Diaphragm coating slurry for solid-state battery and preparation method of diaphragm coating slurry

By modifying the combination of materials such as alumina and carboxymethylcellulose, the adhesion and tensile strength of the ceramic coating in solid-state batteries is improved, and the problem of easy rupture of the ceramic coating under external stress is solved, which significantly improves the battery's Long-term stability.

CN119009380AActive Publication Date: 2024-11-22XINGKE ENERGY TECHNOLOGY (ANHUI) CO LTD

Patent Information

Application Number
CN202411272149.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-11
Publication Date
2024-11-22
Estimated Expiration
2044-09-11

AI Technical Summary

Technical Problem

The ceramic coating in solid-state batteries is prone to rupture under external stress, and insufficient adhesion, which affects the long-term stability of the battery.

Method used

The slurry is coated with modified alumina, carboxymethylcellulose, inorganic sol and nanofiller. The adhesion and stretching of the coating and the diaphragm substrate are improved through the preparation method and stirring process of modified alumina. strength.

Benefits of technology

The adhesion and tensile strength between the coating and the separator substrate are effectively improved, the peeling strength reaches more than 2.81N/cm, and the tensile strength reaches more than 50.2MPa, which significantly enhances the long-term stability of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119009380A_ABST
    Figure CN119009380A_ABST
Patent Text Reader

Abstract

The invention provides diaphragm coating slurry for a solid-state battery and a preparation method of the diaphragm coating slurry, and belongs to the technical field of diaphragm coating slurry. Comprising the following raw material components: 25-30% of modified aluminum oxide, 4-4.5% of carboxymethyl cellulose, 0.6-1% of a dispersing agent, 1.3-1.5% of inorganic sol, 1.5-2% of nano silicate, 0.5-0.8% of an interface compatilizer and the balance of water, the modified aluminum oxide is prepared by pickling aluminum oxide and then carrying out surface treatment with a silane coupling agent. The adhesive force between the coating and the diaphragm base material can be effectively improved, and falling is avoided; meanwhile, the tensile strength is improved, and the coating is prevented from being easily damaged; and the long-term stability of the battery is enhanced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of diaphragm coating slurry, and in particular relates to a diaphragm coating slurry for a solid-state battery and a preparation method thereof. Background Art

[0002] Solid-state batteries refer to batteries whose electrolytes are solid substances. Compared with traditional liquid electrolyte lithium batteries, they have potential advantages in safety, energy density, etc. Due to the difference in the physical state of the electrolyte, there are significant differences in the internal structure and functional realization of the two, which also affects the use of the diaphragm. The diaphragm is located between the positive and negative electrodes of the battery. Its main function is to physically isolate the two poles to prevent short circuits caused by direct contact, which is crucial in any type of lithium battery. In traditional liquid lithium batteries, the diaphragm also needs to ensure that the electrolyte can be fully infiltrated to form an efficient ion transmission channel. In solid-state batteries, although the electrolyte is replaced by a solid electrolyte, the role of the diaphragm is still to maintain the efficiency and stability of ion transmission.

[0003] As battery technology develops from liquid to solid and quasi-solid, the separator is also evolving. In all-solid-state batteries, the electrolyte becomes completely solid, and the traditional separator may no longer be needed. However, most current solid-state battery designs still use some form of separator or composite separator to play a critical role in physical isolation and electrochemical protection to ensure safe and efficient operation of the battery.

[0004] In terms of diaphragm coating slurry, diaphragm coating ceramics can improve its mechanical strength and extend its service life. However, in some application scenarios, such as high-energy-density solid-state batteries, although the mechanical strength of the ceramic coating is improved, it may break due to external stress during battery assembly or use, especially when the battery is impacted or pressurized. The insufficient adhesion between the ceramic coating and the diaphragm substrate will cause the coating to gradually fall off during use. In addition, hard ceramic particles in the coating can easily become stress concentration points, which will also cause the binder skeleton to be more easily destroyed when subjected to stress, affecting the long-term stability of the battery. Summary of the invention

[0005] In order to solve the problems existing in the background technology, the present invention provides a diaphragm coating slurry for solid-state batteries and a preparation method thereof, which can effectively improve the adhesion between the coating and the diaphragm substrate to avoid falling off; at the same time, improve the tensile strength to prevent the coating itself from being easily damaged, thereby enhancing the long-term stability of the battery.

