LED packaging adhesive performance reliability initial evaluation method

By conducting an initial evaluation of LED encapsulation adhesive, preparing encapsulated LED beads and adhesive block samples, testing key indicators, and screening out qualified adhesives, the problem of consuming a large amount of resources in existing technologies is solved, and efficient adhesive screening and evaluation is achieved.

CN119000862APending Publication Date: 2024-11-22SUZHOU KINGLIGHT OPTOELECTRONICS CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411002278.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The performance evaluation process of LED encapsulating adhesives in the current technology consumes a lot of manpower, material resources and time, and lacks efficient screening and evaluation methods.

Method used

An initial evaluation method is adopted, which involves preparing encapsulated LED chip samples and encapsulated adhesive block samples, and testing indicators such as light decay retention rate, glass transition temperature, coefficient of thermal expansion and hardness. The encapsulated adhesives that are qualified in the initial stage are screened out, and only a comprehensive evaluation is carried out on them in the later stage, which saves manpower, material resources and time.

Benefits of technology

By simplifying the initial evaluation process, unqualified encapsulating adhesives can be quickly screened out, ensuring the effectiveness of subsequent evaluations, saving manpower, resources, and time, while meeting the requirements of the encapsulation process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119000862A_ABST
    Figure CN119000862A_ABST
Patent Text Reader

Abstract

The invention discloses an initial evaluation method for reliability of LED packaging glue. The method comprises the following steps: step 1, preparing a packaging lamp bead sample and a packaging glue block sample by using to-be-tested packaging glue; 2, testing an initial evaluation index of the packaged lamp bead sample and an initial evaluation index of the packaged rubber block sample; 3, judging whether the initial evaluation index of the packaging lamp bead sample and the initial evaluation index of the packaging glue block sample are in respective preset ranges, if so, determining that the initial evaluation of the packaging glue to be tested is qualified, and entering a later evaluation step; wherein the initial evaluation indexes of the packaged lamp bead sample comprise the light attenuation maintenance rate, and the initial evaluation indexes of the packaged rubber block sample comprise the glass transition temperature, the thermal expansion coefficient and the hardness. According to the invention, the initial evaluation index of the packaging lamp bead sample and the initial evaluation index of the packaging adhesive block sample are tested, and whether the initial evaluation of the packaging adhesive to be tested is qualified or not is tested through several simple indexes, so that manpower, material resources and time are greatly saved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of LEDs, and in particular to an initial reliability evaluation method for LED packaging adhesive performance. Background Art

[0002] LED packaging technology plays a vital role in the quality of LED products, especially the screening and preparation of packaging glue is a key factor. Glue manufacturers often only evaluate the performance of the resin material itself, and do not conduct a good performance evaluation on the actual packaging lamp bead sample products. After the packaging manufacturer gets the packaging glue, it is necessary to test multiple indicators of the packaging glue. Each indicator test requires the production of a corresponding sample, and some indicators take a long time to test, which requires a lot of manpower, material resources and time. How to save manpower, material resources and time in the evaluation process of LED packaging glue performance is a technical problem that needs to be solved urgently in this field. Summary of the invention

[0003] Therefore, the technical problem to be solved by the present invention is to provide an initial reliability evaluation method for LED packaging adhesive performance that saves manpower, material resources and time.

[0004] In order to solve the above technical problems, the present invention provides a method for evaluating the reliability of LED packaging adhesive performance in an initial stage, comprising the following initial evaluation steps:

[0005] Step 1, preparing packaged lamp bead samples and packaged glue block samples using the packaged glue to be tested;

[0006] Step 2, testing the initial evaluation indexes of the packaged lamp bead samples and the initial evaluation indexes of the packaged rubber block samples;

[0007] Step 3, judging whether the initial evaluation index of the packaged lamp bead sample and the initial evaluation index of the packaged glue block sample are both within their respective preset ranges. If so, the initial evaluation of the packaged glue to be tested is qualified and enters the post-evaluation step; if not, the packaged glue to be tested is unqualified;

[0008] Among them, the initial evaluation indicators of the packaged lamp bead samples include the light decay maintenance rate, and the initial evaluation indicators of the packaged rubber block samples include the glass transition temperature, thermal expansion coefficient and hardness.

[0009] Furthermore, the preset range of the light decay maintenance rate of the packaged lamp bead sample is greater than 95%.

[0010] Furthermore, the preset range of the glass transition temperature of the encapsulation rubber block sample is 110-140°C.

