Method for preparing solar cell, solar cell and application of solar cell

By optimizing the process conditions and annealing treatment of ALD deposition alumina layer, the hydrogen atom content in the alumina layer is reduced, and a dense silicon oxide layer is formed by oxidizing gas, which solves the film explosion problem caused by high-temperature treatment and improves the solar cell Chemical passivation effect and photoelectric conversion efficiency.

CN119008775AActive Publication Date: 2024-11-22TRINA SOLAR CO LTD

Patent Information

Application Number
CN202411109453.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-22
Estimated Expiration
2044-08-13

AI Technical Summary

Technical Problem

During the production process of solar cells, high-temperature treatment causes excessive hydrogen atoms in the alumina layer to overflow, forming hydrogen to break through the silicon nitride film layer, destroying the integrity of the alumina and silicon nitride stack, and reducing battery efficiency.

Method used

By optimizing the process conditions for deposition of ALD alumina layer, the content of hydrogen atoms in the alumina layer is reduced, and oxidation gas is introduced during the annealing process to form a dense silicon oxide layer, reducing the density of interfacial defect states and ensuring chemical passivation effect.

Benefits of technology

It effectively reduces the risk of explosive film of the alumina layer and improves the chemical passivation effect and photoelectric conversion efficiency of solar cells.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119008775A_ABST
    Figure CN119008775A_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing a solar cell, the solar cell and application thereof, and the method comprises the steps: (1) carrying out the ALD deposition of an aluminum oxide layer on the surface of a silicon wafer, and carrying out the ALD deposition of the aluminum oxide layer through a plurality of reaction cycles, each reaction cycle comprises trimethylaluminum steam pulse, first nitrogen purging, water vapor pulse and second nitrogen purging which are carried out in sequence; the ratio of the trimethylaluminum steam pulse time to the water vapor pulse time is 1: (0.5-1.15); (2) carrying out annealing treatment on the silicon wafer in an oxidizing atmosphere; and (3) forming a silicon nitride layer on the surface, far away from the silicon wafer, of the aluminum oxide layer. According to the method, the content of hydrogen atoms in the aluminum oxide layer is reduced by optimizing the technological conditions of ALD deposition of the aluminum oxide layer, so that the film explosion risk of the aluminum oxide layer is reduced. And meanwhile, oxidation gas is introduced in the annealing process, so that a compact silicon oxide layer can be formed between the silicon wafer and aluminum oxide, and a relatively excellent chemical passivation effect is ensured.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of solar cells, and in particular to a method for preparing a solar cell, a solar cell and applications thereof. Background Art

[0002] Atomic layer deposition (ALD) of aluminum oxide uses the principle of self-limiting surface to control the deposition process at the atomic layer scale by exposing the reaction gas to the substrate surface in turn. Thermal ALD deposited aluminum oxide is obtained by direct reaction at a certain temperature using trimethylaluminum as the aluminum source and water as the oxygen source.

[0003] The advantage of atomic layer deposition (ALD) of aluminum oxide is that it can prepare uniform and dense aluminum oxide on a large area substrate, which has good passivation performance for solar cells. However, in the actual production process, when silicon nitride is deposited on the surface of the aluminum oxide film by PECVD, the high temperature will cause the excess hydrogen atoms in the aluminum oxide to overflow and form hydrogen to break through the silicon nitride film layer, resulting in a film explosion phenomenon, which will damage the integrity of the aluminum oxide and silicon nitride stack, and ultimately lead to a decrease in passivation effect and a decrease in battery efficiency. Summary of the invention

[0004] The present application aims to solve at least one of the technical problems in the related art to a certain extent. To this end, the purpose of the present application is to propose a method for preparing a solar cell, a solar cell and its application. The present application can effectively reduce the content of hydrogen atoms in the aluminum oxide layer by optimizing the process conditions of ALD deposition of the aluminum oxide layer, thereby reducing the possibility of H atoms in the aluminum oxide layer forming hydrogen during subsequent high-temperature treatment, and reducing the risk of film explosion of the aluminum oxide layer. At the same time, the introduction of oxidizing gas during the annealing process can promote the formation of a dense silicon oxide layer between the silicon wafer and the aluminum oxide, passivate the dangling bonds on the surface of the crystalline silicon, and reduce the defect state density at the interface, thereby ensuring a relatively excellent chemical passivation effect.

