Sodium ferric phosphate positive electrode material and preparation method thereof, positive electrode and battery

By using core-shell structure and liquid-phase preparation technology in sodium ferric phosphate positive electrode material, a nano-scale small particle structure is formed, which solves the purity and morphology of the existing materials, and significantly improves the capacity and rate performance.

CN119008875APending Publication Date: 2024-11-22SHENZHEN FOUND HOPE NEW ENERGY TECHNOLOGY CO LTD
View PDF 0 Cites 4 Cited by

Patent Information

Application Number
CN202410786810.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-18
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing sodium ferric phosphate materials have low phase purity and blocky morphology, which leads to difficulty in conducting electrons and affects the capacity and rate performance of the material.

Method used

The sodium iron phosphate positive electrode material adopts core-shell structure, with a particle size of 50-1000nm, including a carbon cladding layer, is prepared by liquid phase method of water-soluble raw materials and organic carbon sources, and uses organic solvents to promote grain formation and limit grain growth. , forming a nanoscale small particle structure.

Benefits of technology

It improves the material's phase purity and electron conduction ability, and significantly improves capacity performance and rate performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119008875A_ABST
    Figure CN119008875A_ABST
Patent Text Reader

Abstract

In order to solve the problem of difficult electron conduction caused by low phase purity and blocky morphology of sodium ferric pyrophosphate prepared by the existing preparation method, the invention provides a sodium ferric phosphate positive electrode material and a preparation method thereof, a positive electrode and a battery, the sodium ferric phosphate positive electrode material is of a core-shell structure, the particle size of the core-shell structure is 50-1000nm, and the particle size of the core-shell structure is 10-20nm. The core-shell mechanism comprises a core body and a carbon coating layer, the core body comprises ferric sodium phosphate pyrophosphate, and the thickness of the carbon coating layer is 3-10 nm.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of sodium iron phosphate positive electrode materials, and specifically relates to a sodium iron phosphate positive electrode material and a preparation method thereof, a positive electrode, and a battery. Background Art

[0002] Sodium-ion batteries have a similar working principle to lithium-ion batteries, and sodium resources are abundant and the mining cost is low. Under the same conditions, the manufacturing cost of sodium-ion battery electrode materials is much lower, and it is expected to be widely used in the field of energy storage. Sodium-ion positive electrode materials include transition metal oxides, Prussian blue and its analogs, and polyanion materials. Different materials have obvious differences in capacity, rate and structural stability. Current research shows that transition metal oxides are often accompanied by multiple phase changes in the process of redox and deintercalation of sodium ions, which leads to structural collapse and affects the cyclic stability of the material. The crystal structure of Prussian blue and its analogs contains a large amount of crystalline water, which is easy to decompose and produce gas at high potential, causing the battery to swell and fail. Compared with the first two types of materials, polyanion sodium-ion battery positive electrode materials are undoubtedly the best choice for sodium-ion battery positive electrodes with their stable framework structure and excellent electrochemical properties.

[0003] At present, the polyanion sodium ion battery positive electrode materials that are studied more include metal-based phosphates of non-V systems. However, the sodium iron pyrophosphate material prepared by the prior art often has a low capacity (90-100mAh / g), which is far from the theoretical capacity of 129mAhg of the sodium iron pyrophosphate material. This is mainly because it is difficult to mix the materials evenly by the traditional solid phase mixing method, and whether the raw materials are uniform directly affects the phase purity of the finished material, which leads to the low phase purity of the finished material obtained after sintering, and then leads to low capacity. If the liquid phase method and the traditional alkali solution co-precipitation method are used, although the elements can be mixed evenly, thereby improving the phase purity and capacity of the sodium iron pyrophosphate, the conventional liquid phase method usually causes the material morphology to present a compact micron block after drying, making ion conduction and electron conduction difficult, and ultimately causing a great decrease in the material rate performance. Summary of the invention

[0004] In view of the problem that sodium iron pyrophosphate prepared by the existing preparation method has low phase purity and blocky morphology, which makes electron conduction difficult, the present invention provides a sodium iron phosphate positive electrode material and a preparation method thereof, a positive electrode, and a battery.

