties of composite materials. Asphalt mixture is a typical composite material composed of asphalt, aggregate, mineral powder, etc. There is an interface transition zone between the aggregate phase and the asphalt mortar phase composed of asphalt and mineral powder. From the perspective of microscopic mechanism, the damage of asphalt mixture under the combined effects of temperature, humidity and external load can generally be divided into two types: adhesion damage and cohesive damage. Cohesive damage occurs inside the asphalt mortar away from the aggregate, while adhesion damage, which is the main form of damage, occurs at the interface between the aggregate and the asphalt mortar and its transition zone. Therefore, the adhesion interaction between asphalt and aggregate in the interface transition zone has an important influence on the working state and failure mode of asphalt mixture, which is directly related to the strength composition of asphalt mixture and its performance in resisting water damage, fatigue, cracking and other damage.

[0004] The adhesion properties of the interface transition zone determine important properties of asphalt mixtures, such as tensile strength, fatigue resistance and water resistance. When the adhesion of the interface phase is insufficient, the bond between asphalt and aggregate will weaken, which can easily lead to debonding and cracking of the material, reducing the overall strength and durability. Adhesion failure and cohesive failure are common forms of failure of asphalt mixtures when subjected to stress. Adhesion failure mainly occurs at the interface between aggregate and asphalt mortar. When external loads act on the material, the adhesion at the interface may not be able to withstand the external force and debond. Cohesive failure occurs inside the asphalt mortar, and the fatigue or fracture of the internal structure causes the overall performance of the material to deteriorate. Therefore, when designing and producing asphalt mixtures, it is necessary to pay attention to the adhesion properties of the interface transition zone to improve the overall performance of the asphalt mixture.

[0005] The interface transition zone has always been one of the key issues in the research field of asphalt mixtures. Its characteristic parameters such as thickness, mechanical properties, and interaction strength are of great significance to the evaluation of aggregate-asphalt adhesion, mixture strength composition, water damage resistance, and computer simulation. Through micromechanical properties testing technology, researchers can more accurately analyze the difference between the interface transition zone and asphalt mortar, and then gain a deeper understanding of the adhesion between aggregate and asphalt and the strength composition of the mixture. The feasibility of this method can not only fill the gaps in existing research, but also bring new breakthroughs and progress to the research field of asphalt mixtures. In general, using micromechanical properties testing technology to characterize the thickness, mechanical properties, and interaction strength of the aggregate-asphalt mortar interface transition zone is an important and feasible method. This will help deepen our understanding of the interface transition zone of asphalt mixtures and promote research and development in this field. It is hoped that more research will pay attention to and explore this important issue in the future, providing a more scientific basis and support for the performance optimization and application of asphalt mixtures.

[0006] The existing patent document with the document number CN108956349A discloses a test method for measuring the characteristic parameters of the interface transition zone of asphalt mixture. The method uses a nanoindenter to perform a microscopic mechanical property test at the interface between aggregate and asphalt mortar based on the phenomenon that the mechanical properties of the aggregate and asphalt mortar interface transition zone change. The test points are set at equal distances from the aggregate to the asphalt mortar, and the load-indentation depth curve of each point is obtained. The modulus value is calculated, and the number of test points in the interface transition zone is determined according to the modulus and indentation depth change trend of each test point. The thickness of the interface transition zone is estimated by combining the distribution and spacing of the test points, and then the adhesion coefficient of the interface transition zone is calculated to achieve quantitative characterization of the characteristic parameters such as the thickness, mechanical properties and interaction strength of the aggregate-asphalt mortar interface transition zone. The problem with this prior art is that the quantitative characterization of the characteristic parameters such as the thickness, mechanical properties and interaction strength of the aggregate-asphalt mortar interface transition zone obtained is relatively large compared with the actual situation. In other words, the problem with the prior art is that nanoindentation uses a tapping point measurement method, and due to equipment and technical limitations, the distance between points is large, resulting in the measured interface transition zone range being inaccurate. Summary of the invention

[0007] The technical problems to be solved by the present invention are:

[0008] The purpose of the present invention is to provide a test method for measuring characteristic parameters of the interface transition zone of asphalt mixture, so as to solve the problem that the gap between nanoindentations in the existing test technology for characteristic parameters of the interface transition zone of asphalt mixture is large and the measured interface transition zone range is not accurate enough.

