Long-circulation sodium ion battery positive electrode material and preparation method thereof

By coating the surface of the positive electrode material of sodium-ion batteries with a sodium tetrafluoroborate protective film, the problem of residual alkali was solved, the cycle and rate performance of the battery was improved, and the reuse of the positive electrode active material was realized.

CN119008912AInactive Publication Date: 2024-11-22安徽吉厚智能科技有限公司

Patent Information

Application Number
CN202411249544.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-06
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing sodium-ion battery cathode materials have high residual alkali content during the preparation process, resulting in poor air stability, poor processing performance, and side reactions with the electrolyte during cycling, which affects battery performance.

Method used

A sodium tetrafluoroborate protective film is coated on the surface of the positive electrode active material. Sodium tetrafluoroborate is generated by the reaction of fluoroboric acid with sodium carbonate residue on the material surface, which prevents residual alkali from affecting the cycle process and forms a CEI film to improve battery performance.

Benefits of technology

It significantly improves the cycle and rate performance of sodium-ion batteries, solves the negative impact of residual alkali on battery performance, and enables the reuse of positive electrode active materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119008912A_ABST
    Figure CN119008912A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of sodium-ion batteries, and particularly discloses a long-circulation sodium-ion battery positive electrode material which comprises a positive electrode active material and a protective film coated outside the positive electrode active material, the general formula of the positive electrode active material is Naa (NixFeyMn (1-x-y)) O2; wherein a is greater than or equal to 0.9 and less than or equal to 1.5; 0.1 < = x < = 0.4; 0.1 < = y < = 0.4. According to the long-circulation sodium ion battery positive electrode material and the preparation method thereof provided by the invention, fluoboric acid reacts with residual sodium carbonate on the surface of the material to generate a new substance sodium tetrafluoroborate, and the substance coats the surface of a positive electrode active material in a drying process, so that the influence of existence of residual alkali on a circulation process is prevented.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of sodium ion batteries, and in particular relates to a long-cycle sodium ion battery positive electrode material and a preparation method thereof. Background Art

[0002] At present, layered oxides for sodium-ion batteries are widely used because their preparation process is similar to that of lithium batteries. Among them, the P2 phase material has high voltage, low residual alkali, good processing performance but low capacity; the O3 phase material has high capacity but due to the high sodium ratio in the preparation process, it leads to high residual alkali, poor air stability and poor processing performance; in particular, these residual alkalis will cause gas production during the cycle, and react with the electrolyte to deteriorate the cycle, and more residual alkali will also cause process problems such as gelation of the slurry during the slurry mixing process. Therefore, solving the problem of high residual alkali on the surface of O3 phase materials has become a common goal now. Summary of the invention

[0003] The purpose of the present invention is to overcome the above problems existing in the prior art and provide a long-cycle sodium ion battery positive electrode material and a preparation method thereof. Fluoroboric acid reacts with sodium carbonate remaining on the surface of the material to generate a new substance, sodium tetrafluoroborate, which is coated on the surface of the positive electrode active material during the drying process to prevent the presence of residual alkali from affecting the cycle process.

[0004] In order to achieve the above technical objectives and the above technical effects, the present invention is implemented through the following technical solutions:

[0005] An embodiment of the first aspect of the present invention provides a long-cycle sodium-ion battery positive electrode material, comprising a positive electrode active material and a protective film coated on the outside of the positive electrode active material;

[0006] The general formula of the positive electrode active material is Na a (Ni x Fe y Mn (1-x-y) ) 2 ;

[0007] Among them, 0.9≤a≤1.5;

[0008] 0.1≤x≤0.4;

[0009] 0.1≤y≤0.4.

[0010] Furthermore, the protective film is sodium tetrafluoroborate.

[0011] The embodiment of the second aspect of the present invention provides a method for preparing a positive electrode material for a long cycle sodium ion battery, the preparation method comprising the following steps:

[0012] S1: Weigh the precursor (Ni x Fey Mn (1-x-y) )OH 2 and sodium carbonate, and mix them evenly in a high-speed mixer to obtain a mixture;

[0013] S2: The mixed material is placed in the cartridge and sintered at high temperature in an atmosphere furnace to prepare the positive electrode active material Na a (Ni x Fe y Mn (1-x-y) ) 2 ;

[0014] S3: The positive electrode active material Na a (Ni x Fe y Mn (1-x-y) ) 2 The material is placed in a stirring tank and stirred continuously, and a boric acid aqueous solution is added into the stirring tank for a mixing reaction. The solid content is controlled during the mixing reaction. After the mixing reaction is completed, the long-cycle sodium ion battery positive electrode material is obtained by drying.