[0005] In one aspect of the present application, the present application proposes a method for preparing a solar cell. According to an embodiment of the present application, the method includes:

[0006] (1) performing ALD deposition of an aluminum oxide layer on a surface of a silicon wafer, wherein the ALD deposition of the aluminum oxide layer comprises a plurality of reaction cycles, each reaction cycle comprising a trimethylaluminum vapor pulse, a first nitrogen purge, a water vapor pulse, and a second nitrogen purge performed in sequence; the ratio of the trimethylaluminum vapor pulse time to the water vapor pulse time is 1:(0.5-1.15);

[0007] (2) annealing the silicon wafer in an oxidizing atmosphere;

[0008] (3) forming a silicon nitride layer on a surface of the aluminum oxide layer away from the silicon wafer.

[0009] According to the method for preparing solar cells in the embodiment of the present application, by optimizing the process conditions for ALD deposition of the aluminum oxide layer, the content of hydrogen atoms in the aluminum oxide layer can be effectively reduced, thereby reducing the possibility of H atoms in the aluminum oxide layer forming hydrogen during subsequent high-temperature treatment, and reducing the risk of film explosion of the aluminum oxide layer. At the same time, the introduction of oxidizing gas during the annealing process can promote the formation of a dense silicon oxide layer between the silicon wafer and the aluminum oxide, passivate the dangling bonds on the surface of the crystalline silicon, and reduce the density of defect states at the interface, thereby ensuring a relatively excellent chemical passivation effect. In summary, the present application reduces the risk of film explosion of the aluminum oxide layer while ensuring the chemical passivation effect of the battery through annealing with oxidizing gas.

[0010] In addition, the method for preparing a solar cell according to the above embodiment of the present application may also have the following additional technical features:

[0011] In some embodiments of the present application, in step (1), the ratio of the trimethylaluminum vapor pulse time to the water vapor pulse time is 1:(0.7-1.1).

[0012] In some embodiments of the present application, in step (1), in a single reaction cycle, the trimethylaluminum vapor pulse time accounts for 5% to 16% of the total time of the single reaction cycle; the water vapor pulse time accounts for 5% to 16% of the total time of the single reaction cycle; the first nitrogen purge time accounts for 30% to 40% of the total time of the single reaction cycle; the second nitrogen purge time accounts for 35% to 50% of the total time of the single reaction cycle.

[0013] In some embodiments of the present application, in step (1), the temperature for ALD deposition of the aluminum oxide layer is 200° C. to 350° C.; and / or, the ALD deposition of the aluminum oxide layer includes 20 to 80 reaction cycles.

[0014] In some embodiments of the present application, in step (2), the annealing temperature is 400° C. to 500° C., and the annealing time is 5 min to 15 min.

[0015] In some embodiments of the present application, in step (2), the oxidizing atmosphere includes at least one of oxygen and nitrous oxide.

[0016] In some embodiments of the present application, in step (3), the silicon nitride layer is deposited on the surface of the aluminum oxide layer away from the silicon wafer by a PECVD method, and the deposition temperature is 400° C. to 500° C.

[0017] In a second aspect of the present application, the present application provides a solar cell. According to an embodiment of the present application, the solar cell includes:

[0018] Silicon wafer;

[0019] A silicon oxide layer, wherein the silicon oxide layer is disposed on at least a portion of the surface of the silicon wafer;

[0020] an aluminum oxide layer, the aluminum oxide layer being disposed on at least a portion of the surface of the silicon oxide layer away from the silicon wafer, wherein the percentage of hydrogen atoms in the aluminum oxide layer is 2.5 at.% to 3.6 at.%;

[0021] A silicon nitride layer is disposed on at least a portion of the surface of the aluminum oxide layer away from the silicon oxide layer.

[0022] According to the solar cell of the embodiment of the present application, the percentage of hydrogen atoms in the aluminum oxide layer is relatively low, only 2 at.% to 3 at.%, thereby reducing the possibility of H atoms in the aluminum oxide layer forming hydrogen when the silicon nitride layer is subsequently deposited at high temperature on the surface of the aluminum oxide layer, and reducing the risk of film explosion of the aluminum oxide layer. At the same time, a dense silicon oxide layer is arranged between the silicon wafer and the aluminum oxide layer to passivate the dangling bonds on the surface of the crystalline silicon and reduce the density of defect states at the interface, thereby ensuring a relatively excellent chemical passivation effect. Therefore, the present application ensures the chemical passivation effect of the solar cell while reducing the risk of film explosion of the aluminum oxide layer.

