Preparation method of network modified flow battery graphite felt positive electrode material constructed by loading MOFs (Metal-Organic Frameworks) material on conductive additive

The hydrophilicity of graphite felt is improved through plasma and acid treatment, and the MOFs material is synthesized in the conductive additive network, which solves the problem of insufficient hydrophilicity of graphite felt and significantly improves the electrode activity and efficiency of all vanadium liquid flow batteries.

CN119008977APending Publication Date: 2024-11-22SHENYANG AEROSPACE UNIVERSITY
View PDF 0 Cites 4 Cited by

Patent Information

Application Number
CN202411092848.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The hydrophilicity of the original graphite felt is poor, limiting the penetration of the electrolyte, resulting in low electrochemical activity of the electrode, which in turn affects the efficiency of the all-vana flow battery.

Method used

Plasma treatment and acid treatment are used to improve the hydrophilicity of graphite felt, introduce oxygen-containing functional groups, and synthesize MOFs materials with catalytic activity and large specific surface area in the conductive additive network to form a highly active graphite felt positive electrode material.

Benefits of technology

It significantly improves the hydrophilicity and conductivity of graphite felt, enhances the redox activity of vanadium ions and the reversibility of electrodes, improves the overall efficiency of the battery, and simplifies the preparation process, which is simple to operate, clean and efficient, energy-saving and environmentally friendly. Features.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119008977A_ABST
    Figure CN119008977A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of flow battery energy storage, and particularly relates to a preparation method of a network modified flow battery graphite felt positive electrode material constructed by loading an MOFs (Metal-Organic Frameworks) material on a conductive auxiliary agent. The preparation method comprises the following steps: firstly, cleaning a graphite felt, carrying out plasma and acid soaking dual treatment, then dissolving a conductive additive material in an ethanol solution, completely soaking and drying the treated graphite felt, then preparing a methanol solution of a metal salt and a methanol solution of an organic ligand, mixing, adding the treated graphite felt, carrying out a solvothermal reaction, washing, and drying to obtain the conductive graphite felt. And finally, loading the MOFs material. The MOFs material with a large specific surface area grows on the conductive network in situ, the MOFs material has abundant active sites and a large specific surface area, and the conductive auxiliary agent forms the conductive network on the surface of the carbon tube, so that the conductivity of the electrode and the vanadium ion conversion speed are jointly improved, and the overall efficiency of the all-vanadium redox flow battery is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of liquid flow battery energy storage, and particularly relates to a method for preparing a liquid flow battery graphite felt positive electrode material in which a MOFs material is loaded on a conductive additive to construct a network-modified liquid flow battery. Background Art

[0002] Vanadium redox flow battery (VRFB) has attracted extensive attention in energy storage and conversion due to its long cycle life, high reliability, environmental friendliness, independently adjustable power and capacity, and low operation and maintenance costs. Compared with other energy storage systems, a prominent advantage of VRFB is the use of a single vanadium sulfate solution with different vanadium valence states as the electrolyte, which significantly inhibits cross-contamination of the electrolyte.

[0003] The performance of VRFB is highly dependent on electrodes, diaphragms and electrolytes. People are committed to finding high-performance electrode materials. Most of the metal electrodes in VRFB are inert metals (gold, platinum and titanium-based metals) with good conductivity and mechanical stability. Metal electrodes were widely used in the early development of vanadium batteries, but the surface of these metal electrodes is easily passivated during the reaction process, and the electrode resistance increases. In addition, most metal electrodes with better performance are precious metals, which are expensive, making them unable to be used on a large scale in the field of VRFB. Carbon-based electrodes have the advantages of low cost, high stability and strong corrosion resistance, which can basically meet the needs of vanadium batteries for electrode materials. Among them, graphite felt has a three-dimensional network structure, which can provide transfer channels and reaction sites for vanadium ions and is widely used in the current field of liquid flow batteries. However, the original graphite felt has poor hydrophilicity, which is not conducive to the penetration of electrolyte, reduces the electrochemical activity of the electrode, and thus restricts the battery efficiency. In order to realize the large-scale application of graphite felt electrodes, the modification of graphite felt electrodes has become the focus of research. Summary of the invention