[0015] Furthermore, in step S1, the sodium carbonate is battery-grade sodium carbonate.

[0016] Further, in step S1, the precursor (Ni x Fe y Mn (1-x-y) )OH 2 In the process of uniformly mixing the sodium carbonate and the sodium carbonate in the high-speed mixer, the rotation speed of the high-speed mixer is 500-1000r / min, and the mixing time is 30-60min.

[0017] Furthermore, in step S2, during the high temperature sintering process, the sintering temperature is 800-1000°C, and the sintering time is 10-15h.

[0018] Furthermore, in step S3, the concentration of the boric acid aqueous solution is 0.05-0.10 mol / L.

[0019] Furthermore, in step S3, during the mixing reaction, the solid content is controlled to be 70-90%; preferably, the solid content is controlled to be 80%.

[0020] Furthermore, in step S3, the mixing reaction time is 30-60 min.

[0021] Furthermore, in step S3, during the drying process, the drying temperature is 150-200°C.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] 1. The present invention provides a long-cycle sodium-ion battery positive electrode material, wherein a protective film is coated on the outside of the positive electrode active material, and the protective film is sodium tetrafluoroborate, which can prevent the presence of residual alkali from affecting the cycle process.

[0024] 2. The present invention provides a method for preparing a long-cycle sodium-ion battery positive electrode material. In the preparation method, a precursor (Ni x Fe y Mn (1-x-y) )OH 2 and sodium carbonate as raw materials to prepare positive electrode active materials, and then the positive electrode active materials are mixed with a boric acid and fluoric acid aqueous solution, and by controlling the concentration, solid content and mixing reaction time of fluoric acid during the mixing reaction process, fluoric acid reacts with sodium carbonate remaining on the surface of the positive electrode active material to generate a new substance, sodium tetrafluoroborate, which is coated on the surface of the positive electrode active material during the drying process. During the cycle of the battery, the sodium tetrafluoroborate on the surface of the positive electrode active material is more conducive to the formation of a CEI film, thereby significantly improving the cycle and rate performance of the battery.

[0025] 3. In the prior art, the sodium carbonate remaining on the surface of the positive electrode active material is generally removed by washing with water. This method will cause the sodium ions inside the positive electrode active material to dissolve, thereby reducing the capacity of the positive electrode active material. The present invention generates a new substance, sodium tetrafluoroborate, by reacting fluoroboric acid with the sodium carbonate remaining on the surface of the material. This not only solves the problem of sodium carbonate remaining on the surface of the positive electrode active material, but also allows the residual alkali to be reused. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] The drawings described herein are used to provide a further understanding of the present invention and constitute a part of this application. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:

[0027] Figure 1 is a scanning electron microscope image of the positive electrode material prepared in Example 1 of the present invention;

[0028] Figure 2 is the XRD pattern of the positive electrode material prepared in Example 1 of the present invention;

[0029] Figure 3 The particle size diagram of the positive electrode material prepared in Example 1 of the present invention is

[0030] Figure 4 This is a scanning electron microscope image of the positive electrode material prepared in Comparative Example 1 of the present invention;

[0031] Figure 5 It is a scanning electron microscope image of the positive electrode material prepared in Comparative Example 2 of the present invention. DETAILED DESCRIPTION

[0032] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0033] The embodiment of the first aspect of the present invention provides a long-cycle sodium ion battery positive electrode material, comprising a positive electrode active material and a protective film coated on the outside of the positive electrode active material, wherein the protective film is sodium tetrafluoroborate;

[0034] The general formula of the positive electrode active material is Na a (Ni x Fe y Mn (1-x-y) ) 2 ;

[0035] Among them, 0.9≤a≤1.5;

[0036] 0.1≤x≤0.4;

[0037] 0.1≤y≤0.4.