[0023] In addition, the solar cell according to the above embodiment of the present application may also have the following additional technical features:

[0024] In some embodiments of the present application, the thickness of the silicon oxide layer is 0.5 nm to 2 nm.

[0025] In some embodiments of the present application, the thickness of the aluminum oxide layer is 3 nm to 10 nm; and / or the thickness of the silicon nitride layer is 30 nm to 120 nm.

[0026] In a third aspect of the present invention, a solar cell module is provided. According to an embodiment of the present invention, the solar cell module has the solar cell of the above embodiment. Thus, the solar cell in the solar cell module has a relatively excellent open circuit voltage (Voc), fill factor (FF) and photoelectric conversion efficiency (PCE).

[0027] Additional aspects and advantages of the present application will be given in part in the description below, and in part will become apparent from the description below, or will be learned through the practice of the present application. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] The above and / or additional aspects and advantages of the present application will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0029] Figure 1A schematic diagram of a process for preparing a solar cell according to an embodiment of the present application;

[0030] Figure 2 Schematic diagram of the structure of a solar cell according to an embodiment of the present application.

[0031] Reference numerals:

[0032] 1-silicon wafer, 2-silicon oxide layer, 3-aluminum oxide layer, 4-silicon nitride layer. DETAILED DESCRIPTION

[0033] Embodiments of the present application are described in detail below, and examples of the embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are intended to be used to explain the present application, and should not be construed as limiting the present application.

[0034] In one aspect of the present application, the present application provides a method for preparing a solar cell. According to an embodiment of the present application, referring to the attached Figure 1 , the method comprises: S100: performing ALD deposition of an aluminum oxide layer on the surface of a silicon wafer, wherein the ALD deposition of the aluminum oxide layer comprises a plurality of reaction cycles, each reaction cycle comprising a trimethylaluminum vapor (TMA) pulse, a first nitrogen purge, a water vapor pulse and a second nitrogen purge in sequence; the ratio of the trimethylaluminum vapor (TMA) pulse time to the water vapor pulse time is 1:(0.5-1.15); S200: annealing the silicon wafer in an oxidizing atmosphere; S300: forming a silicon nitride layer on the surface of the aluminum oxide layer away from the silicon wafer. Thus, the present application can effectively reduce the content of hydrogen atoms in the aluminum oxide layer by optimizing the process conditions of the ALD deposition of the aluminum oxide layer, thereby reducing the possibility of the H atoms in the aluminum oxide layer forming hydrogen during subsequent high-temperature treatment, and reducing the risk of the aluminum oxide layer exploding. At the same time, the introduction of oxidizing gas during the annealing process can promote the formation of a dense silicon oxide layer between the silicon wafer and the aluminum oxide, passivate the dangling bonds on the surface of the crystalline silicon, and reduce the defect state density at the interface, thereby ensuring a relatively excellent chemical passivation effect. In summary, the present application reduces the risk of explosion of the aluminum oxide layer and ensures the chemical passivation effect of the battery through oxidizing gas annealing.

[0035] The following is a detailed description of the principle by which the method for preparing a solar cell proposed by the present invention can achieve the above beneficial effects:

[0036] The present application can effectively reduce the content of H atoms in the aluminum oxide layer (the percentage of hydrogen atoms in the aluminum oxide layer can be reduced to 2.5at.%~3.6at.%) by adjusting the process parameters TMA and water pulse time of the ALD deposition of the aluminum oxide layer, thereby reducing the possibility of H atoms in the aluminum oxide layer forming hydrogen during subsequent high-temperature treatment and reducing the risk of film explosion of the aluminum oxide layer.

[0037] However, the reduction of H atoms in the aluminum oxide layer will reduce the chemical passivation effect of the aluminum oxide layer, resulting in a decrease in the open circuit voltage Voc of the battery. The inventors found that during the annealing process, the introduction of oxidizing gas can effectively promote the formation of a denser silicon oxide layer at the interface between the aluminum oxide layer and the crystalline silicon, passivate the dangling bonds on the surface of the crystalline silicon, and reduce the defect state density at the interface, thereby ensuring the chemical passivation effect of the battery. Therefore, the present application reduces the risk of film explosion of the aluminum oxide layer while ensuring the chemical passivation effect of the battery through annealing with oxidizing gas.