[0005] The technical solution adopted by the present invention to solve the above technical problems is as follows:

[0006] On the one hand, the present invention provides a sodium iron phosphate positive electrode material, which has a core-shell structure, the particle size of the core-shell structure is 50-1000nm, the core-shell structure includes a core body and a carbon coating layer, the core body includes sodium iron pyrophosphate, and the thickness of the carbon coating layer is 3-10nm.

[0007] In the present invention, the core-shell structure particle size is 50-1000nm, which is conducive to the high-speed conduction of ions and electrons, and has better capacity performance and rate performance. The carbon coating layer can be used as a conductive layer to improve the conductivity of the surface of the sodium iron phosphate positive electrode material.

[0008] Optionally, the core body further includes a conductive agent, which is doped into the sodium iron pyrophosphate, and the conductive agent includes one or more of graphene oxide, carbon nanotubes, and carbon black.

[0009] On the other hand, the present invention provides a method for preparing the sodium iron phosphate positive electrode material as described in any one of the above, comprising the following steps:

[0010] Obtaining a water-soluble organic carbon source and a water-soluble raw material containing a Na source, an Fe source, and a P source;

[0011] dissolving the organic carbon source and the water-soluble raw material in water to obtain a mixed solution;

[0012] Adding an organic solvent to the mixed solution in a stirring state until no more crystals are precipitated in the mixed solution;

[0013] drying the mixed solution containing the crystal grains to obtain a precursor powder;

[0014] The precursor powder is calcined to obtain a sodium iron phosphate positive electrode material.

[0015] Optionally, the mass ratio of the mixed solution to the organic solvent is (1:1)-(10:1).

[0016] Optionally, the organic solvent includes one or more of N-methylpyrrolidone, dimethylformamide, methanol, ethanol, ethylene glycol, propanol, isopropanol, propylene glycol, n-butanol, acetonitrile, and acetone.

[0017] Optionally, the organic carbon source includes one or more of glucose, sucrose, polyvinyl pyrrolidone, cellulose, starch, polyethylene glycol, polystyrene, polyvinyl alcohol, polyethylene, polypropylene, citric acid, and stearic acid;

[0018] The water-soluble raw materials include at least two of ferric nitrate, ferric sulfate, ferric acetate, ferric chloride, ferric citrate, ferric tartrate, ferric tribromide, sodium dihydrogen phosphate, disodium hydrogen phosphate, sodium phosphate, sodium pyrophosphate, phosphoric acid, sodium hexametaphosphate, sodium carbonate, sodium acetate, sodium sulfide, sodium chloride, and sodium sulfate.

[0019] Optionally, the mass of the organic carbon source is 2%-20% of the mass of the water-soluble raw material; the mass ratio of the sum of the mass of the organic carbon source and the water-soluble raw material to the mass of the water is (1:1)-(10:1).

[0020] Optionally, the drying method is drying or spray drying, and the drying is stirring drying at 78-82° C.;

[0021] The calcination conditions are: in a protective atmosphere, heating to 450°C-600°C at a heating rate of 5-10°C / min, and calcining for 5-30 hours.

[0022] On the other hand, the present invention provides a positive electrode, comprising the sodium iron phosphate positive electrode material as described in any one of the above, or comprising the sodium iron phosphate positive electrode material prepared by the preparation method of the sodium iron phosphate positive electrode material as described in any one of the above.

[0023] In another aspect, the present invention provides a battery comprising the positive electrode as described above.

[0024] In the present invention, water-soluble raw materials, water-soluble organic carbon sources and liquid phase methods are used to make the elements in the precursor powder before calcination evenly distributed, which is conducive to improving the purity of the physical phase. At the same time, organic solvents are used as grain generation promoters, and the growth of grains is limited by the principle of competitive crystallization, so that the sodium iron phosphate positive electrode material after calcination presents a morphology composed of nano-sized particles, which is conducive to the high-speed conduction of ions and electrons, and has better capacity performance and rate performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is a SEM image of a sodium iron phosphate positive electrode material provided in Example 1 of the present invention at 1 μm. DETAILED DESCRIPTION

[0026] In order to make the technical problems, technical solutions and beneficial effects solved by the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0027] An embodiment of the present invention provides a sodium iron phosphate positive electrode material, which has a core-shell structure, a particle size of the core-shell structure is 50-1000nm, the core-shell structure includes a core body and a carbon coating layer, the core body includes sodium iron pyrophosphate, and the thickness of the carbon coating layer is 3-10nm.