[0004] The purpose of the present invention is to provide a method for preparing a graphite felt cathode material for a modified liquid flow battery in which a MOFs material is loaded on a conductive additive to construct a network. The present invention adopts a plasma treatment and acid treatment process to improve the hydrophilicity of the graphite felt, and introduces a large number of oxygen-containing functional groups, and then uses a conductive additive material to form a stable chemical bond with the oxygen-containing functional groups on the surface of the graphite felt, forming a uniform conductive network on the surface of the graphite felt, thereby improving the hydrophilicity and conductivity of the graphite felt, and finally synthesizing a MOFs material with catalytic activity and a large specific surface area on the surface of the graphite felt, which is loaded in the conductive network to form a highly active graphite felt cathode material with strong hydrophilicity, strong conductivity, and a large number of reactive active sites.

[0005] In order to achieve the above object, the technical solution of the present invention is as follows:

[0006] On the one hand, the present invention provides a method for preparing a graphite felt positive electrode material for a liquid flow battery in which a MOFs material is loaded on a conductive additive to construct a network-modified material, the method comprising the following steps:

[0007] (1) soaking the graphite felt in an ethanol solution, ultrasonically cleaning it, and then drying it to obtain a graphite felt;

[0008] (2) subjecting the graphite felt 1 obtained in step (1) to plasma treatment to obtain graphite felt 2;

[0009] (3) soaking the graphite felt 2 obtained in step (2) in a sulfuric acid solution for acid treatment, rinsing with deionized water to remove excess acid, and drying to obtain graphite felt 3;

[0010] (4) dispersing a conductive aid in ethanol to obtain a conductive aid solution;

[0011] (5) soaking the graphite felt 3 obtained in step (3) in the conductive auxiliary agent solution obtained in step (4), taking out, and drying to obtain graphite felt 4;

[0012] (6) mixing the methanol solution of the metal salt and the methanol solution of the organic ligand with the graphite felt 4 obtained in step (5), and performing a solvothermal reaction to obtain graphite felt 5;

[0013] (7) The graphite felt obtained in step (6) is washed with methanol to remove unreacted metal salts and organic ligands, dried by vacuum heating, and then carbonized in an inert atmosphere to obtain a network-modified graphite felt material in which a MOFs material is loaded on a conductive additive.

[0014] In the above technical solution, further, in step (1), the thickness of the graphite felt is 1 to 4 mm, and the size of the graphite felt is based on the size of the electrode sheet in the battery testing system, such as 1×1 cm, 2×2 cm, 3×3 cm.

[0015] In the above technical solution, further, in step (1), the temperature of the ultrasonic cleaning is 10-50°C, and the time is 20-120 minutes; the temperature of the drying is 60-100°C.

[0016] In the above technical solution, further, in step (2), the plasma treatment power is 500-900W, the treatment time is 60-120s, the treatment method is to treat the back and front sides separately, and the plasma treatment equipment is a normal temperature and pressure rotary jet type plasma surface treatment equipment.

[0017] In the above technical solution, further, in step (3), the sulfuric acid concentration is 70-98wt%; the acid treatment temperature is 60-90°C, and the treatment time is 1-6h; the drying temperature is 60-100°C.

[0018] In the above technical solution, further, in step (4), the conductive aid is one of CNT and GO; and the concentration of the conductive aid in the conductive aid solution is 0.5-5 mg / mL.

[0019] In the above technical solution, further, in step (6), the Co(NO 3 ) 2 6H 2 O.Ni(NO 3 ) 2 6H 2 O, Cu(NO 3 ) 2 ·3H 2 O、Zn(NO 3 ) 2 6H 2 One of the O, used to improve electrode activity.

[0020] In the above technical solution, further, in step (6), the organic ligand is one of dimethylimidazole, phthalic acid, and trimesic acid, which is used to synthesize MOFs materials with metal salts.

[0021] In the above technical scheme, further, in step (6), the concentration of the methanol solution of the metal salt is 0.02-0.2 g / mL; the concentration of the methanol solution of the organic ligand is 0.02-0.2 g / mL; the temperature of the solvent thermal reaction is 25-120°C, and the reaction time is 24-36 hours.