[0038] Specifically, refer to the attached Figure 1 The above method for preparing a solar cell comprises the following steps:

[0039] S100: ALD deposition of aluminum oxide layer on the surface of silicon wafer

[0040] In this step, an aluminum oxide layer is deposited by ALD on the surface of a silicon wafer with an emitter and after texturing. The above-mentioned ALD deposition of aluminum oxide layer includes 20 to 80 reaction cycles, and the thickness of the formed aluminum oxide layer is about 3nm to 10nm. Each reaction cycle includes a trimethylaluminum vapor (TMA) pulse, a first nitrogen purge, a water vapor pulse and a second nitrogen purge in sequence. During the trimethylaluminum vapor (TMA) pulse, trimethylaluminum vapor (TMA) reacts with the OH-group on the surface of the silicon wafer in a half reaction. The purpose of the first nitrogen purge is to remove the remaining gas. During the water vapor pulse, another half reaction is completed. The purpose of the second nitrogen purge is to remove the remaining gas. The specific reaction process is:

[0041] 1)Al(CH3)3+OH-=>O-Al-(CH3)2+CH4;

[0042] 2) Use N2 to purge to remove the remaining Al(CH3)3 gas and CH4 gas;

[0043] 3)O-Al-(CH3)2+H2O=>O-AlOH-(2)+(O)2-Al-CH3+CH4;

[0044] 4) Use N2 to purge to remove the remaining H2O and CH4. Complete a single cycle.

[0045] In an embodiment of the present application, the temperature for ALD deposition of the aluminum oxide layer is 200°C to 350°C, for example, 200°C, 220°C, 240°C, 260°C, 280°C, 300°C, 330°C, 350°C, etc.

[0046] In an embodiment of the present application, the ratio of the trimethylaluminum vapor (TMA) pulse time to the water vapor pulse time is 1:(0.5-1.15), for example, it can be 1:0.5, 1:0.6, 1:0.7, 1:0.8, 1:0.9, 1:1, 1:1.1, 1:1.15, etc. By limiting the ratio of the trimethylaluminum vapor (TMA) pulse time to the water vapor pulse time within the above range, the content of hydrogen atoms in the aluminum oxide layer can be effectively reduced (the percentage of hydrogen atoms in the aluminum oxide layer can be reduced to 2.5 at.%-3.6 at.%), thereby reducing the possibility of H atoms in the aluminum oxide layer forming hydrogen during subsequent high-temperature treatment, and reducing the risk of film explosion of the aluminum oxide layer. The inventors have discovered that if the proportion of the water vapor pulse time is too large, the percentage of hydrogen atoms in the deposited aluminum oxide layer will be too high, which will cause the high temperature to cause excess hydrogen atoms in the aluminum oxide to overflow and form hydrogen to break through the silicon nitride film layer, resulting in a film explosion phenomenon when silicon nitride is deposited on the surface of the aluminum oxide film layer by the PECVD method in the subsequent step; if the proportion of the water vapor pulse time is too small, the quality of the deposited aluminum oxide layer will be poor, thereby affecting the passivation effect of the aluminum oxide layer.

[0047] As some preferred embodiments, the ratio of the trimethylaluminum vapor (TMA) pulse time to the water vapor pulse time is 1:(0.7-1.1), which can further effectively reduce the content of hydrogen atoms in the aluminum oxide layer, thereby further reducing the possibility of H atoms in the aluminum oxide layer forming hydrogen during subsequent high-temperature treatment, and further reducing the risk of film explosion of the aluminum oxide layer.

[0048] In the embodiments of the present application, the pulse flow rates of TMA and water do not need to be limited, and the pulse flow rates of TMA and water are assumed to be unchanged.

[0049] According to some specific embodiments of the present application, in a single reaction cycle, the trimethylaluminum vapor (TMA) pulse time accounts for 5% to 16% of the total time of a single reaction cycle (as an example, it can be 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, etc.); the water vapor pulse time accounts for 5% to 16% of the total time of a single reaction cycle (as an example, it can be 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, etc.). 14%, 15%, etc.); the first nitrogen purge time accounts for 30% to 40% of the total time of a single reaction cycle (as an example, it can be 30%, 31%, 32%, 33%, 34%, 35%, 36%, 37%, 38%, 39%, 40%, etc.); the second nitrogen purge time accounts for 35% to 50% of the total time of a single reaction cycle (as an example, it can be 35%, 36%, 38%, 39%, 40%, 42%, 44%, 46%, 48%, 50%, etc.). Therefore, by limiting the time proportion of each process, the content of hydrogen atoms in the aluminum oxide layer can be further effectively reduced, thereby further reducing the possibility of H atoms in the aluminum oxide layer forming hydrogen during subsequent high-temperature treatment, and further reducing the risk of explosion of the aluminum oxide layer.