[0011] Furthermore, the preset range of the glass transition temperature of the encapsulation rubber block sample is 120-130°C.

[0012] Furthermore, the preset range of the thermal expansion coefficient of the packaging rubber block sample in an environment of 60-80° C. is less than 50 ppm.

[0013] Furthermore, the preset range of the thermal expansion coefficient of the packaging rubber block sample in an environment of 160-180° C. is less than 110 ppm.

[0014] Furthermore, the preset range of the hardness of the packaging rubber block sample is greater than 85D.

[0015] Furthermore, the initial evaluation index of the encapsulated rubber block sample also includes whiteness decay rate.

[0016] Furthermore, the preset range of the whiteness decay rate of the packaging rubber block sample is less than 10%.

[0017] Furthermore, the preset range of the whiteness decay rate of the packaging rubber block sample is less than 6.5%.

[0018] The above-mentioned technical scheme of the present invention has the following advantages over the prior art: the reliability initial evaluation method of the performance of LED packaging glue described in the present invention, when evaluating the performance of LED packaging glue, first performs an initial evaluation, tests the initial evaluation indicators of the packaging lamp bead samples and the initial evaluation indicators of the packaging glue block samples, screens out the packaging glue with unqualified initial evaluation indicators, and only performs a post-evaluation on the packaging glue with qualified initial evaluation indicators, and tests other evaluation indicators of the packaging lamp bead samples, saving manpower, material resources and time; further, the initial evaluation indicators of the packaging lamp bead samples include the light decay maintenance rate, and the initial evaluation indicators of the packaging glue block samples include the glass transition temperature, the thermal expansion coefficient and the hardness. The time required for testing these indicators is short, and when these initial evaluation indicators are all qualified, it is experimentally verified that the ultrasonic scanning of the packaging lamp bead samples is good, the PCT24H aging test results are OK, the TS200 rounds of hot and cold shock test results are OK, the packaging process effect and reliability of the packaging lamp bead samples and the packaging glue block samples meet the requirements, and the initial evaluation of the packaging glue to be tested is tested to determine whether it is qualified, further saving manpower, material resources and time. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] In order to make the contents of the present invention more clearly understood, the present invention is further described in detail below based on specific embodiments of the present invention in conjunction with the accompanying drawings.

[0020] Figure 1 The present invention is a flow chart of the method for initially evaluating the reliability of LED packaging glue performance.

[0021] Figure 2 The test results of the initial evaluation indicators of various embodiments of the present invention;

[0022] Figure 3 The ultrasonic scanning results, aging test results, and thermal shock results of various embodiments of the present invention are shown. DETAILED DESCRIPTION

[0023] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.

[0024] See also Figure 1 As shown, it is a flow chart of the method for initial reliability evaluation of LED packaging adhesive performance in the present invention.

[0025] The initial evaluation method for the reliability of LED encapsulation adhesive performance includes the following initial evaluation steps:

[0026] Step 1, preparing packaged lamp bead samples and packaged glue block samples using the packaged glue to be tested;

[0027] Step 2, testing the initial evaluation indexes of the packaged lamp bead samples and the initial evaluation indexes of the packaged rubber block samples;

[0028] Step 3: determine whether the initial evaluation index of the packaged lamp bead sample and the initial evaluation index of the packaged glue block sample are both within their respective preset ranges. If so, the initial evaluation of the packaged glue to be tested is qualified and enters the post-evaluation step; if not, the packaged glue to be tested is unqualified;

[0029] Among them, the initial evaluation indicators of the packaged lamp bead samples include the light decay maintenance rate, and the initial evaluation indicators of the packaged rubber block samples include the glass transition temperature, thermal expansion coefficient and hardness.

[0030] In step one, the encapsulated lamp bead samples and encapsulated rubber block samples are formed by preparing glue, dispensing glue, and curing. When preparing glue, the glue can be mixed by vacuum degassing and stirring equipment, and the mixed bubbles in the raw materials can be squeezed out by vacuum technology. The principle is to use a vacuum pump to evacuate the vacuum and use the air pressure difference to squeeze out the bubbles inside the product. This technology can effectively remove the bubbles in the glue to prevent these bubbles from affecting the further processing of the glue. The mixed glue is applied to the lamp bead shell and cured to form an encapsulated lamp bead sample. After the mixed glue is cured in the mold shell, it is divided into encapsulated rubber block samples by conventional methods such as mechanical cutting. The rubber block can also be made with the help of an easy-to-demold mold, which is convenient and quick. The easy-to-demold mold is made of polytetrafluoroethylene material. It should be noted that the number of encapsulated lamp bead samples made by each encapsulation glue is consistent with the number of its initial evaluation indicators, and the number of encapsulated rubber block samples made by each encapsulation glue is consistent with the number of its initial evaluation indicators.