[0028] In the present invention, the core-shell structure particle size is 50-1000nm, which is conducive to the high-speed conduction of ions and electrons, and has better capacity performance and rate performance. The carbon coating layer can be used as a conductive layer to improve the conductivity of the surface of the sodium iron phosphate positive electrode material.

[0029] In a preferred embodiment, the particle size of the core-shell structure is 50-600 nm.

[0030] In some embodiments, the core further comprises a conductive agent, the conductive agent is doped in the sodium iron pyrophosphate, and the conductive agent comprises one or more of graphene oxide, carbon nanotubes, and carbon black. On the other hand, an embodiment of the present invention provides a method for preparing a sodium iron phosphate positive electrode material as described above, comprising the following steps:

[0031] Obtaining a water-soluble organic carbon source and a water-soluble raw material containing a Na source, an Fe source, and a P source;

[0032] The organic carbon source and the water-soluble raw material are dissolved in water to obtain a mixed solution; specifically, the dissolution temperature is 25°C-100°C.

[0033] An organic solvent is added to the mixed solution in a stirring state until no more crystals are precipitated in the mixed solution; specifically, stirring is performed for 1-5 hours after the crystals are precipitated.

[0034] drying the mixed solution containing the crystal grains to obtain a precursor powder;

[0035] The precursor powder is calcined to obtain a sodium iron phosphate positive electrode material.

[0036] In the present invention, water-soluble raw materials, water-soluble organic carbon sources and liquid phase methods are used to make the elements in the precursor powder before calcination evenly distributed, which is conducive to improving the purity of the physical phase. At the same time, organic solvents are used as grain generation promoters, and the growth of grains is limited by the principle of competitive crystallization, so that the sodium iron phosphate positive electrode material after calcination presents a morphology composed of nano-sized particles, which is conducive to the high-speed conduction of ions and electrons, and has better capacity performance and rate performance.

[0037] In some embodiments, a conductive agent is added to the mixed solvent before adding the organic solvent.

[0038] In a specific embodiment, the amount of the conductive agent added is 0.2%-2.5% of the mass of the water-soluble raw material.

[0039] In a specific embodiment, the molar ratio of Na:Fe:P in the water-soluble raw material is (3.8-4.2):(2.8-3.2):4.

[0040] In some embodiments, the mass ratio of the mixed solution to the organic solvent is (1:1)-(10:1).

[0041] In a preferred embodiment, the mass ratio of the organic solvent to the mixed solution is 1:3.

[0042] In a preferred embodiment, the organic solvent is added by slow dripping, specifically, dripping can be performed by a Rongguo peristaltic pump.

[0043] In some embodiments, the organic solvent includes one or more of N-methylpyrrolidone (NMP), dimethylformamide (DME), methanol, ethanol, ethylene glycol, propanol, isopropanol, propylene glycol, n-butanol, acetonitrile, and acetone.

[0044] In a preferred embodiment, the organic solvent is ethanol.

[0045] In some embodiments, the organic carbon source includes one or more of glucose, sucrose, polyvinyl pyrrolidone (PVP), cellulose, starch, polyethylene glycol (PEG), polystyrene (PS), polyvinyl alcohol (PVA), polyethylene (PE), polypropylene (PP), citric acid, and stearic acid;

[0046] The water-soluble raw materials include at least two of ferric nitrate, ferric sulfate, ferric acetate, ferric chloride, ferric citrate, ferric tartrate, ferric tribromide, sodium dihydrogen phosphate, disodium hydrogen phosphate, sodium phosphate, sodium pyrophosphate, phosphoric acid, sodium hexametaphosphate, sodium carbonate, sodium acetate, sodium sulfide, sodium chloride, and sodium sulfate.

[0047] In a preferred embodiment, the organic carbon source is glucose, the water-soluble raw materials are ferric nitrate and sodium dihydrogen phosphate, and the molar ratio of Na:Fe:P is 4:2.912:4.

[0048] In some embodiments, the mass of the organic carbon source is 2%-20% of the mass of the water-soluble raw material; the mass ratio of the sum of the mass of the organic carbon source and the water-soluble raw material to the mass of the water is (1:1)-(20:1).