[0050] S200: Annealing of silicon wafers in an oxidizing atmosphere

[0051] In this step, the silicon wafer is annealed in an oxidizing atmosphere. The inventors found that the reduction of H atoms in the aluminum oxide layer formed in step S100 will reduce the chemical passivation effect of the aluminum oxide layer, resulting in a decrease in the open circuit voltage Voc of the battery. In view of this, the present application introduces an oxidizing gas during the annealing process, which can effectively promote the formation of a denser silicon oxide layer at the interface between the aluminum oxide layer and the crystalline silicon, passivate the dangling bonds on the surface of the crystalline silicon, and reduce the defect state density at the interface, thereby ensuring the chemical passivation effect of the battery.

[0052] According to some further specific embodiments of the present application, the annealing temperature is 400°C to 500°C (as an example, it can be 400°C, 410°C, 420°C, 430°C, 440°C, 450°C, 460°C, 470°C, 480°C, 490°C, 500°C, etc.), and the annealing time is 5min to 15min (as an example, it can be 5min, 6min, 7min, 8min, 9min, 10min, 11min, 12min, 13min, 14min, 15min, etc.). By limiting the annealing temperature and annealing time within the above range, it can further effectively promote the formation of a denser silicon oxide layer at the interface between the aluminum oxide layer and the crystalline silicon, passivate the dangling bonds on the surface of the crystalline silicon, and reduce the defect state density at the interface, thereby further ensuring the chemical passivation effect of the battery.

[0053] In the embodiments of the present application, the specific type of the above-mentioned oxidizing atmosphere is not particularly limited, and those skilled in the art can select it according to actual needs. As some preferred schemes, the above-mentioned oxidizing atmosphere includes at least one of oxygen and nitrous oxide, for example, a mixed gas of nitrogen and oxygen with different flow ratios or a mixed gas of nitrogen and nitrous oxide with different flow ratios can be used.

[0054] S300: forming a silicon nitride layer on the surface of the aluminum oxide layer away from the silicon wafer

[0055] In the embodiment of the present application, the silicon nitride layer can be deposited on the surface of the aluminum oxide layer away from the silicon wafer by using the PECVD method. Since the process conditions of the aluminum oxide layer deposited by ALD are optimized in step S100, the content of hydrogen atoms in the aluminum oxide layer is effectively reduced. Therefore, when the silicon nitride is deposited on the surface of the aluminum oxide film layer by using the PECVD method in step S300, the high temperature will not cause the excess hydrogen atoms in the aluminum oxide to overflow to form hydrogen gas to break through the silicon nitride film layer and produce a film explosion phenomenon, thereby avoiding the integrity of the aluminum oxide and silicon nitride stack from being damaged.

[0056] According to some other specific embodiments of the present application, the temperature for depositing the silicon nitride layer on the surface of the aluminum oxide layer by PECVD is 400°C to 500°C, and as an example, it can be 400°C, 410°C, 420°C, 430°C, 440°C, 450°C, 460°C, 470°C, 480°C, 490°C, 500°C, etc.

[0057] In the second aspect of the present application, the present application provides a solar cell. According to an embodiment of the present application, the solar cell is prepared by the method of the above embodiment. Specifically, referring to the attached Figure 2 The solar cell includes: a silicon wafer 1; a silicon oxide layer 2, wherein the silicon oxide layer 2 is arranged on at least a portion of the surface of the silicon wafer 1; an aluminum oxide layer 3, wherein the aluminum oxide layer 3 is arranged on at least a portion of the surface of the silicon oxide layer 2 away from the silicon wafer 1, and the hydrogen atom content percentage in the aluminum oxide layer 3 is 2at.% to 3at.%; and a silicon nitride layer 4, wherein the silicon nitride layer 4 is arranged on at least a portion of the surface of the aluminum oxide layer 3 away from the silicon oxide layer 2.