[0009] The present invention takes into account the phenomenon that there are differences in mechanical properties between the interface transition zone and asphalt under the interaction between asphalt and aggregate, and utilizes atomic force microscopic mechanical property testing technology to distinguish the interface transition zone, measure the microscopic mechanical properties, adhesion and thickness of the interface transition zone, and realize the characterization of the characteristic parameters of the interface transition zone.

[0010] The present invention adopts a technical solution to solve the above technical problems: a test method for measuring characteristic parameters of the transition zone of the asphalt mixture interface, comprising the following steps:

[0011] Step 1: Prepare Marshall specimens of asphalt mixture;

[0012] Step 2: Cutting the specimen: Use a metallographic cutting machine to cut the specimen (the size of the specimen after cutting is 15*15*15mm), and the specimen includes the aggregate-asphalt interface transition area; the metallographic cutting machine is within the existing technical scope;

[0013] Step 3: Grinding the specimen: Grinding the specimen with a metallographic grinder (using sandpaper of different mesh sizes) to make it flat, and then polishing it to obtain an atomic force microscope test specimen;

[0014] Step 4: Perform an atomic force microscope test on the polished sample: fix the atomic force microscope sample on the atomic force microscope test platform, select a clear and flat interface transition area between aggregate and asphalt under the atomic force microscope; set a test area in the interface transition area between aggregate and asphalt, use the peak force quantitative nanometer test mode to perform the atomic force microscope test, and use the NanoScope Analysis 3.0 software configured by the atomic force microscope to obtain the morphology (for viewing), modulus distribution map and adhesion distribution map of the test area; the adhesion distribution map reflects the strength of the adhesion interaction in the aggregate-asphalt interface transition zone in the specimen;

[0015] Step 5: Use NanoScope Analysis 3.0 software to analyze the obtained results (morphology of the test area, modulus distribution map, and adhesion distribution map):

[0016] The modulus distribution map and adhesion distribution map are processed by the section module of NanoScope Analysis 3.0 software (the modulus distribution map and adhesion distribution map are input to the section module, and the section module outputs data) to obtain the modulus value and adhesion value of each point at the selected position (straight line) in the test area;

[0017] Step 6: De-noise and smooth the modulus values ​​and adhesion values ​​at each position in the test area to obtain the modulus distribution curve and adhesion distribution curve at the selected position, where the range of continuous change is the asphalt mixture interface transition zone. By comparing the asphalt mixture interface transition zone on the modulus distribution curve and the asphalt mixture interface transition zone on the adhesion distribution curve, the thickness range of the asphalt mixture interface transition zone is obtained.

[0018] The present invention has the following beneficial effects:

[0019] The present invention provides a test method for measuring characteristic parameters of the asphalt mixture interface transition zone. According to the phenomenon that the mechanical properties of the asphalt mixture interface transition zone change, an atomic force microscope is used to perform a microscopic mechanical property test at the interface between the aggregate and the mortar in the asphalt mixture sample. The selected test area includes three phases: asphalt, aggregate and interface transition zone. The experimental results are obtained and the results are analyzed using NanoScope Analysis 3.0 software. By analyzing the modulus and adhesion distribution diagram, the thickness of the interface transition zone can be obtained, reflecting the strength of the adhesion interaction between the aggregate and the asphalt interface transition zone, and the quantitative characterization of characteristic parameters such as the thickness, mechanical properties and interaction strength of the asphalt mixture interface transition zone can be achieved.

[0020] Compared with the prior art, the present invention uses atomic force microscopy to measure the mechanical properties of each microscopic phase of asphalt mixture, and calculates the thickness of the interface transition zone according to the difference in mechanical properties between the interface transition zone and asphalt. It is a practical and feasible test method for characterizing the characteristic parameters of the microscopic interface transition zone of different asphalt mixtures. No one in the prior art has proposed to use atomic force microscopy to measure the mechanical properties of the interface transition zone of asphalt mixture. In contrast, most current studies regard the boundary zone between the two phases as a continuous and homogeneous interface phase, which has a large error from the actual situation. The empirical formula method or microscope observation can only obtain the thickness of the asphalt film between the two aggregates of the mixture, which is significantly different from the interface transition zone. The present invention measures and calculates the thickness of the interface transition zone of the asphalt mixture, and quantitatively characterizes the strength of the interaction between the aggregate and the asphalt interface transition zone, which can effectively improve the performance and durability of the asphalt mixture and provide more reliable material support for road construction and maintenance. Based on the solution proposed by the present invention, in future research, the relationship between the interface transition zone and the performance of other phase materials can be further explored to provide more theoretical guidance and practical experience for the design and application of high-performance asphalt mixtures.