[0049] In a preferred embodiment, the mass of the organic carbon source is 5%-15% of the mass of the water-soluble raw material; the mass ratio of the sum of the mass of the organic carbon source and the water-soluble raw material to the mass of the water is (1:1)-(10:1).

[0050] In some embodiments, the drying method is drying or spray drying, and the drying is stirring drying at 78-82°C;

[0051] The calcination conditions are: in a protective atmosphere, heating to 450°C-600°C at a heating rate of 5-10°C / min, and calcining for 5-30 hours. Specifically, the protective atmosphere is nitrogen or argon.

[0052] On the other hand, the present invention provides a positive electrode, comprising the sodium iron phosphate positive electrode material as described in any one of the above, or comprising the sodium iron phosphate positive electrode material prepared by the preparation method of the sodium iron phosphate positive electrode material as described in any one of the above.

[0053] On the other hand, an embodiment of the present invention provides a battery, comprising the positive electrode as described above.

[0054] The present invention is further described below by way of examples.

[0055] Example 1

[0056] This embodiment is used to illustrate the sodium iron phosphate positive electrode material and battery disclosed in the present invention, and includes the following operating steps:

[0057] (1) Preparation of mixed solution: iron nitrate and sodium dihydrogen phosphate were selected as raw materials, and the specific amount was 2 mol sodium dihydrogen phosphate dihydrate (NaH 2 PO 4 ·2H 2 O), 1.456 mol iron nitrate nonahydrate (Fe(NO 3 ) 3 9H 2 O), and glucose was selected as the organic carbon source in an amount of 0.5 mol. The above raw materials were added to 200 g of water, heated to 80° C., and stirred for more than 10 minutes until the solution was clear and mixed evenly.

[0058] (2) Select ethanol as the organic solvent, and slowly add 500 mL of ethanol into the mixed solution through a peristaltic pump. After all the ethanol is added, continue stirring for 30 minutes.

[0059] (3) The suspension solution obtained in step (2) was stirred and dried in an oven at 80° C. to obtain a precursor powder.

[0060] (4) placing the precursor powder in step (3) in a tube furnace, heating the temperature to 500° C. at a heating rate of 10° C. / min, and keeping the temperature for 10 h, finally obtaining sodium iron phosphate positive electrode material powder. Figure 1This is the SEM image of the target product synthesized in this example. It can be seen from the figure that the target product is composed of small particles of 20-50nm.

[0061] (5) Assembling a battery: Using the sodium iron pyrophosphate powder prepared above as the positive electrode active material, the mixture is mixed in a ratio of positive electrode active material: conductive agent: binder = 90:5:5, and is prepared into an electrode by coating-rolling and the like; subsequently, the electrode is used as the positive electrode, metallic sodium is used as the negative electrode, and glass fiber is used as the separator to assemble into a half-cell.

[0062] Example 2

[0063] This example is used to illustrate the sodium iron phosphate positive electrode material and battery disclosed in the present invention, and includes most of the operating steps in Example 1, except that: in step (1), ferrous sulfate nonahydrate (Fe 2 (SO 4 ) 3 9H 2 O), phosphoric acid (H 3 PO 4 ) and sodium dihydrogen phosphate dihydrate are used as raw materials, the specific dosage is 1.1 mol sodium dihydrogen phosphate dihydrate, 0.9 mol phosphoric acid, 1.5 mol ferric sulfate nonahydrate, and sucrose is selected as the organic carbon source, the dosage is 0.5 mol.

[0064] In step (2), dimethylformamide (DMF) is selected as the organic solvent.

[0065] The calcination temperature in step (4) is 550°C.

[0066] Example 3

[0067] This example is used to illustrate the sodium iron phosphate positive electrode material and battery disclosed in the present invention, and includes most of the operating steps in Example 1, except that: in step (1), ferric acetate and sodium dihydrogen phosphate dihydrate are selected as raw materials, and the specific amounts are 2 mol sodium dihydrogen phosphate dihydrate and 1.52 mol ferric acetate. At the same time, polyvinyl pyrrolidone is selected as an organic carbon source, and the amount is 0.5 mol.