[0058] According to the solar cell of the embodiment of the present application, the percentage of hydrogen atoms in the aluminum oxide layer is relatively low, only 2.5 at.% to 3.6 at.%, thereby reducing the possibility of H atoms in the aluminum oxide layer forming hydrogen when the silicon nitride layer is subsequently deposited at high temperature on the surface of the aluminum oxide layer, and reducing the risk of film explosion of the aluminum oxide layer. At the same time, a dense silicon oxide layer is arranged between the silicon wafer and the aluminum oxide layer to passivate the dangling bonds on the surface of the crystalline silicon and reduce the density of defect states at the interface, thereby ensuring a relatively excellent chemical passivation effect. Therefore, the present application ensures the chemical passivation effect of the solar cell while reducing the risk of film explosion of the aluminum oxide layer.

[0059] According to some specific embodiments of the present application, the thickness of the above-mentioned silicon oxide layer is 0.5nm~2nm, and as an example it can be 0.5nm, 0.6nm, 0.8nm, 1nm, 1.2nm, 1.4nm, 1.6nm, 1.8nm, 2nm, etc., thereby further ensuring the passivation of the dangling bonds on the surface of the silicon wafer, reducing the defect state density at the interface, thereby ensuring a relatively excellent chemical passivation effect.

[0060] According to some further specific embodiments of the present application, the thickness of the aluminum oxide layer is 3 nm to 10 nm, and as an example, it can be 3 nm, 4 nm, 5 nm, 6 nm, 7 nm, 8 nm, 9 nm, 10 nm, etc. And / or, the thickness of the silicon nitride layer is 30 nm to 120 nm, and as an example, it can be 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm, 100 nm, 110 nm, 120 nm, etc.

[0061] In a third aspect of the present invention, a solar cell module is provided. According to an embodiment of the present invention, the solar cell module has the solar cell of the above embodiment. Thus, the solar cell in the solar cell module has a relatively excellent open circuit voltage (Voc), fill factor (FF) and photoelectric conversion efficiency (PCE).

[0062] A battery module is a finished module with power generation output function produced by connecting multiple of the above-mentioned solar cells in series and / or in parallel, and undergoing processes such as lamination and packaging. Specifically, the battery module includes photovoltaic glass, packaging film, battery cells, packaging film, backplane, etc.

[0063] The embodiments of the present application are described in detail below. It should be noted that the embodiments described below are exemplary and are only used to explain the present application, and cannot be construed as limiting the present application. Wherein, the concentrated sulfuric acid used below is a concentrated sulfuric acid chemical with a mass fraction of 98%. In addition, if not explicitly stated, all reagents used in the following embodiments are commercially available, or can be synthesized according to this article or known methods, and the reaction conditions not listed are also easily available to those skilled in the art.

[0064] Example 1

[0065] This embodiment provides a method for preparing a solar cell, comprising:

[0066] 1) An n-type silicon wafer with a thickness of 150 μm and a resistivity of 2 Ω is selected as the substrate and polished to remove mechanical damage and dirt on the surface.

[0067] 2) P-poly-Si, n-poly-Si and isolation regions are formed on the back of the battery in sequence by laser melting, wet etching, LPCVD and PE-poly. There is a tunneling oxide layer between p-poly-Si and n-poly-Si and the n-type substrate silicon. A pyramid-shaped velvet structure is formed on the front of the battery by velveting.

[0068] 3) The cleaned silicon wafer is placed in an atomic layer aluminum oxide deposition chamber to deposit an aluminum oxide layer at a deposition temperature of 290°C. The pulse time of TMA is 7 seconds, the first nitrogen purge time is 15 seconds, the pulse time of water is 5 seconds, and the second nitrogen purge time is 20 seconds. The thickness of the formed aluminum oxide layer is about 6 nm.

[0069] 4) The silicon wafer with aluminum oxide deposited is placed in a PECVD tube, and the temperature is raised to 450°C for annealing. During the annealing process, a mixed gas of nitrogen and nitrous oxide with a flow ratio of 4:1 is introduced, and the temperature is kept constant for 10 minutes, so that a silicon oxide layer with a thickness of about 1 nm is formed at the interface between the silicon wafer and the aluminum oxide layer. Then, a silicon nitride film with a thickness of about 1 nm is plated.

[0070] Example 2

[0071] The preparation method of Example 2 is basically the same as that of Example 1, except that:

[0072] 3) The pulse time of TMA was 7 s, the time of the first nitrogen purge was 15 s, the pulse time of water was 4 s, and the time of the second nitrogen purge was 20 s.