[0038] The embodiment of the second aspect of the present invention provides a method for preparing a positive electrode material for a long cycle sodium ion battery, the preparation method comprising the following steps:

[0039] S1: Preparation of mixture

[0040] According to the general formula of the positive electrode active material provided by the embodiment of the first aspect of the present invention, the precursor (Ni x Fe y Mn (1-x-y) )OH 2 and battery grade sodium carbonate, the precursor (Ni x Fe y Mn (1-x-y) )OH 2 and battery-grade sodium carbonate in a high-speed mixer for 30-60 minutes, and after mixing evenly, a mixture is prepared;

[0041] In step S1, the speed of the high-speed mixer is 500-1000 r / min;

[0042] S2: Preparation of positive electrode active materials

[0043] The mixed material prepared in step S1 is placed in a box body and sintered at 800-1000°C for 10-15h in an atmosphere furnace to prepare the positive electrode active material Na a (Ni x Fe y Mn(1-x-y) ) 2 ;

[0044] S3: Preparation of long-cycle sodium-ion battery cathode materials

[0045] Prepare a boric acid aqueous solution with a concentration of 0.05-0.10 mol / L;

[0046] The positive electrode active material Na a (Ni x Fe y Mn (1-x-y) ) 2 The mixture is placed in a stirring tank and stirred continuously. During the stirring process, the prepared boric acid and fluoric acid aqueous solution is added into the stirring tank for a mixing reaction for 30-60 minutes. During the mixing reaction process, the solid content is controlled to be 70-90%. Finally, the long-cycle sodium ion battery positive electrode material is prepared by drying.

[0047] Wherein, preferably the solid content is 80%;

[0048] In step S3, during the drying process, the drying temperature is 150-200°C.

[0049] In the prior art, the sodium carbonate remaining on the surface of the positive electrode active material is generally removed by washing with water, which may cause the sodium ions inside the positive electrode active material to dissolve, thereby reducing the capacity of the positive electrode active material.

[0050] In the preparation method, a precursor (Ni x Fe y Mn (1-x-y) )OH 2 and sodium carbonate as raw materials to prepare positive electrode active materials, and then the positive electrode active materials are mixed with a boric acid and fluoric acid aqueous solution, and by controlling the concentration, solid content and mixing reaction time of fluoric acid during the mixing reaction process, fluoric acid reacts with sodium carbonate remaining on the surface of the positive electrode active material to generate a new substance, sodium tetrafluoroborate, which is coated on the surface of the positive electrode active material during the drying process. During the cycle of the battery, the sodium tetrafluoroborate on the surface of the positive electrode active material is more conducive to the formation of a CEI film, thereby significantly improving the cycle and rate performance of the battery.

[0051] The following are specific examples. Unless otherwise specified, all raw materials in the following examples can be obtained from commercial sources.

[0052] Example 1

[0053] This embodiment provides a method for preparing a positive electrode material for a long-cycle sodium ion battery, the method comprising the following steps:

[0054] S1: Preparation of mixture

[0055] According to the general formula of the positive electrode active material, wherein the sodium ratio a is 1.01, weigh 1 kg of the precursor (Ni 0.2 Fe 0.2 Mn 0.6 )OH 2 and 0.72 kg of battery-grade sodium carbonate, the precursor (Ni 0.2 Fe 0.2 Mn 0.6 )OH 2 and battery-grade sodium carbonate in a high-speed mixer at a speed of 800 r / min for 45 min, and after mixing evenly, a mixture is prepared;

[0056] S2: Preparation of positive electrode active materials

[0057] The mixed material prepared in step S1 is placed in the box body and sintered at high temperature in an atmosphere furnace. The sintering atmosphere is air, the sintering temperature is 950°C, and the sintering time is 12h to prepare the positive electrode active material Na 1.01 (Ni 0.2 Fe 0.2 Mn 0.6 ) 2 ;

[0058] S3: Preparation of positive electrode material coated with sodium tetrafluoroborate

[0059] Prepare a 0.05 mol / L aqueous solution of boric acid;

[0060] The positive electrode active material Na 1.01 (Ni 0.2 Fe 0.2 Mn 0.6 ) 2 The mixture was placed in a stirring tank and stirred continuously. During the stirring process, the prepared boric acid and fluoric acid aqueous solution was added into the stirring tank for mixing reaction for 30 minutes. During the mixing reaction process, the solid content was controlled to be 80%. The mixture was dried at 150° C. to obtain a positive electrode material coated with sodium tetrafluoroborate.