[0031] In step 2, the light decay maintenance rate of the packaged lamp bead sample refers to the ratio of the luminous flux of the packaged lamp bead sample at a specific time during its life span to the initial luminous flux of the lamp, expressed as a percentage. As time goes by, the luminous flux of the light source will decrease, and the effective life is defined according to the luminous flux maintenance rate. The light decay maintenance rate of the packaged lamp bead sample is measured using a German IS standard machine and an energy device. The energy device may include a heating device and a UV test chamber. The heating device may be a high-temperature oven and a tunnel oven, etc. The UV test chamber may be operated under UV light irradiation conditions in different bands. The energy shock can be carried out in different environments to simulate the future use environment of the LED packaged lamp beads, which is closer to actual use.

[0032] The glass transition temperature (tg) of the encapsulated rubber block sample refers to the temperature corresponding to the transition of the encapsulated rubber block sample from the glass state to the highly elastic state. The thermal expansion coefficient of the encapsulated rubber block sample refers to the change in the length value of the encapsulated rubber block sample caused by a unit temperature change. The glass transition temperature and thermal expansion coefficient of the encapsulated rubber block sample were measured using the Japanese Hitachi Q700TMA instrument: a disc with a diameter of 5cm and a thickness of 2cm was made, and the test conditions were 25-200C, 3C / min for measurement. The determination of the glass transition temperature is to use the extrapolation method on the test curve within the above temperature test range to fit the inflection point value.

[0033] The hardness of the encapsulated rubber block sample refers to the material's ability to resist a hard object from pressing into its surface. Use a Shore hardness tester to measure the hardness of the encapsulated rubber block sample. First, turn on the machine and reset it, then adjust the upper and lower spacing by 1 cm and then conduct the test.

[0034] In some embodiments, the preset range of the light decay maintenance rate of the packaged lamp bead sample is greater than 95%.

[0035] In some embodiments, the preset range of the glass transition temperature of the encapsulation block sample is 110-140°C.

[0036] In some embodiments, the preset range of the glass transition temperature of the encapsulation block sample is 120-130°C.

[0037] In some embodiments, the predetermined range of the thermal expansion coefficient of the packaging block sample in an environment of 60-80° C. is less than 50 ppm.

[0038] In some embodiments, the predetermined range of the thermal expansion coefficient of the packaging block sample in an environment of 160-180° C. is less than 110 ppm.

[0039] In some embodiments, the preset range of the hardness of the packaging block sample is greater than 85D.

[0040] In some embodiments, the initial evaluation index of the packaging rubber block sample further includes whiteness decay rate.

[0041] Since the overall quality of current LED packaging glue is good, the whiteness decay rate of most packaging glue block samples of LED packaging glue supports can meet the standards. Therefore, the whiteness decay rate of the packaging glue block samples is used as an optional initial evaluation indicator. A whiteness meter and an energy device are used to measure the whiteness decay rate of the glue block. The energy device can include a heating device and a UV test chamber. The heating device can be a high-temperature oven and a tunnel oven, etc. The UV test chamber can be operated under UV light irradiation conditions in different bands. Energy impact can be carried out in different environments to simulate the future use environment of LED packaging lamp beads, which is closer to actual use.

[0042] In some embodiments, the preset range of the whiteness decay rate of the packaging rubber block sample is less than 10%.

[0043] In some embodiments, the preset range of the whiteness decay rate of the packaging rubber block sample is less than 6.5%.

[0044] Example 1

[0045] The reliability initial evaluation method of LED packaging adhesive performance includes the following initial evaluation steps:

[0046] Step 1: Select the LED encapsulation glue EC019 currently used in the production line, mix glue A and glue B, dispense glue, and cure to form encapsulated lamp bead samples and prepare encapsulated glue block samples;

[0047] Step 2: Test the light decay maintenance rate of the packaged lamp bead sample and the glass transition temperature, thermal expansion coefficient, whiteness decay rate and hardness of the packaged rubber block sample. The light decay maintenance rate of the packaged lamp bead sample is 95.45%, the glass transition temperature of the packaged rubber block sample is 130.5°C, the thermal expansion coefficient in the environment of 60-80°C is 41.1, the thermal expansion coefficient in the environment of 160-180°C is 104.7, the whiteness decay rate is 6.24%, and the hardness is 88D;