[0022] In the above technical solution, further, in step (7), the temperature of the vacuum heating drying is 60-100°C, and the time is 12-24 hours; the temperature of the carbonization treatment is 450-700°C, and the time is 2-4 hours.

[0023] Another aspect of the present invention provides an application of the graphite felt positive electrode material obtained by the above preparation method in an all-vanadium liquid flow battery.

[0024] The beneficial effects of the present invention are:

[0025] 1. The present invention uses normal temperature and pressure plasma equipment to treat graphite felt. The surface of the graphite fiber is etched and oxygen-containing polar groups are introduced, which significantly improves the hydrophilicity of the surface of the graphite felt. The introduction of oxygen-containing functional groups also increases the active sites of the graphite felt.

[0026] 2. The present invention controls the number of functional groups on the surface of graphite felt by acid treatment, introduces more oxygen-containing functional groups, increases the number of negative charges, and improves the electrode's VO 2+ / VO 2 + catalytic level.

[0027] 3. The present invention loads MOFs materials with a large specific surface area, and MOFs particles are evenly distributed in the superconducting network, thereby improving the redox activity of vanadium ions on the electrode surface, the electrode reversibility, and the overall efficiency of the battery.

[0028] 4. The preparation method of the present invention is simple to operate, clean, efficient, energy-saving and environmentally friendly. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 The process flow chart of the preparation method of the present invention is as follows;

[0030] Figure 2 The SEM images of the graphite felt after plasma treatment and the original graphite felt of Example 1, (a) is the original graphite felt, (b) is the graphite felt after plasma treatment;

[0031] Figure 3 The scanning electron microscope images of ZIF-67 / GO@GF in Example 1, (a) is a scanning electron microscope image, and (b) is a local magnified image;

[0032] Figure 4 The hydrophilicity test diagram of ZIF-67 / GO@GF and original graphite felt in Example 1, (a) is original graphite felt, (b) is ZIF-67 / GO@GF;

[0033] Figure 5 CV curves of the positive electrode of ZIF-67 / GO@GF and original graphite felt in Example 1;

[0034] Figure 6 This is the positive electrode EIS graph of ZIF-67 / GO@GF and original graphite felt in Example 1;

[0035] Figure 7 The cell efficiency of ZIF-67 / GO@GF and original graphite felt at different current densities in Example 1;

[0036] Figure 8 The charge and discharge curves of ZIF-67 / GO@GF and original graphite felt in Example 1. DETAILED DESCRIPTION

[0037] In order to make the purpose, technical scheme and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. The following embodiments are preferred technical schemes of the present invention. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. The embodiments of the present invention are at normal temperature and pressure.

[0038] Unless otherwise specified, the materials used in the embodiments of the present invention can be obtained through commercial channels or prepared according to conventional methods well known to those skilled in the art.

[0039] Example 1

[0040] The preparation method of ZIF-67 / GO@GF in the embodiment of the present invention comprises the following steps:

[0041] (1) cutting the graphite felt into a size of 2×2 cm in length and width and 3 mm in thickness, completely immersing it in a beaker containing an ethanol solution, placing it in an ultrasonic cleaning machine for ultrasonic cleaning at 25° C. for 2 h, and drying it at 70° C. for 4 h to obtain a graphite felt;

[0042] (2) treating the graphite felt 1 obtained in step (1) with plasma at a power of 500 W for 90 seconds on both sides to obtain graphite felt 2;

[0043] (3) soaking the graphite felt II obtained in step (2) in a 98 wt % sulfuric acid solution, heating in a water bath at 85° C. for 4 h, rinsing with deionized water, and drying in a drying oven at 60° C. for 12 h to obtain graphite felt III;

[0044] (4) Weigh 0.06 g of GO in 20 mL of ethanol and ultrasonicate for 60 min to prepare a GO solution with a concentration of 3 mg / mL;

[0045] (5) soaking the graphite felt 3 obtained in (3) in the GO solution obtained in step (4), taking it out after soaking for 20 minutes, and drying it at 70° C. to obtain graphite felt 4;

[0046] (6) Weigh 1.35 g Co(NO 3 ) 2 6H 2 O was dissolved in 60 ml of methanol and stirred evenly to prepare Co(NO 3 ) 2 5.6 g of 2-methylimidazole was dissolved in 60 ml of methanol to prepare a 0.093 g / mL 2-methylimidazole methanol solution, the two solutions were mixed, the graphite felt obtained in step (5) was immersed in the above solution, and allowed to stand at 25° C. for 24 h for solvothermal reaction to obtain graphite felt 5;

[0047] (7) The graphite felt obtained in step (6) was cleaned with methanol several times, dried by vacuum heating at 60° C. for 12 h, and then carbonized at 500° C. in an argon atmosphere for 2 h. The obtained sample was recorded as ZIF-67 / GO@GF.