[0006] In order to achieve the above-mentioned purpose, in a first aspect, the present invention provides a diaphragm coating slurry for solid-state batteries, which comprises the following raw material components, measured by mass percentage: 25-30% modified alumina, 4-4.5% carboxymethyl cellulose, 0.6-1% dispersant, 1.3-1.5% inorganic sol, 1.5-2% nanofiller, 0.5-0.8% interfacial compatibilizer and balance water; the modified alumina is prepared by acid-washing alumina and then surface-treating the surface with a silane coupling agent.

[0007] Furthermore, the preparation method of the modified alumina is as follows:

[0008] A1. Immerse the aluminum oxide in a 5-6% hydrofluoric acid aqueous solution, stir at 70-80r / min for 3-4 minutes at room temperature, then filter and wash with water until neutral to obtain roughened aluminum oxide;

[0009] A2. Immerse the roughened alumina obtained in A1 in a 10-11% silane coupling agent n-butanol solution, heat to 80-85°C, stir at 55-65r / min for 4-4.5h, then filter and dry to obtain modified alumina.

[0010] Furthermore, the silane coupling agent is γ-aminopropyltriethoxysilane.

[0011] Furthermore, the inorganic sol includes silica sol and / or aluminum sol.

[0012] Furthermore, the nanofiller includes any one of nanosilicate, carbon nanotube and graphene.

[0013] Furthermore, the nano-silicate includes any one of kaolin, anorthite, quartz, and tourmaline powder, or a mixture of at least two of them.

[0014] Furthermore, the dispersant is polyethylene glycol dioleate.

[0015] Furthermore, the interfacial compatibilizer is maleic anhydride grafted polyethylene.

[0016] In a second aspect, the present invention provides a method for preparing the above-mentioned solid-state battery separator coating slurry, comprising the following steps:

[0017] S1. dissolving carboxymethyl cellulose in water to obtain a colloidal solution;

[0018] S2, mixing the modified alumina and the nanofiller to obtain mixed particles;

[0019] S3. Put the colloidal solution obtained in S1 and the mixed particles obtained in S2 into a blender, and then add a dispersant, an inorganic sol and an interfacial compatibilizer, stir and mix well to obtain a diaphragm coating slurry for a solid-state battery.

[0020] Furthermore, in S3, the stirring speed is 1500-1700 r / min, and the stirring time is 50-60 min.

[0021] This application has the following beneficial effects:

[0022] The addition of carboxymethyl cellulose in the present invention can form a protective film on the surface of the material. When the dosage is appropriate, the film can maintain a certain porosity and prevent the loss of pores caused by excessive sealing. Carboxymethyl cellulose has good water retention capacity. When the dosage is increased, more hydrogels will be formed in the coating. These hydrogels gradually lose water during the drying process, leaving tiny pores, increasing the number of pores and the porosity. If the content of carboxymethyl cellulose is too high, the pores will be dense, and more dense connections will appear. The pore size will increase, the porosity will increase, but the number of pores will decrease, thereby affecting the peeling strength of the coating and the tensile strength of the prepared diaphragm.

[0023] The modified alumina coating has a more optimized pore structure, which makes it easier for silica sol and nano-silicate to enter and fill the pores. It has been verified by experiments that when the content of carboxymethyl cellulose is 4-4.5%, the alumina is modified by the present invention and silica sol and calcined kaolin (4000 mesh) are added, and the two work synergistically, and the adhesion of the coating and the tensile strength of the diaphragm are improved best.