[0021] In summary, the present invention can use atomic force microscopy to quickly obtain the distribution map of the morphology, modulus and adhesion of the three phases of asphalt, aggregate and interface transition zone in this area, and then use the section module of NanoScope Analysis 3.00 software to effectively determine the range of the interface transition zone and analyze its mechanical properties. Compared with the current nanoindentation SEM method, nanoindentation only makes points within the range, and determines the range of the interface transition zone by the number of points. SEM needs to be used in conjunction with FT-IR to identify the element distribution, the area is relatively fuzzy and the use is relatively cumbersome. The present invention (AFM) can accurately identify the location of the interface transition zone within the test range, and analyze the mechanical properties of the interface transition zone, and the test method is relatively simple and convenient. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] The present invention can be better understood by referring to the description given below in conjunction with the accompanying drawings, which together with the following detailed description are included in this specification and form a part of this specification, and are used to further illustrate the preferred embodiments of the present invention and explain the principles and advantages of the present invention.

[0023] Figure 1 A schematic diagram of an atomic force microscope specimen and an atomic force microscope test area of ​​the present invention;

[0024] Figure 2 Schematic diagram of the AFM test area under a microscopic microscope; in the figure: 1 is the specimen block, 3 is asphalt;

[0025] Figure 3 is the adhesion force and modulus distribution curve; Figure 3 It can be seen that the interface transition zone of asphalt mixture is found;

[0026] Among them, 1 is a small piece of asphalt mixture (specimen), 2 is aggregate phase, 3 is asphalt phase (light green), 4 is test area, 5 is interface transition area (micrometer level), 6 is atomic force microscope test area (one side of the specimen). Asphalt mixture is a typical composite material composed of asphalt, aggregate (coarse aggregate), mineral powder (fine aggregate), etc.

[0027] Figure 4 The AC-16 gradation curve is shown in Figure 1. Basalt aggregate and limestone powder are mixed as the first ore combination, and limestone aggregate and limestone powder are mixed as the second ore combination. Both ore combinations use AC-16 gradation. The gradation curve is shown in Figure 1. Figure 4 shown. DETAILED DESCRIPTION

[0028] Combination Figure 1-4The test method for measuring characteristic parameters of the asphalt mixture interface transition zone according to the present invention is described as follows, which comprises the following steps:

[0029] Step 1: Prepare Marshall specimens of asphalt mixture;

[0030] Step 2: Cutting the specimen: Use a metallographic cutting machine to cut the specimen (15*15*15mm after cutting), and the specimen includes the transition area between the aggregate and the asphalt interface;

[0031] Step 3: Grinding the specimen: Grinding the specimen with a metallographic grinder (using sandpaper of different mesh sizes) to make it flat, and then polishing it to obtain an atomic force microscope test specimen;

[0032] Step 4: Perform an atomic force microscope test on the polished sample: fix the atomic force microscope test sample on the atomic force microscope test platform, select a clear and flat interface transition area between aggregate and asphalt under the atomic force microscope; set a test area in the interface transition area between aggregate and asphalt, use the peak force quantitative nano test mode to perform the atomic force microscope test, and use the NanoScope Analysis 3.0 software configured by the atomic force microscope to obtain the morphology (for viewing), modulus distribution map and adhesion distribution map of the test area; the adhesion distribution map reflects the strength of the adhesion interaction in the aggregate-asphalt mortar interface transition zone in the specimen;

[0033] Step 5: Use NanoScope Analysis 3.0 software to analyze the obtained results (morphology of the test area, modulus distribution map, and adhesion distribution map):

[0034] The modulus distribution map and adhesion distribution map are processed by the section module of NanoScope Analysis 3.0 software (the modulus distribution map and adhesion distribution map are input to the section module, and the section module outputs data) to obtain the modulus value and adhesion value of each point at the selected position (straight line) in the test area;

[0035] Step 6: De-noise and smooth the modulus values ​​and adhesion values ​​at each position in the test area to obtain the modulus distribution curve and adhesion distribution curve at the selected position, where the range of continuous change is the asphalt mixture interface transition zone. By comparing the asphalt mixture interface transition zone on the modulus distribution curve and the asphalt mixture interface transition zone on the adhesion distribution curve, the thickness range of the asphalt mixture interface transition zone is obtained.