[0048] Figure 2This is the SEM image of the graphite felt after plasma treatment and the original graphite felt in Example 1. It can be seen from the figure that the surface of the original graphite felt is smooth, without scratches, and some impurities are adsorbed on the surface; after the plasma treatment, the impurities on the surface of the graphite felt are blown away, and some uniform scratches appear on the fiber surface. The scratches produced after plasma treatment further increase the specific surface area of ​​the graphite fiber.

[0049] Figure 3 This is a scanning electron microscope image of ZIF-67 / GO@GF prepared in Example 1. It can be seen from the figure that graphene has an ultra-thin, flexible sheet structure. The surface of the graphite felt after plasma and acid treatment contains a large number of active functional groups. The oxygen-containing functional groups on the surface of graphene oxide combine with the functional groups on the surface of graphite felt, so that graphene can be coated on the surface of graphite fiber. ZIF-67 is a small particle with a regular dodecahedral structure, which grows in situ on the surface of graphene, and finally forms an integrated structure with graphite fiber as the matrix, graphene oxide sheets wrapped on the surface of graphite fiber, and ZIF-67 particles grown on the graphene sheets.

[0050] The hydrophilicity test of ZIF-67 / GO@GF and original graphite felt is shown in the figure. Figure 4 As shown, the contact angle of the untreated original graphite felt electrode is about 157.7°, while the graphite felt treated with plasma and introduced with MOFs material can quickly absorb deionized water, and its contact angle is about 0°, showing excellent hydrophilicity.

[0051] Figure 5 and Figure 6 The electrochemical behavior of ZIF-67 / GO@GF and original graphite felt was studied using an electrochemical workstation and a three-electrode system. ZIF-67 / GO@GF and original graphite felt were cut into 1×1 cm sizes as working electrodes, saturated calomel electrode as reference electrode, and platinum sheet as auxiliary electrode. The electrochemical properties of the electrodes were investigated by cyclic voltammetry (CV) and electrochemical impedance spectroscopy (EIS). The electrolyte solution was 0.1 mol / L VOSO 4 +3.0mol / LH 2 SO 4 solution; CV test scan rate is 5mV / s; EIS frequency is 10 -2 ~10 5 Hz, the amplitude of the sinusoidal AC signal is 10mV.

[0052] like Figure 5 As shown, ZIF-67 / GO@GF shows symmetrical oxidation peaks and reduction peaks at a scan rate of 5 mV / s, while the original graphite felt only shows an oxidation peak but no reduction peak, indicating that ZIF-67 / GO@GF has good electrochemical reversibility and the original graphite felt has poor electrochemical reversibility.

[0053] like Figure 6 As shown, R s is the sum of the resistance of the electrolyte solution and the electrode, that is, the ohmic resistance, and R ct represents the charge transfer resistance in the interface between the electrolyte solution and the battery. It is worth noting that the R ct The value is 103Ω lower than that of GF. The R s The value is 2.155Ω lower than that of GF, and the semicircular diameter of ZIF-67 / GO@GF is also smaller than that of GF. This is because the introduction of the conductive network formed by the composite material ZIF-67 / GO@GF is more conducive to the conduction between the fibers, making the contact between the fibers and the electrolyte more sufficient, and the charge transfer resistance is also reduced.

[0054] Table 1 shows the impedance fitting data of graphite felt and ZIF-67 / GO@GF.