[0024] The present invention can effectively improve the adhesion between the coating and the diaphragm substrate, with the measured peel strength reaching over 2.81 N / cm, effectively preventing it from falling off; at the same time, it can improve the tensile strength, with the measured tensile strength reaching over 50.2 MPa, effectively preventing the coating from being damaged by the force; the long-term stability of the battery is excellent. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 , a comparative trend chart of peel strength test data of ceramic diaphragm coatings obtained in Examples 1-6 of the present invention and Comparative Examples 1-11;

[0026] Figure 2 , a comparative trend chart of the tensile strength test data of the ceramic diaphragms prepared in Examples 1-6 of the present invention and Comparative Examples 1-11. DETAILED DESCRIPTION

[0027] The present application is further described in detail below with reference to the embodiments.

[0028] Unless otherwise specified, the raw materials used in the examples and comparative examples of the present application are all commercially available.

[0029] Example 1: (1) Preparation of modified alumina, the preparation method is as follows:

[0030] A1. Immerse the aluminum oxide in a 5.5% hydrofluoric acid aqueous solution, stir at 75r / min for 3.5min at room temperature, then filter and wash with water until neutral to obtain roughened aluminum oxide.

[0031] The alumina was calcined α-alumina, 260 mesh, purchased from Zibo Yishengjia Aluminum Co., Ltd. Hydrofluoric acid (first-grade product) was purchased from Shaanxi Lanxin Chemical Co., Ltd.

[0032] A2. Immerse the roughened alumina obtained in A1 into a 10.5% γ-aminopropyltriethoxysilane n-butanol solution, heat to 82°C, stir at 60 r / min for 4.2 h, then filter and dry to obtain modified alumina.

[0033] Among them, γ-aminopropyltriethoxysilane (KH550) was purchased from Shandong Hengyu New Materials Co., Ltd. n-Butanol was purchased from Jinan Century Tongda Chemical Co., Ltd.

[0034] (2) Preparing a solid-state battery separator coating slurry, the preparation method is as follows:

[0035] S1. According to the mass percentage, weigh the raw material components of modified alumina 28%, carboxymethyl cellulose 4.2%, dispersant 0.8%, inorganic sol 1.4%, nano filler 1.8%, interfacial compatibilizer 0.6% and water 63.2%.

[0036] The modified alumina is prepared by (1). Carboxymethyl cellulose was purchased from Hebei Shenghai Environmental Protection Technology Co., Ltd. The inorganic sol is silica sol, specifically chemical nano-grade acidic silica sol (30%), purchased from Guangzhou Changhao Chemical Co., Ltd. The nanofiller is nano-silicate, specifically calcined kaolin (4000 mesh), purchased from Changxing Innovation Ultrafine Powder Co., Ltd. The dispersant is polyethylene glycol dioleate (content 98%, density 10g / cm 3 ), purchased from Wuhan Kamik Technology Co., Ltd. The interfacial compatibilizer was maleic anhydride grafted polyethylene (grafting rate 0.8-1.0%), purchased from Shandong Shoucheng Chemical Co., Ltd.

[0037] S2, dissolving the carboxymethyl cellulose weighed in S1 in the water weighed in S1 to obtain a colloidal solution. Specifically, after the two are mixed, stirring at 150 r / min for 10 min.

[0038] S3, the modified alumina weighed in S1 and the nanofiller weighed in S1 are mixed to obtain mixed particles. Specifically, after the two are mixed, they are stirred at 100 r / min for 10 minutes.

[0039] S4. Put the colloidal solution obtained in S2 and the mixed particles obtained in S3 into a blender, and then add the dispersant, inorganic sol and interfacial compatibilizer weighed in S1, stir at a constant speed of 1600 r / min for 55 min, and mix well to obtain a diaphragm coating slurry for solid-state batteries.

[0040] (3) A ceramic diaphragm is prepared, and the preparation method is as follows: First, a PE film with a thickness of 12±2 μm and a brand of SK from South Korea is selected and purchased from Shenzhen Yuanchenghui Electronics Co., Ltd. Then, the solid-state battery diaphragm coating slurry prepared in (2) is coated on the PE film, and the water is dried in an oven at a temperature of 55-65°C to form a coating with a thickness of about 4 μm, thereby obtaining a ceramic diaphragm.