[0048] Step three, compare the light decay maintenance rate of the packaged lamp bead samples and the glass transition temperature, thermal expansion coefficient, whiteness decay rate and hardness of the packaging glue block samples with their respective preset ranges. If the light decay maintenance rate of the packaged lamp bead samples and the glass transition temperature, thermal expansion coefficient, whiteness decay rate and hardness of the packaging glue block samples are all qualified, the initial evaluation of the packaging glue to be tested is qualified, and the later reliability evaluation of the packaging glue can be carried out.

[0049] In order to further verify the effectiveness of the initial reliability evaluation method of the LED encapsulation adhesive in Example 1, the following tests were performed on the encapsulated lamp bead samples:

[0050] The packaged lamp bead samples are subjected to ultrasonic scanning, aging test and hot and cold shock test. Ultrasonic scanning is a means of detecting impurities, cracks and gaps in LED lamp beads, and the effect of the packaging process is quickly evaluated through color changes. Reliability evaluation refers to the tolerance test of packaged lamp bead samples under different environments, and the state of the LED lamp beads is used as the judgment. If there is no dead light or dim light, it is OK, and if there is any one of them, it is NG. The specific implementation environment of the aging test is 125℃, 100% humidity and 1.5 atmospheres, which is called the PCT experiment; the hot and cold shock test is 200 rounds of hot and cold shock in an environment of -40-100℃, which is called the TS test.

[0051] After testing, the ultrasonic scanning, aging test and hot and cold shock test of the packaged lamp bead samples all passed.

[0052] Example 2

[0053] The reliability initial evaluation method of LED packaging adhesive performance includes the following initial evaluation steps:

[0054] Step 1: Select a packaging glue EC012 that has just been sent by a glue manufacturer, mix glue A and glue B, dispense glue, and cure to form packaging lamp bead samples and packaging glue block samples;

[0055] Step 2: Test the light decay maintenance rate of the packaged lamp bead sample and the glass transition temperature, thermal expansion coefficient, whiteness decay rate and hardness of the packaged rubber block sample. The light decay maintenance rate of the packaged lamp bead sample is 96.05%, the glass transition temperature of the packaged rubber block sample is 128.4°C, the thermal expansion coefficient in the environment of 60-80°C is 37.7, the thermal expansion coefficient in the environment of 160-180°C is 74.7, the whiteness decay rate is 5.64%, and the hardness is 87D;

[0056] Step three, compare the light decay maintenance rate of the packaged lamp bead samples and the glass transition temperature, thermal expansion coefficient, whiteness decay rate and hardness of the packaging glue block samples with their respective preset ranges. If the light decay maintenance rate of the packaged lamp bead samples and the glass transition temperature, thermal expansion coefficient, whiteness decay rate and hardness of the packaging glue block samples are all qualified, the initial evaluation of the packaging glue to be tested is qualified, and the later reliability evaluation of the packaging glue can be carried out.

[0057] In order to further verify the effectiveness of the initial reliability evaluation method of the LED encapsulation adhesive in this embodiment 2, the following tests were performed on the encapsulated lamp bead samples:

[0058] The packaged lamp bead samples are subjected to ultrasonic scanning, aging test and hot and cold shock test. Ultrasonic scanning is a means of detecting impurities, cracks and gaps in LED lamp beads, and the effect of the packaging process is quickly evaluated through color changes. Reliability evaluation refers to the tolerance test of packaged lamp bead samples under different environments, and the state of the LED lamp beads is used as the judgment. If there is no dead light or dim light, it is OK, and if there is any one of them, it is NG. The specific implementation environment of the aging test is 125℃, 100% humidity and 1.5 atmospheres, which is called the PCT experiment; the hot and cold shock test is 200 rounds of hot and cold shock in an environment of -40-100℃, which is called the TS test.

[0059] After testing, the ultrasonic scanning, aging test and hot and cold shock test of the packaged lamp bead samples all passed.