[0055] Table 1

[0056]

[0057] The ZIF-67 / GO@GF sample prepared in Example 1 and the original graphite felt were used as the positive electrode, and the negative electrode was the untreated graphite felt. The batteries were assembled and the battery performance was tested. The positive and negative electrolytes were both 20 mL of 3.5-valent vanadium. -2 Up to 200mAcm -2 The charge and discharge tests were carried out under variable current density. The results are as follows Figure 7 The coulombic efficiency, voltage efficiency and energy efficiency of the battery with the graphite felt prepared in Example 1 as the positive electrode at different current densities are higher than those of the unmodified original graphite felt. -2 At a current density of 1.547 W, the coulomb efficiency is 97.71%, the voltage efficiency is 70.81%, and the energy efficiency is 69.01%. Compared with the energy efficiency of the original graphite felt, which is only 64%, it has increased by 7.8%. Figure 8 As shown in the figure, ZIF-67 / GO@GF sample and original graphite felt were used as positive electrode, and untreated graphite felt was used as negative electrode. -2 Charge and discharge test at current density of 80mA / cm 2At a current density of 1.35V, the battery with ZIF-67 / GO@GF as the positive electrode has a charging voltage of 1.5V compared to the battery with the original graphite felt as the positive electrode, indicating that ZIF-67 / GO@GF has a lower charging voltage. During the discharge process, the battery with ZIF-67 / GO@GF as the positive electrode showed a higher discharge voltage of 1.42V, while the discharge voltage of the original graphite felt was 1.29V. The modified electrode material has a smaller charging voltage and a larger discharge voltage, which indicates that the ZIF-67 / GO@GF electrode has a smaller electrochemical polarization.

[0058] Example 2

[0059] The preparation method of Ni-MOF / CNT@GF in the embodiment of the present invention comprises the following steps:

[0060] (1) cutting the graphite felt into a size of 2×2 cm in length and width and 3 mm in thickness, completely immersing it in a beaker containing an ethanol solution, placing it in an ultrasonic cleaning machine for ultrasonic cleaning at 25° C. for 2 h, and drying it at 70° C. for 6 h to obtain a graphite felt;

[0061] (2) treating the front and back surfaces of the graphite felt obtained in step (1) with plasma at a power of 500 W for 120 s to obtain graphite felt 2;

[0062] (3) soaking the graphite felt II obtained in step (2) in a sulfuric acid solution with a concentration of 80 wt%, heating it in a water bath at 85° C. for 4 h, rinsing it with deionized water, and drying it in a drying oven at 60° C. for 12 h to obtain graphite felt III;

[0063] (4) Weigh 0.06 g of CNT and ultrasonicate it in 20 mL of ethanol for 60 min to prepare a CNT solution with a concentration of 3 mg / mL;

[0064] (5) soaking the graphite felt 3 obtained in (3) in the CNT solution obtained in step (4), taking it out after soaking for 20 minutes, and drying it at 70° C. to obtain graphite felt 4;

[0065] (6) Weigh 3.0 g Ni(NO 3 ) 2 6H 2 O was dissolved in 60 ml of methanol and stirred evenly to prepare a Ni(NO 3 ) 2 6.6 g of 2-methylimidazole was dissolved in 60 ml of methanol to prepare a 0.11 g / mL 2-methylimidazole methanol solution, the two solutions were mixed, the graphite felt obtained in step (5) was immersed in the above solution, and allowed to stand at room temperature for 48 h for solvothermal reaction to obtain graphite felt 5;

[0066] (7) The graphite felt obtained in step (6) was cleaned with methanol several times, dried by vacuum heating at 60° C. for 12 h, and then carbonized at 550° C. in an argon atmosphere for 4 h. The obtained sample was recorded as Ni-MOF / CNT@GF.

[0067] The Ni-MOF / CNT@GF sample prepared in Example 2 was used as the positive electrode and the untreated graphite felt as the negative electrode. The battery was assembled and the battery performance was tested. The positive and negative electrolytes were both 20 mL of 3.5-valent vanadium. The test results are shown in Table 2.