[0061] The prepared positive electrode material coated with sodium tetrafluoroborate was subjected to rate tests of 0.1C, 0.5C, 1C, 5C, and 10C and a 1C-50 cycle test. The test results are shown in Table 1.

[0062] Example 2

[0063] This embodiment provides a method for preparing a positive electrode material for a long-cycle sodium ion battery, the method comprising the following steps:

[0064] S1: Preparation of mixture

[0065] According to the general formula of the positive electrode active material, wherein the sodium ratio a is 0.9, weigh 1 kg of the precursor (Ni0.1 Fe 0.1 Mn 0.8 )OH 2 and 0.72 kg of battery-grade sodium carbonate, the precursor (Ni 0.1 Fe 0.1 Mn 0.8 )OH 2 and battery-grade sodium carbonate in a high-speed mixer at a speed of 500 r / min for 60 min, and after mixing evenly, a mixture is prepared;

[0066] S2: Preparation of positive electrode active materials

[0067] The mixed material prepared in step S1 is placed in a box body and sintered at high temperature in an atmosphere furnace. The sintering atmosphere is air, the sintering temperature is 800°C, and the sintering time is 15h to prepare the positive electrode active material Na 0.9 (Ni 0.1 Fe 0.1 Mn 0.8 ) 2 ;

[0068] S3: Preparation of positive electrode material coated with sodium tetrafluoroborate

[0069] Prepare a 0.08 mol / L aqueous solution of boric acid;

[0070] The positive electrode active material Na 0.9 (Ni 0.1 Fe 0.1 Mn 0.8 ) 2 The mixture was placed in a stirring tank and stirred continuously. During the stirring process, the prepared boric acid and fluoric acid aqueous solution was added into the stirring tank for a mixing reaction for 60 minutes. During the mixing reaction process, the solid content was controlled to be 70%. The mixture was dried at 200° C. to obtain a positive electrode material coated with sodium tetrafluoroborate.

[0071] The prepared positive electrode material coated with sodium tetrafluoroborate was subjected to rate tests of 0.1C, 0.5C, 1C, 5C, and 10C and a 1C-50 cycle test. The test results are shown in Table 1.

[0072] Example 3

[0073] This embodiment provides a method for preparing a positive electrode material for a long-cycle sodium ion battery, the method comprising the following steps:

[0074] S1: Preparation of mixture

[0075] According to the general formula of the positive electrode active material, wherein the sodium ratio a is 1.50, weigh 1 kg of the precursor (Ni 0.4 Fe 0.4 Mn0.2 )OH 2 and 0.72 kg of battery-grade sodium carbonate, the precursor (Ni 0.4 Fe 0.4 Mn 0.2 )OH 2 and battery-grade sodium carbonate in a high-speed mixer at a speed of 1000 r / min for 30 min, and after mixing evenly, a mixture is prepared;

[0076] S2: Preparation of positive electrode active materials

[0077] The mixed material prepared in step S1 is placed in a box body and sintered at high temperature in an atmosphere furnace. The sintering atmosphere is air, the sintering temperature is 1000°C, and the sintering time is 10 hours to prepare the positive electrode active material Na 1.50 (Ni 0.4 Fe 0.4 Mn 0.2 ) 2 ;

[0078] S3: Preparation of positive electrode material coated with sodium tetrafluoroborate

[0079] Prepare a 0.10 mol / L aqueous solution of boric acid;

[0080] The positive electrode active material Na 1.50 (Ni 0.4 Fe 0.4 Mn 0.2 ) 2 The mixture was placed in a stirring tank and stirred continuously. During the stirring process, the prepared boric acid and fluoric acid aqueous solution was added into the stirring tank for mixing reaction for 40 minutes. During the mixing reaction process, the solid content was controlled to be 90%. The mixture was dried at 180° C. to obtain a positive electrode material coated with sodium tetrafluoroborate.