[0068] In step (4), the temperature is kept at 500° C. for 15 h.

[0069] Example 4

[0070] This example is used to illustrate the sodium iron phosphate positive electrode material and battery disclosed in the present invention, and includes most of the operating steps in Example 1, except that: in step (1), ferric nitrate nonahydrate and sodium pyrophosphate are selected as raw materials, and the specific amounts used are 0.5 mol sodium pyrophosphate, 1 mol phosphoric acid, and 1.456 mol ferric nitrate nonahydrate.

[0071] Example 5

[0072] This example is used to illustrate the sodium iron phosphate positive electrode material and battery disclosed in the present invention, and includes most of the operating steps in Example 1, except that the mass ratio of the mixed solution to ethanol is 1:1, and the amount of ethanol added is 1500 mL.

[0073] Example 6

[0074] This example is used to illustrate the sodium iron phosphate positive electrode material and battery disclosed in the present invention, and includes most of the operating steps in Example 1, except that the mass ratio of the mixed solution to ethanol is 10:1, and the amount of ethanol added is 150 mL.

[0075] Example 7

[0076] This example is used to illustrate the sodium iron phosphate positive electrode material and battery disclosed in the present invention, and includes most of the operating steps in Example 1, except that the mass ratio of the mixed solution to ethanol is 15:1, and the amount of ethanol added is 100 mL.

[0077] Example 8

[0078] This example is used to illustrate the sodium iron phosphate positive electrode material and battery disclosed in the present invention, and includes most of the operating steps in Example 1, except that 10 g of carbon nanotubes are added to the mixed solution before step (2).

[0079] Example 9

[0080] This example is used to illustrate the sodium iron phosphate positive electrode material and battery disclosed in the present invention, and includes most of the operating steps in Example 1, except that the mass of the organic carbon source is 2% of the mass of the water-soluble raw material, and the amount of the organic carbon source is 0.1 mol.

[0081] Example 10

[0082] This example is used to illustrate the sodium iron phosphate positive electrode material and battery disclosed in the present invention, and includes most of the operating steps in Example 1, except that the mass of the organic carbon source is 20% of the mass of the water-soluble raw material, and the amount of the organic carbon source is 1.1 mol.

[0083] Embodiment 11

[0084] This example is used to illustrate the sodium iron phosphate positive electrode material and battery disclosed in the present invention, and includes most of the operating steps in Example 1, except that the mass of the organic carbon source is 30% of the mass of the water-soluble raw material, and the amount of the organic carbon source is 1.6 mol.

[0085] Example 12

[0086] This example is used to illustrate the sodium iron phosphate positive electrode material and battery disclosed in the present invention, and includes most of the operating steps in Example 1, except that the mass of the organic carbon source is 1% of the mass of the water-soluble raw material, and the amount of the organic carbon source is 0.05 mol.

[0087] Comparative Example 1

[0088] This comparative example is used to compare and illustrate the sodium iron phosphate positive electrode material and battery disclosed in the present invention, and includes most of the operating steps in Example 1, except that step (2) is not included, and the mixed solution is directly stirred and dried.

[0089] Performance Testing

[0090] 1. The rate performance of the batteries prepared in the above examples and comparative examples was tested using a three-electrode system.

[0091] Rate performance test: Charge and discharge were carried out at current rates of 0.1C, 0.2C, 0.5C, and 1C to evaluate the rate performance of the material. The test results are shown in Table 1.

[0092] Table 1

[0093]

[0094] It can be seen from the test results of Examples 1-12 and Comparative Example 1 that the battery assembled using the sodium iron phosphate positive electrode material prepared in this embodiment as the positive electrode active material is conducive to the high-speed conduction of ions and electrons, and has better capacity performance and rate performance. It can be seen from the test results of Example 1 and Examples 5-8 that when the mass ratio of the mixed solution to ethanol is in the range of (1:1)-(10:1), it is beneficial to limit the growth of grains, but when the amount of ethanol added is too small, the grain growth size increases, affecting the composition morphology of the sodium iron phosphate positive electrode material, and further affecting the discharge capacity and rate performance of the battery. It can be seen from the test results of Example 1 and Example 8 that by adding a conductive agent, the electronic conductivity of the sodium iron phosphate positive electrode material is further increased, thereby increasing the rate performance of the battery. It can be seen from the test results of Example 1 and Examples 9-12 that when the mass of the organic carbon source is 2%-20% of the mass of the water-soluble raw material, a dense coating layer can be formed on the surface of the sodium iron phosphate positive electrode material. When it is lower or higher than this range, it will affect the formation of the coating layer, thereby affecting the discharge capacity and rate performance of the battery.