[0073] Example 3

[0074] The preparation method of Example 3 is basically the same as that of Example 1, except that:

[0075] 3) The pulse time of TMA was 7 s, the time of the first nitrogen purge was 15 s, the pulse time of water was 6 s, and the time of the second nitrogen purge was 20 s.

[0076] Example 4

[0077] The preparation method of Example 4 is basically the same as that of Example 1, except that:

[0078] 3) The pulse time of TMA was 7 s, the time of the first nitrogen purge was 15 s, the pulse time of water was 7 s, and the time of the second nitrogen purge was 20 s.

[0079] Example 5

[0080] The preparation method of Example 5 is basically the same as that of Example 1, except that:

[0081] 3) The pulse time of TMA was 7 s, the time of the first nitrogen purge was 15 s, the pulse time of water was 8 s, and the time of the second nitrogen purge was 20 s.

[0082] Example 6

[0083] The preparation method of Example 6 is basically the same as that of Example 1, except that:

[0084] 4) The temperature was raised to 400° C. for annealing. During the annealing process, a mixed gas of nitrogen and nitrous oxide with a flow ratio of 4:1 was introduced and the temperature was kept constant for 15 minutes to form a silicon oxide layer with a thickness of about 1 nm at the interface between the silicon wafer and the aluminum oxide layer.

[0085] Example 7

[0086] The preparation method of Example 7 is basically the same as that of Example 1, except that:

[0087] 4) The temperature was raised to 500° C. for annealing. During the annealing process, a mixed gas of nitrogen and nitrous oxide with a flow ratio of 4:1 was introduced and the temperature was kept constant for 5 minutes to form a silicon oxide layer with a thickness of about 1 nm at the interface between the silicon wafer and the aluminum oxide layer.

[0088] Example 8

[0089] The preparation method of Example 8 is basically the same as that of Example 1, except that:

[0090] 4) During the annealing process, a mixed gas of nitrogen and oxygen with a flow ratio of 4:1 was introduced.

[0091] Comparative Example 1

[0092] The preparation method of Comparative Example 1 is basically the same as that of Example 1, except that:

[0093] 3) The pulse time of TMA was 7 s, the time of the first nitrogen purge was 15 s, the pulse time of water was 9 s, and the time of the second nitrogen purge was 20 s.

[0094] Comparative Example 2

[0095] The preparation method of Comparative Example 2 is basically the same as that of Example 1, except that:

[0096] 3) The pulse time of TMA was 7 s, the time of the first nitrogen purge was 15 s, the pulse time of water was 3 s, and the time of the second nitrogen purge was 20 s.

[0097] Comparative Example 3

[0098] The preparation method of Comparative Example 3 is basically the same as that of Example 1, except that:

[0099] 4) No oxidizing gas is introduced during the annealing process.

[0100] The percentage of hydrogen atom content in the aluminum oxide layers deposited in Examples 1 to 8 and Comparative Examples 1 to 3 was tested, and the film explosion of the aluminum oxide layers deposited in Examples 1 to 8 and Comparative Examples 1 to 3 was observed. The short-circuit current (Isc), open-circuit voltage (Voc), fill factor (FF) and photoelectric conversion efficiency (Eta) of the solar cells deposited in Examples 1 to 8 and Comparative Examples 1 to 3 were tested, and the results are shown in Table 1.

[0101] Table 1

[0102]

[0103] As can be seen from Table 1, the percentage of hydrogen atoms in the aluminum oxide layer of Comparative Example 1 is high and the film explosion phenomenon occurs, while the percentage of hydrogen atoms in the aluminum oxide layers of Examples 1 to 8 are all low and the film explosion phenomenon does not occur; it can be seen that if the proportion of the water vapor pulse time is too large, the percentage of hydrogen atoms in the deposited aluminum oxide layer will be too high, resulting in the film explosion phenomenon. In addition, compared with Comparative Example 1, the open circuit voltage (Voc) and Eta of Examples 1 to 8 are improved.

[0104] It can be seen from Table 1 that compared with Comparative Example 2, the open circuit voltage (Voc) and Eta of Examples 1 to 8 are significantly improved. It can be seen that if the proportion of the water vapor pulse time is too small, the quality of the deposited aluminum oxide layer will be poor, thereby affecting the passivation effect of the aluminum oxide layer.