[0081] The prepared positive electrode material coated with sodium tetrafluoroborate was subjected to rate tests of 0.1C, 0.5C, 1C, 5C, and 10C and a 1C-50 cycle test. The test results are shown in Table 1.

[0082] Comparative Example 1

[0083] This comparative example provides a method for preparing a long-cycle sodium ion battery positive electrode material, the method comprising the following steps:

[0084] S1: Preparation of mixture

[0085] According to the general formula of the positive electrode active material, wherein the sodium ratio a is 1.01, weigh 1 kg of the precursor (Ni 0.2 Fe 0.2 Mn 0.6 )OH 2and 0.72 kg of battery-grade sodium carbonate, the precursor (Ni 0.2 Fe 0.2 Mn 0.6 )OH 2 and battery-grade sodium carbonate in a high-speed mixer at a speed of 800 r / min for 45 min, and after mixing evenly, a mixture is prepared;

[0086] S2: Preparation of positive electrode active materials

[0087] The mixed material prepared in step S1 is placed in the box body and sintered at high temperature in an atmosphere furnace. The sintering atmosphere is air, the sintering temperature is 950°C, and the sintering time is 12h to prepare the positive electrode material Na 1.01 (Ni 0.2 Fe 0.2 Mn 0.6 ) 2 ;

[0088] The prepared positive electrode active material was subjected to rate tests of 0.1C, 0.5C, 1C, 5C, and 10C and a 1C-50 cycle test. The test results are shown in Table 1.

[0089] Comparative Example 2

[0090] This comparative example provides a method for preparing a long-cycle sodium ion battery positive electrode material, the method comprising the following steps:

[0091] S1: Preparation of mixture

[0092] According to the general formula of the positive electrode active material, wherein the sodium ratio a is 1.01, weigh 1 kg of the precursor (Ni 0.2 Fe 0.2 Mn 0.6 )OH 2 and 0.72 kg of battery-grade sodium carbonate, the precursor (Ni 0.2 Fe 0.2 Mn 0.6 )OH 2 and battery-grade sodium carbonate in a high-speed mixer at a speed of 800 r / min for 45 min, and after mixing evenly, a mixture is prepared;

[0093] S2: Preparation of positive electrode active materials

[0094] The mixed material prepared in step S1 is placed in the box body and sintered at high temperature in an atmosphere furnace. The sintering atmosphere is air, the sintering temperature is 950°C, and the sintering time is 12h to prepare the positive electrode active material Na 1.01 (Ni 0.2 Fe 0.2 Mn 0.6 ) 2 ;

[0095] S3: Preparation of positive electrode materials

[0096] The positive electrode active material Na 1.01 (Ni 0.2 Fe 0.2 Mn 0.6 ) 2 The mixture was placed in a stirring tank and stirred continuously. During the stirring process, deionized water was added to the stirring tank for a mixing reaction for 30 minutes. During the mixing reaction process, the solid content was controlled to be 80%. The positive electrode material was prepared by drying at 150° C.;

[0097] The prepared positive electrode material was subjected to rate tests of 0.1C, 0.5C, 1C, 5C, and 10C and a 1C-50 cycle test. The test results are shown in Table 1.

[0098] Table 1

[0099]

[0100]

[0101] According to the data in Table 1, the 1C-50 cycle retention rates of the positive electrode materials prepared in Examples 1-3 are better than those of Comparative Examples 1-2, indicating that the positive electrode materials provided by the present invention have better performance.

[0102] Figures 1 to 3 The scanning electron microscope image, XRD image and particle size image of the positive electrode material prepared in Example 1 are respectively; Figure 4 This is a scanning electron microscope image of the positive electrode material prepared in Comparative Example 1. Figure 5 This is a scanning electron microscope image of the positive electrode material prepared in Comparative Example 2.

[0103] The invention provides a long-cycle sodium ion battery positive electrode material. The positive electrode material is coated with a protective film on the outside, and the protective film is sodium tetrafluoroborate, which can prevent the influence of residual alkali on the cycle process.