[0068] Table 2

[0069]

[0070] Example 3

[0071] The method for preparing Zn-MOF / CNT@GF according to the embodiment of the present invention comprises the following steps:

[0072] (1) cutting the graphite felt into a size of 2×2 cm in length and width and 3 mm in thickness, completely immersing it in a beaker containing an ethanol solution, placing it in an ultrasonic cleaning machine for ultrasonic cleaning at 40° C. for 2 h, and drying it at 70° C. for 12 h to obtain a graphite felt;

[0073] (2) treating the front and back surfaces of the graphite felt 1 obtained in step (1) with plasma at a power of 800 W for 100 s to obtain graphite felt 2;

[0074] (3) soaking the graphite felt II obtained in step (2) in a 90 wt% sulfuric acid solution, heating in a water bath at 85° C. for 4 h, rinsing with deionized water, and drying in a drying oven at 60° C. for 12 h to obtain graphite felt III;

[0075] (4) Weigh 0.08 g of CNT and ultrasonicate it in 50 mL of ethanol for 60 min to prepare a CNT solution with a concentration of 1.6 mg / mL;

[0076] (5) soaking the graphite felt 3 obtained in (3) in the CNT solution obtained in step (4), taking it out after soaking for 40 minutes, and drying it at 70° C. to obtain graphite felt 4;

[0077] (6) Weigh 3.0 g Zn(NO 3 ) 2 6H 2 O was dissolved in 60 ml of methanol and stirred evenly to prepare a Zn(NO 3 ) 23 g of 2-methylimidazole was dissolved in 60 ml of methanol to prepare a methanol solution of 2-methylimidazole with a concentration of 0.05 g / mL. The two solutions were mixed, and the graphite felt obtained in step (5) was immersed in the above solution and allowed to stand at room temperature for 48 h for solvothermal reaction to obtain graphite felt 5.

[0078] (7) The graphite felt obtained in step (6) was cleaned with methanol several times, dried by vacuum heating at 80° C. for 12 h, and then carbonized at 450° C. in an argon atmosphere for 3 h. The obtained sample was recorded as Zn-MOF / CNT@GF.

[0079] The Zn-MOF / CNT@GF sample prepared in Example 3 was used as the positive electrode and the untreated graphite felt was used as the negative electrode. The battery was assembled and the battery performance was tested. The positive and negative electrode electrolytes were both 20 mL of 3.5-valent vanadium. The test results are shown in Table 3.

[0080] Table 3

[0081]

[0082] Example 4

[0083] The method for preparing Cu-C / GO / GF according to an embodiment of the present invention comprises the following steps:

[0084] (1) cutting the graphite felt into a size of 2×2 cm in length and width and 3 mm in thickness, completely immersing it in a beaker containing an ethanol solution, placing it in an ultrasonic cleaning machine for ultrasonic cleaning at 40° C. for 60 min, and drying it at 70° C. for 4 h to obtain a graphite felt;

[0085] (2) treating the front and back surfaces of the graphite felt 1 obtained in step (1) with plasma at a power of 600 W for 120 s to obtain graphite felt 2;

[0086] (3) soaking the graphite felt II obtained in step (2) in a 95 wt% sulfuric acid solution, heating in a water bath at 85° C. for 4 h, rinsing with deionized water, and drying in a drying oven at 60° C. for 12 h to obtain graphite felt III;

[0087] (4) Weigh 0.06 g of GO and add it to 20 mL of ethanol and ultrasonicate for 60 min to prepare a GO solution with a concentration of 3 mg / mL;

[0088] (5) soaking the graphite felt 3 obtained in (3) in the GO solution obtained in step (4), taking it out after soaking for 20 minutes, and drying it at 80° C. to obtain graphite felt 4;

[0089] (6) Weigh 3.0 g Cu(NO 3 ) 2 6H 2O was dissolved in 60 ml of methanol and stirred evenly to prepare a concentration of 0.05 g / mL Cu(NO 3 ) 2 3 g of trimesic acid was weighed and dissolved in 60 ml of methanol to prepare a methanol solution of trimesic acid with a concentration of 0.05 g / mL. The two solutions were mixed, and the graphite felt No. 4 obtained in step (5) was immersed in the above solution, and the solvent was subjected to thermal reaction at 120° C. for 12 hours to obtain graphite felt No. 5.

[0090] (7) The graphite felt obtained in step (6) was cleaned with methanol several times, dried by vacuum heating at 80° C. for 24 h, and then carbonized at 600° C. in an argon atmosphere for 4 h. The obtained sample was recorded as Cu-C / GO / GF.