[0105] It can be seen from Table 1 that, compared with Comparative Example 3, the open circuit voltage (Voc) and Eta of Examples 1 to 8 are significantly improved. It can be seen that if the oxidizing gas is not introduced during the annealing process, the chemical passivation effect of the aluminum oxide layer will be reduced.

[0106] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present application. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.

[0107] Although the embodiments of the present application have been shown and described above, it can be understood that the above embodiments are exemplary and cannot be understood as limitations on the present application. Ordinary technicians in this field can change, modify, replace and modify the above embodiments within the scope of the present application.

Claims

1. A method for preparing a solar cell, characterized in that: include: (1) performing ALD deposition of an aluminum oxide layer on a surface of a silicon wafer, wherein the ALD deposition of the aluminum oxide layer comprises a plurality of reaction cycles, each reaction cycle comprising a trimethylaluminum vapor pulse, a first nitrogen purge, a water vapor pulse, and a second nitrogen purge performed in sequence; the ratio of the trimethylaluminum vapor pulse time to the water vapor pulse time is 1:(0.5-1.15); (2) annealing the silicon wafer in an oxidizing atmosphere; (3) forming a silicon nitride layer on a surface of the aluminum oxide layer away from the silicon wafer.

2. The method according to claim 1, characterized in that In step (1), the ratio of the trimethylaluminum vapor pulse time to the water vapor pulse time is 1:(0.7-1.1).

3. The method according to claim 1, characterized in that In step (1), in a single reaction cycle, the trimethylaluminum vapor pulse time accounts for 5% to 16% of the total time of the single reaction cycle; the water vapor pulse time accounts for 5% to 16% of the total time of the single reaction cycle; the first nitrogen purge time accounts for 30% to 40% of the total time of the single reaction cycle; and the second nitrogen purge time accounts for 35% to 50% of the total time of the single reaction cycle.

4. The method according to claim 1, characterized in that: In step (1), the temperature for ALD deposition of the aluminum oxide layer is 200° C. to 350° C.; And / or, the ALD deposition of the aluminum oxide layer includes 20 to 80 reaction cycles.

5. The method according to any one of claims 1 to 4, characterized in that: In step (2), the annealing temperature is 400° C. to 500° C., and the annealing time is 5 min to 15 min.

6. The method according to any one of claims 1 to 4, characterized in that: In step (2), the oxidizing atmosphere includes at least one of oxygen and nitrous oxide.

7. The method according to any one of claims 1 to 4, characterized in that: In step (3), the silicon nitride layer is deposited on the surface of the aluminum oxide layer away from the silicon wafer by using a PECVD method, and the deposition temperature is 400° C. to 500° C.

8. A solar cell, characterized in that: include: Silicon wafer; A silicon oxide layer, wherein the silicon oxide layer is disposed on at least a portion of the surface of the silicon wafer; an aluminum oxide layer, the aluminum oxide layer being disposed on at least a portion of the surface of the silicon oxide layer away from the silicon wafer, wherein the percentage of hydrogen atoms in the aluminum oxide layer is 2.5 at.% to 3.6 at.%; A silicon nitride layer is disposed on at least a portion of the surface of the aluminum oxide layer away from the silicon oxide layer.

9. The solar cell according to claim 8, characterized in that The thickness of the silicon oxide layer is 0.5 nm to 2 nm.

10. The solar cell according to claim 8, characterized in that The thickness of the aluminum oxide layer is 3nm to 10nm; And / or, the thickness of the silicon nitride layer is 30 nm to 120 nm.

11. A solar cell module, characterized in that: A solar cell manufactured by the method according to any one of claims 1 to 7 or a solar cell according to any one of claims 8 to 10.

Citation Information

Patent Citations

  • Cell piece passivation layer intermediate, and solar cell piece and preparation method thereof

    CN109728104A

  • Solar cell with composite dielectric passivation layer structure and preparation process thereof

    CN110459615A

  • Low-pressure annealing method for crystalline silicon solar cell

    CN112670374A

  • Method and device for preparing aluminum oxide passivation film by using ALD (atomic layer deposition) method

    CN117568780A

Cited By

  • Solar cell and preparation method thereof

    CN120152431A

  • Solar cell composite passivation layer and preparation method thereof, and solar cell

    CN120500161A

  • Solar cell passivation layer preparation process, passivation layer structure and solar cell

    CN120512942A

  • Solar cell front film layer with anti-UV attenuation effect and preparation method thereof

    CN120614909A

  • Anti-attenuation film layer of battery and preparation method of anti-attenuation film layer