[0060] Example 3

[0061] The reliability initial evaluation method of LED packaging adhesive performance includes the following initial evaluation steps:

[0062] Step 1: Select a packaging glue 2259C that has just been sent by a glue manufacturer, mix glue A and glue B, dispense glue, and cure to form packaging lamp bead samples and packaging glue block samples;

[0063] Step 2: Test the light decay maintenance rate of the packaged lamp bead sample and the glass transition temperature, thermal expansion coefficient, whiteness decay rate and hardness of the packaged rubber block sample. The light decay maintenance rate of the packaged lamp bead sample is 97.32%, the glass transition temperature of the packaged rubber block sample is 108.2°C, the thermal expansion coefficient in the environment of 60-80°C is 52.6, the thermal expansion coefficient in the environment of 160-180°C is 124.1, the whiteness decay rate is 6.58%, and the hardness is 80D;

[0064] Step three, compare the light decay maintenance rate of the packaged lamp bead sample and the glass transition temperature, thermal expansion coefficient, whiteness decay rate and hardness of the packaged glue block sample with their respective preset ranges, the initial evaluation of the light decay maintenance rate of the packaged lamp bead sample is qualified, the glass transition temperature of the packaged glue block sample is unqualified, the thermal expansion coefficient of the packaged glue block sample is unqualified, the whiteness decay rate of the packaged glue block sample is qualified, the hardness of the packaged glue block sample is unqualified, the initial evaluation of the tested packaging glue is unqualified, and there is no need to conduct a later reliability evaluation on the packaging glue;

[0065] In order to further verify the effectiveness of the initial reliability evaluation method of the LED encapsulation adhesive in this embodiment 3, the following tests were performed on the encapsulated lamp bead samples:

[0066] The packaged lamp bead samples are subjected to ultrasonic scanning, aging test and hot and cold shock test. Ultrasonic scanning is a means of detecting impurities, cracks and gaps in LED lamp beads, and the effect of the packaging process is quickly evaluated through color changes. Reliability evaluation refers to the tolerance test of packaged lamp bead samples under different environments, and the state of the LED lamp beads is used as the judgment. If there is no dead light or dim light, it is OK, and if there is any one of them, it is NG. The specific implementation environment of the aging test is 125℃, 100% humidity and 1.5 atmospheres, which is called the PCT experiment; the hot and cold shock test is 200 rounds of hot and cold shock in an environment of -40-100℃, which is called the TS test.

[0067] After testing, the ultrasonic scanning of the packaged lamp bead samples failed, the aging test of the packaged lamp bead samples failed, the hot and cold shock test of the packaged lamp bead samples failed, and the reliability evaluation of the packaging glue to be tested failed.

[0068] Example 4

[0069] The reliability initial evaluation method of LED packaging adhesive performance includes the following initial evaluation steps:

[0070] Step 1: Select a packaging glue 3001A just sent by a glue manufacturer, mix, dispense and cure glue A and glue B to form packaging lamp bead samples and packaging glue block samples;

[0071] Step 2: Test the light decay maintenance rate of the packaged lamp bead sample and the glass transition temperature, thermal expansion coefficient, whiteness decay rate and hardness of the packaged rubber block sample. The light decay maintenance rate of the packaged lamp bead sample is 96.59%, the glass transition temperature of the packaged rubber block sample is 120.7°C, the thermal expansion coefficient in the environment of 60-80°C is 48.6, the thermal expansion coefficient in the environment of 160-180°C is 114.8, the whiteness decay rate is 4.71%, and the hardness is 85D;

[0072] Step three, compare the light decay maintenance rate of the packaged lamp bead sample and the glass transition temperature, thermal expansion coefficient, whiteness decay rate and hardness of the packaging glue block sample with their respective preset ranges. The initial evaluation of the light decay maintenance rate of the packaged lamp bead sample is qualified, the glass transition temperature of the packaging glue block sample is qualified, the thermal expansion coefficient of the packaging glue block sample is unqualified, the whiteness decay rate of the packaging glue block sample is qualified, the hardness of the packaging glue block sample is qualified, and the initial evaluation of the packaging glue to be tested is unqualified, and there is no need to conduct a subsequent reliability evaluation on the packaging glue.

[0073] In order to further verify the effectiveness of the initial reliability evaluation method of the LED encapsulation adhesive in this embodiment 4, the following tests were performed on the encapsulated lamp bead samples:

[0074] The packaged lamp bead samples are subjected to ultrasonic scanning, aging test and hot and cold shock test. Ultrasonic scanning is a means of detecting impurities, cracks and gaps in LED lamp beads, and the effect of the packaging process is quickly evaluated through color changes. Reliability evaluation refers to the tolerance test of packaged lamp bead samples under different environments, and the state of the LED lamp beads is used as the judgment. If there is no dead light or dim light, it is OK, and if there is any one of them, it is NG. The specific implementation environment of the aging test is 125℃, 100% humidity and 1.5 atmospheres, which is called the PCT experiment; the hot and cold shock test is 200 rounds of hot and cold shock in an environment of -40-100℃, which is called the TS test.