[0036] Basalt aggregate and limestone powder are mixed as the first ore combination, and limestone aggregate and limestone powder are mixed as the second ore combination. Both ore combinations adopt AC-16 grading. The grading curve is as follows: Figure 4 shown.

[0037] The first mineral material combination (basalt aggregate and limestone powder) and the second mineral material combination (limestone aggregate and limestone powder) were mixed with base asphalt and SBS modified asphalt respectively under AC-16 grading, and basalt asphalt mixture and limestone asphalt mixture were prepared by Marshall compaction.

[0038] The model of the metallographic cutting machine is SQ-100.

[0039] In step 3, the specimens are polished in sequence using metallographic sandpapers of different mesh sizes under cold water conditions, and polishing is performed using polishing cloth and polishing liquid.

[0040] The polishing liquid is a diamond polishing liquid with a particle size of W2.5. The specific operation is to wet the polishing cloth and fix it on a metallographic grinder, drip the polishing liquid, and start the grinder to polish the test piece.

[0041] The test area of ​​the atomic force microscope test in step 4 is 20×20 μm (20*20 micrometers, one ten-millionth of a millimeter).

[0042] The specific implementation steps of step 5 are as follows: import the test result image obtained in NanoScope Analysis 3.0 software, use the Flatten module to smooth the morphology image under the Height Sensor image; switch to the DMTmodulus image, use the Flatten module to smooth the morphology image, then select the section module, and measure the continuous change curve of the modulus distribution from the aggregate area to the asphalt area; switch to the Adhesion image, use the Flatten module to smooth the morphology image, then select the section module, and measure the continuous change curve of the adhesion distribution from the aggregate area to the asphalt area. Finally, the modulus and adhesion distribution curves are obtained according to the measurement, and the characteristics of the distribution curves are analyzed to obtain the range of the interface transition zone.

[0043] Embodiment: Step 1: prepare an asphalt mixture Marshall specimen; the asphalt mixture Marshall specimen in step 1 is prepared by mixing basalt aggregate, limestone aggregate, limestone mineral powder with base asphalt and SBS modified asphalt under AC-16 grading.

[0044] Step 2: Cutting the specimen: Use a metallographic cutting machine to cut the specimen, which includes the interface area between aggregate and asphalt;

[0045] Step 3: Grinding the specimen: Use a metallographic cutting machine and a metallographic grinder to grind the specimen flat, and then polish it to obtain an atomic force microscope test specimen; in step 3, use metallographic sandpaper of different mesh sizes to grind the specimen in turn under cold water conditions, and polish it with a polishing cloth and polishing liquid.

[0046] Step 4: Atomic force microscope test: Fix the tested specimen on the atomic force microscope test platform, select a clear and flat interface area between aggregate and asphalt under the microscope of the atomic force microscope; set up a test area in the interface area between aggregate and asphalt, use the peak force mode to perform the atomic force microscope test, and obtain the morphology, modulus distribution map and adhesion distribution map of the test area; the test area of ​​the atomic force microscope test in step 4 is 20×20μm. Specific implementation steps of step 4: Import the test result image obtained in NanoScope Analysis 3.0 software, extract the morphology, modulus distribution map and adhesion distribution map, select the section module for analysis, obtain the modulus and adhesion distribution curves, analyze the distribution curves, and obtain the range of the interface transition zone.

[0047] Step 5: Use NanoScope Analysis 3.0 software to analyze the results obtained, determine the range of the interface transition zone, and determine the range of the interface transition zone based on the position of the test points;

[0048] Step 6: Based on the adhesion force distribution diagram, reflect the strength of the adhesion interaction in the transition zone between the aggregate and asphalt interface in the specimen.