[0104] The present invention also provides a method for preparing a long-cycle sodium ion battery positive electrode material. In the preparation method, a precursor (Ni x Fe y Mn (1-x-y) )OH 2and sodium carbonate as raw materials to prepare positive electrode materials, which are then mixed with a boric acid and fluoroboric acid aqueous solution. By controlling the concentration, solid content and mixing reaction time of fluoroboric acid during the mixing reaction, fluoroboric acid reacts with sodium carbonate remaining on the surface of the material to generate a new substance, sodium tetrafluoroborate. This substance is coated on the surface of the positive electrode material during the drying process. During the cycle of the battery, the sodium tetrafluoroborate on the surface of the positive electrode material is more conducive to the formation of a CEI film, thereby significantly improving the cycle and rate performance of the battery.

[0105] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0106] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, and these changes and improvements all fall within the scope of the present invention to be protected.

Claims

1. A long cycle sodium ion battery positive electrode material, characterized in that: It includes a positive electrode active material and a protective film coated on the outside of the positive electrode active material; The general formula of the positive electrode active material is Na a (Ni x Fe y Mn (1-x-y) )O2; Among them, 0.9≤a≤1.5; 0.1≤x≤0.4; 0.1≤y≤0.4。 2. A long cycle sodium ion battery positive electrode material according to claim 1, characterized in that: The protective film is sodium tetrafluoroborate.

3. A method for preparing a long-cycle sodium ion battery positive electrode material according to any one of claims 1 to 2, characterized in that: The preparation method comprises the following steps: S1: Weigh the precursor (Ni x Fe y Mn (1-x-y) ) OH2 and sodium carbonate are mixed uniformly in a high-speed mixer to obtain a mixture; S2: The mixed material is placed in the cartridge and sintered at high temperature in an atmosphere furnace to prepare the positive electrode active material Na a (Ni x Fe y Mn (1-x-y) )O2; S3: The positive electrode active material Na a (Ni x Fe y Mn (1-x-y) )O2 is placed in a stirring tank. During the continuous stirring process, an aqueous solution of boric acid and fluoric acid is added into the stirring tank for a mixing reaction. The solid content is controlled during the mixing reaction. After the mixing reaction is completed, the long-cycle sodium ion battery positive electrode material is obtained by drying.

4. The method for preparing a long cycle sodium ion battery positive electrode material according to claim 3, characterized in that: In step S1, the sodium carbonate is battery-grade sodium carbonate.

5. The method for preparing a long cycle sodium ion battery positive electrode material according to claim 3, characterized in that: In step S1, the precursor (Ni x Fe y Mn (1-x-y) ) During the process of uniformly mixing OH2 and sodium carbonate in the high-speed mixer, the speed of the high-speed mixer is 500-1000r / min and the mixing time is 30-60min.

6. The method for preparing a long cycle sodium ion battery positive electrode material according to claim 3, characterized in that: In step S2, during the high temperature sintering process, the sintering temperature is 800-1000°C and the sintering time is 10-15h.

7. The method for preparing a long cycle sodium ion battery positive electrode material according to claim 3, characterized in that: In step S3, the concentration of the boric acid aqueous solution is 0.05-0.10 mol / L.

8. The method for preparing a long cycle sodium ion battery positive electrode material according to claim 3, characterized in that: In step S3, during the mixing reaction, the solid content is controlled to be 70-90%.

9. The method for preparing a long cycle sodium ion battery positive electrode material according to claim 3, characterized in that: In step S3, the mixing reaction time is 30-60 min.

10. The method for preparing a long cycle sodium ion battery positive electrode material according to claim 3, characterized in that: In step S3, during the drying process, the drying temperature is 150-200°C.

Citation Information

Patent Citations

  • Sodium ion battery positive electrode material as well as preparation method and application thereof

    CN112928252A

  • Coated positive electrode material as well as preparation method and application thereof

    CN115188945A

  • Method for reducing content of residual alkali on surface of layered positive electrode material of sodium-ion battery, positive electrode material of sodium-ion battery and sodium-ion battery

    CN116495800A

  • Preparation method of low-residual alkali sodium ion battery layered oxide positive electrode material

    CN118062908A

  • Lithium secondary battery

    JP1997092280A

Cited By

  • Fluoro boric acid composite coated sodium ion battery layered positive electrode material and preparation method thereof

    CN119890284A