[0075] After testing, the ultrasonic scanning of the packaged lamp bead samples failed, the aging test of the packaged lamp bead samples passed, the hot and cold shock test of the packaged lamp bead samples failed, and the reliability evaluation of the packaging glue to be tested failed.

[0076] from Figure 2 and Figure 3 It can be seen that the ultrasonic scanning results of LED package lamp beads, PCT24H aging test results and TS200 rounds of hot and cold shock test results are related to the TG glass transition temperature, thermal expansion coefficient α1, thermal expansion coefficient α2 and hardness of the packaging glue.

[0077] In the prior art, the four packaging glues of Example 1 and Example 4 are all subjected to complete reliability test evaluation (needing to undergo high temperature and high humidity test for 14 days, high and low temperature test for 14 days, water bath test for 7 days, salt water test for 2 days, stewing box test for 3 days, and red ink test for 2 days) before qualified packaging glue can be tested.

[0078] In the present invention, the two packaging glues of Example 1 and Example 2 were subjected to complete reliability test evaluation, and the two glues of Example 3 and Example 4 were only subjected to initial reliability evaluation, and qualified packaging glues were tested.

[0079] Those skilled in the art know that when testing packaging glue, operators, testing equipment and time are all indispensable, therefore, in the prior art, four embodiments are subjected to complete reliability test evaluation, while in the present invention, two embodiments are subjected to complete reliability test evaluation, and the other two embodiments are subjected to only initial reliability evaluation, which greatly saves manpower, material resources and time.

[0080] Obviously, the above embodiments are merely examples for clear explanation and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the protection scope of the invention.

Claims

1. A method for evaluating the reliability of LED packaging adhesive performance in an early stage, characterized in that: The initial evaluation steps include: Step 1, preparing packaged lamp bead samples and packaged glue block samples using the packaged glue to be tested; Step 2, testing the initial evaluation indexes of the packaged lamp bead samples and the initial evaluation indexes of the packaged rubber block samples; Step 3, judging whether the initial evaluation index of the packaged lamp bead sample and the initial evaluation index of the packaged glue block sample are both within their respective preset ranges. If so, the initial evaluation of the packaged glue to be tested is qualified and enters the post-evaluation step; if not, the packaged glue to be tested is unqualified; Among them, the initial evaluation indicators of the packaged lamp bead samples include the light decay maintenance rate, and the initial evaluation indicators of the packaged rubber block samples include the glass transition temperature, thermal expansion coefficient and hardness.

2. The method for early reliability evaluation of LED packaging adhesive performance according to claim 1, characterized in that: The preset range of the light decay maintenance rate of the packaged lamp bead sample is greater than 95%.

3. The method for early reliability evaluation of LED packaging adhesive performance according to claim 1, characterized in that: The preset range of the glass transition temperature of the encapsulation block sample is 110-140°C.

4. The method for early reliability evaluation of LED packaging adhesive performance according to claim 3, characterized in that: The preset range of the glass transition temperature of the encapsulation block sample is 120-130°C.

5. The method for early reliability evaluation of LED packaging adhesive performance according to claim 1, characterized in that: The preset range of the thermal expansion coefficient of the packaging rubber block sample in an environment of 60-80° C. is less than 50 ppm.

6. The method for early reliability evaluation of LED packaging adhesive performance according to claim 1, characterized in that: The preset range of the thermal expansion coefficient of the packaging rubber block sample in an environment of 160-180° C. is less than 110 ppm.

7. The method for early reliability evaluation of LED packaging adhesive performance according to claim 1, characterized in that: The preset range of the hardness of the encapsulation block sample is greater than 85D.

8. The method for early reliability evaluation of LED packaging adhesive performance according to claim 1, characterized in that: The initial evaluation index of the encapsulated rubber block samples also includes the whiteness decay rate.

9. The method for early reliability evaluation of LED packaging adhesive performance according to claim 7, characterized in that: The preset range of the whiteness decay rate of the packaging rubber block sample is less than 10%.

10. The method for early reliability evaluation of LED packaging adhesive performance according to claim 9, characterized in that: The preset range of the whiteness decay rate of the packaging rubber block sample is less than 6.5%.