[0091] The Cu-C / GO / GF sample prepared in Example 4 was used as the positive electrode and the untreated graphite felt as the negative electrode. The battery was assembled and the battery performance test was performed. The positive and negative electrode electrolytes were both 20 mL of 3.5-valent vanadium. The test results are shown in Table 4.

[0092] Table 4

[0093]

[0094] The above embodiments are only preferred embodiments of the present invention and are not intended to limit the implementation methods. The protection scope of the present invention shall be subject to the scope defined in the claims. Other different forms of changes or modifications may be made based on the above description. Obvious changes or modifications derived therefrom are still within the protection scope of the present invention.

Claims

1. A method for preparing a graphite felt positive electrode material for a liquid flow battery by loading a MOFs material on a conductive additive to construct a network-modified liquid flow battery, characterized in that: The steps include: (1) soaking the graphite felt in an ethanol solution, ultrasonically cleaning it, and then drying it to obtain a graphite felt; (2) subjecting the graphite felt 1 obtained in step (1) to plasma treatment to obtain graphite felt 2; (3) soaking the graphite felt 2 obtained in step (2) in a sulfuric acid solution for acid treatment, rinsing with deionized water, and then drying to obtain graphite felt 3; (4) dispersing a conductive aid in ethanol to obtain a conductive aid solution; (5) soaking the graphite felt obtained in step (3) in the conductive additive obtained in step (4), taking out, and drying to obtain graphite felt 4; (6) mixing the methanol solution of the metal salt and the methanol solution of the organic ligand with the graphite felt 4 obtained in step (5), and performing a solvothermal reaction to obtain graphite felt 5; (7) The graphite felt obtained in step (6) is washed with methanol, dried by vacuum heating, and then carbonized in an inert atmosphere to obtain a network-modified graphite felt material in which a MOFs material is loaded on a conductive additive.

2. The preparation method according to claim 1, characterized in that: In step (1), the temperature of the ultrasonic cleaning is 10 to 50° C. and the time is 20 to 120 min; The drying temperature is 60-100°C.

3. The preparation method according to claim 1, characterized in that: In step (2), the plasma treatment power is 500-900W, the treatment time is 60-120s, and the treatment method is to treat the back and front sides separately.

4. The preparation method according to claim 1, characterized in that: In step (3), the concentration of sulfuric acid is 70 to 98 wt %; The acid treatment temperature is 60 to 90°C and the treatment time is 1 to 6 hours; The drying temperature is 60-100°C.

5. The preparation method according to claim 1, characterized in that: In step (4), the conductive additive is one of CNT and GO; The concentration of the conductive additive solution is 0.5-5 mg / mL.

6. The preparation method according to claim 1, characterized in that: In step (6), the metal salt is one of Co(NO3)2·6H2O, Ni(NO3)2·6H2O, Cu(NO3)2·3H2O, and Zn(NO3)2·6H2O.

7. The preparation method according to claim 1, characterized in that: In step (6), the organic ligand is one of dimethylimidazole, phthalic acid, and trimesic acid.

8. The preparation method according to claim 1, characterized in that: In step (6), the concentration of the methanol solution of the metal salt is 0.02 to 0.2 g / mL; The concentration of the methanol solution of the organic ligand is 0.02 to 0.2 g / mL; The temperature of the solvent thermal reaction is 25 to 120° C., and the reaction time is 24 to 36 hours.

9. The preparation method according to claim 1, characterized in that: In step (7), the vacuum heating drying is carried out at a temperature of 60 to 100° C. for a time of 12 to 24 hours; The temperature of the carbonization treatment is 450-700° C. and the time is 2-4 hours.

10. Use of the graphite felt positive electrode material prepared by the preparation method according to any one of claims 1 to 9 in an all-vanadium liquid flow battery.

Citation Information

Cited By

  • Preparation method and application of nitrogen and oxygen double-doped porous carbon loaded graphite felt electrode

    CN119786627A

  • Graphite felt / high-entropy MOF electrode, lignin-based fuel cell and method for co-production of aviation fuel components

    CN120376664A

  • Modified graphite felt electrode for all-vanadium redox flow battery and preparation method of modified graphite felt electrode

    CN120809843A

  • Modified graphite felt electrode for all-vanadium redox flow battery and preparation method thereof

    CN120809843B