[0049] Embodiment: The present invention is further described below in conjunction with the accompanying drawings:

[0050] The atomic force microscopy technology in the present invention is a test method for measuring the microscopic mechanical properties of materials. The test is based on the van der Waals force between the probe and the sample. Therefore, the method is not affected by the conductive properties of the sample and can be used for the study of insulators, semiconductors, and conductors. The imaging principle is that when the probe scans the sample surface, the force between the probe and the sample will cause the probe cantilever to deflect, and the photodetector collects the curvature or deflection of the cantilever beam. After computer processing, an image of the surface morphology can be generated. The peak force mode principle is to use a fixed frequency of 2kHz to make a force curve at each pixel on the sample surface. During the force curve, the maximum value of the force applied by the probe to the sample is called the peak force. The peak force is used for feedback, and the peak force between the probe and the sample is kept constant by moving the scanning tube, thereby reflecting the morphology and mechanical properties of the sample. With the help of a high-definition microscope in an atomic force microscope, the probe can realize the test of the mechanical properties of different phases of materials inside the composite material. Therefore, the atomic force microscopy technology is suitable for measuring the mechanical property differences of each microscopic material phase in asphalt mixture, thereby distinguishing the interface transition zone and realizing the characterization of the characteristic parameters of the interface transition zone.

[0051] Example:

[0052] This embodiment uses the following steps to measure the characteristic parameters of the asphalt mixture interface transition zone:

[0053] Preparation of test specimens: The first mineral material combination (basalt aggregate and limestone powder) and the second mineral material combination (limestone aggregate and limestone powder) were mixed with base asphalt and SBS modified asphalt respectively under AC-16 grading, and basalt asphalt mixture and limestone asphalt mixture were prepared by Marshall compaction. Subsequently, the formed asphalt mixture was cut into asphalt mixture blocks 1 with a length and width of 1-1.5 cm and a height of about 1 cm. The asphalt mixture blocks 1 were required to contain a test area 4 of uniform and flat aggregate and asphalt mortar;

[0054] Grinding the specimen: Use a metallographic grinder with 240, 400, 800, and 1200 mesh metallographic sandpaper to grind the specimen under water cooling until the surface is smooth. It is required to first use 240 mesh sandpaper to initially grind the surface of the small piece of asphalt mixture flat, and then use 400-1200 mesh sandpaper to grind the surface one by one until it is smooth. The grinding time for each mesh sandpaper is 2 minutes. After grinding and cleaning, polishing treatment is performed. The particle size of the polishing liquid used is W2.5, and the atomic force microscope test specimen is obtained;

[0055] Atomic force microscopy test: fix the test specimen on the atomic force microscopy test platform, select a clear and flat interface area between aggregate and asphalt mortar under the microscope of the atomic force microscopy instrument, set up a test area in the interface area between aggregate and asphalt, and the atomic force microscopy test test area is 20×20μm, including the interface transition zone, aggregate and asphalt three phases. The atomic force microscopy test is carried out in peak force mode to obtain the morphology, modulus distribution map and adhesion distribution map of the test area.

[0056] Analysis of interface transition zone thickness: The test result image was imported into NanoScope Analysis 3.0 software, and the morphology, modulus distribution diagram and adhesion distribution diagram were extracted. The section module was selected for analysis to obtain the modulus and adhesion distribution curves. The distribution curves were analyzed to obtain the range of the interface transition zone. The thickness range of the interface transition zone between basalt aggregate and asphalt was 6 to 8 μm, and the thickness range of the interface transition zone between limestone aggregate and asphalt was 8 to 12 μm.

[0057] Comparison of adhesion in the interface transition zone: The adhesion and modulus of the interface transition zone of SBS modified asphalt mixture are significantly higher than those of the interface transition zone of base asphalt mixture, the modulus of the interface transition zone of basalt asphalt mixture is higher than that of limestone asphalt mixture, and the adhesion of the interface transition zone of basalt asphalt mixture is lower than that of limestone asphalt mixture. This reflects the strength of the adhesion interaction in the aggregate-asphalt mortar interface transition zone in different mixture samples.

[0058] It should be understood that the various forms of processes shown above can be used to reorder, add or delete steps. As long as the expected results of the technical solutions disclosed in this application can be achieved, they are all within the protection scope of the present invention.

[0059] Although the present invention has been described according to a limited number of embodiments, it will be apparent to those skilled in the art, with the benefit of the above description, that other embodiments are contemplated within the scope of the invention thus described. The disclosure of the present invention is intended to be illustrative rather than restrictive of the scope of the invention, which is defined by the appended claims.