[0095] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A sodium iron phosphate positive electrode material, characterized in that: The sodium iron phosphate positive electrode material has a core-shell structure, the particle size of the core-shell structure is 50-1000nm, the core-shell structure includes a core body and a carbon coating layer, the core body includes sodium iron pyrophosphate, and the thickness of the carbon coating layer is 3-10nm.

2. The sodium iron phosphate positive electrode material according to claim 1, characterized in that The core body further includes a conductive agent, which is doped into the sodium iron pyrophosphate, and the conductive agent includes one or more of graphene oxide, carbon nanotubes, and carbon black.

3. A method for preparing the sodium iron phosphate positive electrode material as claimed in claim 1 or 2, characterized in that: The following steps are involved: Obtaining a water-soluble organic carbon source and a water-soluble raw material containing a Na source, an Fe source, and a P source; dissolving the organic carbon source and the water-soluble raw material in water to obtain a mixed solution; Adding an organic solvent to the mixed solution in a stirring state until no more crystals are precipitated in the mixed solution; drying the mixed solution containing the crystal grains to obtain a precursor powder; The precursor powder is calcined to obtain a sodium iron phosphate positive electrode material.

4. The method for preparing the sodium iron phosphate positive electrode material according to claim 3, characterized in that: The mass ratio of the mixed solution to the organic solvent is (1:1)-(10:1).

5. The method for preparing the sodium iron phosphate positive electrode material according to claim 3, characterized in that: The organic solvent includes one or more of N-methylpyrrolidone, dimethylformamide, methanol, ethanol, ethylene glycol, propanol, isopropanol, propylene glycol, n-butanol, acetonitrile and acetone.

6. The method for preparing the sodium iron phosphate positive electrode material according to claim 3, characterized in that: The organic carbon source includes one or more of glucose, sucrose, polyvinyl pyrrolidone, cellulose, starch, polyethylene glycol, polystyrene, polyvinyl alcohol, polyethylene, polypropylene, citric acid, and stearic acid; The water-soluble raw materials include at least two of ferric nitrate, ferric sulfate, ferric acetate, ferric chloride, ferric citrate, ferric tartrate, ferric tribromide, sodium dihydrogen phosphate, disodium hydrogen phosphate, sodium phosphate, sodium pyrophosphate, phosphoric acid, sodium hexametaphosphate, sodium carbonate, sodium acetate, sodium sulfide, sodium chloride, and sodium sulfate.

7. The method for preparing the sodium iron phosphate positive electrode material according to claim 3, characterized in that: The mass of the organic carbon source is 2%-20% of the mass of the water-soluble raw material; the mass ratio of the sum of the mass of the organic carbon source and the water-soluble raw material to the mass of the water is (1:1)-(10:1).

8. The method for preparing the sodium iron phosphate positive electrode material according to claim 3, characterized in that: The drying method is drying or spray drying, and the drying is stirring drying at 78-82°C; The calcination conditions are: in a protective atmosphere, heating to 450°C-600°C at a heating rate of 5-10°C / min, and calcining for 5-30 hours.

9. A positive electrode, characterized in that The invention comprises the sodium iron phosphate positive electrode material according to claim 1 or 2, or comprises the sodium iron phosphate positive electrode material prepared by the preparation method of the sodium iron phosphate positive electrode material according to any one of claims 3 to 8.

10. A battery, characterized in that: Comprising the positive electrode as claimed in claim 9.

Citation Information

Cited By

  • Iron-based phosphate positive electrode material and preparation method and application thereof

    CN119812287A

  • Iron-based phosphate positive electrode material and preparation method and application thereof

    CN119812287B

  • Sodium ferric pyrophosphate positive electrode material and preparation method thereof

    CN119920899A

  • A sodium ferric pyrophosphate positive electrode material and a preparation method thereof

    CN119920899B