[0041] Example 2: The difference between this example and Example 1 is that: (1) modified alumina is prepared, and the preparation method is as follows:

[0042] A1. Immerse the alumina in a 5% hydrofluoric acid aqueous solution, stir at 70r / min for 3 minutes at room temperature, then filter and wash with water until neutral to obtain roughened alumina.

[0043] A2. Immerse the roughened alumina obtained in A1 into a 10% γ-aminopropyltriethoxysilane n-butanol solution, heat to 80°C, stir at 55 r / min for 4 hours, then filter and dry to obtain modified alumina.

[0044] Example 3: The difference between this example and Example 1 is that: (1) modified alumina is prepared, and the preparation method is as follows:

[0045] A1. Immerse the alumina in a 6% hydrofluoric acid aqueous solution, stir at 80r / min for 4 minutes at room temperature, then filter and wash with water until neutral to obtain roughened alumina.

[0046] A2. The roughened alumina obtained in A1 is immersed in a 11% γ-aminopropyltriethoxysilane n-butanol solution, heated to 85°C, stirred at 65 r / min for 4.5 h, then filtered and dried to obtain modified alumina.

[0047] Example 4: The difference between this example and Example 1 is that: (2) a diaphragm coating slurry for a solid-state battery is prepared, and the preparation method thereof is as follows:

[0048] S1. According to the mass percentage, weigh the raw material components of modified alumina 25%, carboxymethyl cellulose 4%, dispersant 0.6%, inorganic sol 1.3%, nano filler 1.5%, interfacial compatibilizer 0.5% and water 67.1%.

[0049] S2. Dissolve the carboxymethyl cellulose weighed in S1 in the water weighed in S1 to obtain a colloidal solution.

[0050] S3. Evenly mix the modified alumina weighed in S1 and the nanofiller weighed in S1 to obtain mixed particles.

[0051] S4. Put the colloidal solution obtained in S2 and the mixed particles obtained in S3 into a blender, and then add the dispersant, inorganic sol and interfacial compatibilizer weighed in S1, stir at a constant speed of 1500 r / min for 50 min, and mix well to obtain a diaphragm coating slurry for solid-state batteries.

[0052] Example 5: The difference between this example and Example 1 is that: (2) a diaphragm coating slurry for a solid-state battery is prepared, and the preparation method thereof is as follows:

[0053] S1. According to the mass percentage, weigh the raw material components of modified alumina 30%, carboxymethyl cellulose 4.5%, dispersant 1%, inorganic sol 1.5%, nano filler 2%, interfacial compatibilizer 0.8% and water 60.2%.

[0054] S2. Dissolve the carboxymethyl cellulose weighed in S1 in the water weighed in S1 to obtain a colloidal solution.

[0055] S3. Evenly mix the modified alumina weighed in S1 and the nanofiller weighed in S1 to obtain mixed particles.

[0056] S4. Put the colloidal solution obtained in S2 and the mixed particles obtained in S3 into a blender, and then add the dispersant, inorganic sol and interfacial compatibilizer weighed in S1, stir at a constant speed of 1700 r / min for 60 min, and mix well to obtain a diaphragm coating slurry for solid-state batteries.

[0057] Example 6: The difference between this example and Example 1 is that: (2) a diaphragm coating slurry for a solid-state battery is prepared, and the preparation method thereof is as follows:

[0058] S1. According to the mass percentage, weigh the raw material components: 30% modified alumina, 4% carboxymethyl cellulose, 1% dispersant, 1.5% inorganic sol, 2% nano filler, 0.8% interfacial compatibilizer and 60.7% water.

[0059] S2. Dissolve the carboxymethyl cellulose weighed in S1 in the water weighed in S1 to obtain a colloidal solution.