Claims

1. A test method for measuring characteristic parameters of the transition zone of the asphalt mixture interface. Features: The following steps are involved: Step 1: Prepare Marshall specimens of asphalt mixture; Step 2: Cutting the specimen: Use a metallographic cutting machine to cut the specimen, which includes the transition area between the aggregate and asphalt interface; Step 3: Grinding the specimen: Grinding the specimen flat with a metallographic grinder, and then polishing it to obtain an atomic force microscope test specimen; Step 4: Perform an atomic force microscope test on the polished sample: fix the atomic force microscope test sample on the atomic force microscope test platform, and select a clear and flat interface transition area between aggregate and asphalt under the atomic force microscope; A test area was set up in the transition area between aggregate and asphalt interface, and the atomic force microscope test was carried out using the peak force quantitative nano-test mode. The morphology, modulus distribution map and adhesion distribution map of the test area were obtained using the NanoScope Analysis 3.0 software configured with the atomic force microscope. The adhesion distribution map reflects the strength of the adhesion interaction in the transition area between the aggregate and asphalt mortar interface in the specimen. Step 5: Use NanoScope Analysis 3.0 software to analyze the obtained results, the morphology of the test area, the modulus distribution map, and the adhesion distribution map: The modulus distribution map and adhesion distribution map were processed by the section module of NanoScope Analysis 3.0 software to obtain the modulus value and adhesion value of each point in the selected position of the test area; Step 6: De-noise and smooth the modulus values ​​and adhesion values ​​at each position in the test area to obtain the modulus distribution curve and adhesion distribution curve at the selected position, where the range of continuous change is the asphalt mixture interface transition zone. By comparing the asphalt mixture interface transition zone on the modulus distribution curve and the asphalt mixture interface transition zone on the adhesion distribution curve, the thickness range of the asphalt mixture interface transition zone is obtained.

2. A test method for measuring characteristic parameters of the asphalt mixture interface transition zone according to claim 1, Features: Basalt aggregate and limestone powder are mixed as the first aggregate combination, and limestone aggregate and limestone powder are mixed as the second aggregate combination. Both aggregate combinations adopt AC-16 grading. The first mineral aggregate combination and the second mineral aggregate combination were mixed with base asphalt and SBS modified asphalt respectively under AC-16 grading, and basalt asphalt mixture and limestone asphalt mixture were prepared by Marshall compaction.

3. A test method for measuring characteristic parameters of the asphalt mixture interface transition zone according to claim 1 or 2, Features: The model of the metallographic cutting machine is SQ-100.

4. A test method for measuring characteristic parameters of an asphalt mixture interface transition zone according to claim 1, Features: In step 3, the specimens are polished in sequence using metallographic sandpapers of different mesh sizes under cold water conditions, and polishing is performed using polishing cloth and polishing liquid.

5. A test method for measuring characteristic parameters of the asphalt mixture interface transition zone according to claim 4, Features: The polishing liquid is a diamond polishing liquid with a particle size of W2.

5. The specific operation is to wet the polishing cloth and fix it on a metallographic grinder, drip the polishing liquid, and start the grinder to polish the test piece.

6. A test method for measuring characteristic parameters of an asphalt mixture interface transition zone according to claim 1, Features: The test area of ​​the atomic force microscope test in step 4 is 20×20 μm.

7. A test method for measuring characteristic parameters of an asphalt mixture interface transition zone according to claim 1, Features: The specific implementation steps of step 5 are as follows: import the test result image obtained in NanoScope Analysis 3.0 software, use the Flatten module to smooth the morphology image under the Height Sensor image; switch to the DMTmodulus image, use the Flatten module to smooth the morphology image, then select the section module, and measure the continuous change curve of the modulus distribution from the aggregate area to the asphalt area; switch to the Adhesion image, use the Flatten module to smooth the morphology image, then select the section module, and measure the continuous change curve of the adhesion distribution from the aggregate area to the asphalt area. Finally, the modulus and adhesion distribution curves are obtained according to the measurement, and the characteristics of the distribution curves are analyzed to obtain the range of the interface transition zone.

Citation Information

Cited By

  • Method for evaluating water stability of asphalt mixture

    CN120044087A

  • Method for dividing RAP aggregate interface transition area in recycled asphalt mixture

    CN120539196A

  • Asphalt mineral powder interface modulus distribution calculation method, system and equipment and storage medium

    CN120977448A