[0060] S3. Evenly mix the modified alumina weighed in S1 and the nanofiller weighed in S1 to obtain mixed particles.

[0061] S4. Put the colloidal solution obtained in S2 and the mixed particles obtained in S3 into a blender, and then add the dispersant, inorganic sol and interfacial compatibilizer weighed in S1, stir at a constant speed of 1600 r / min for 55 min, and mix well to obtain a diaphragm coating slurry for solid-state batteries.

[0062] Comparative Example 1: The difference between this comparative example and Example 1 is that: the modified alumina is replaced by alumina; the silica sol and calcined kaolin (4000 mesh) are deleted; and the mass percentage of carboxymethyl cellulose used is 2.5%.

[0063] Specifically, in the preparation of the diaphragm coating slurry for solid-state batteries: S1, weigh the raw material components of 28% aluminum oxide, 2.5% carboxymethyl cellulose, 0.8% dispersant, 0.6% interfacial compatibilizer and 68.1% water in percentage by mass.

[0064] Comparative Example 2: The difference between this comparative example and Example 1 is that the modified alumina is replaced by alumina; and the silica sol and calcined kaolin (4000 mesh) are deleted.

[0065] Specifically, in the preparation of the diaphragm coating slurry for solid-state batteries: S1, weigh the raw material components 28% aluminum oxide, 4.2% carboxymethyl cellulose, 0.8% dispersant, 0.6% interfacial compatibilizer and 66.4% water in percentage by mass.

[0066] Comparative Example 3: The difference between this comparative example and Example 1 is that: the modified alumina is replaced by alumina; the silica sol and calcined kaolin (4000 mesh) are deleted; and the mass percentage of carboxymethyl cellulose is 6%.

[0067] Specifically, in the preparation of the diaphragm coating slurry for solid-state batteries: S1. According to the mass percentage, weigh the raw material components of modified alumina 28%, carboxymethyl cellulose 6%, dispersant 0.8%, interfacial compatibilizer 0.6% and water 64.6%.

[0068] Comparative Example 4: This comparative example differs from Example 1 in that silica sol and calcined kaolin (4000 mesh) are deleted, and the mass percentage of carboxymethyl cellulose used is 2.5%.

[0069] Specifically, in the preparation of the diaphragm coating slurry for solid-state batteries: S1. According to the mass percentage, weigh the raw material components of modified alumina 28%, carboxymethyl cellulose 2.5%, dispersant 0.8%, interfacial compatibilizer 0.6% and water 68.1%.

[0070] Comparative Example 5: This comparative example differs from Example 1 in that silica sol and calcined kaolin (4000 mesh) are deleted.

[0071] Specifically, in the preparation of the diaphragm coating slurry for solid-state batteries: S1. According to the mass percentage, weigh the raw material components of modified alumina 28%, carboxymethyl cellulose 4.2%, dispersant 0.8%, interfacial compatibilizer 0.6% and water 66.4%.

[0072] Comparative Example 6: The difference between this comparative example and Example 1 is that silica sol and calcined kaolin (4000 mesh) are deleted; and the mass percentage of carboxymethyl cellulose is 6%.

[0073] Specifically, in the preparation of the diaphragm coating slurry for solid-state batteries: S1. According to the mass percentage, weigh the raw material components of modified alumina 28%, carboxymethyl cellulose 6%, dispersant 0.8%, interfacial compatibilizer 0.6% and water 64.6%.

[0074] Comparative Example 7: This comparative example differs from Example 1 in that the modified alumina is replaced by alumina; and the mass percentage of carboxymethyl cellulose used is 2.5%.

[0075] Specifically, in the preparation of the diaphragm coating slurry for solid-state batteries: S1, according to the mass percentage, weigh the raw material components of 28% aluminum oxide, 2.5% carboxymethyl cellulose, 0.8% dispersant, 1.4% silica sol, 1.8% calcined kaolin (4000 mesh), 0.6% interfacial compatibilizer and 64.9% water.

[0076] Comparative Example 8: The difference between this comparative example and Example 1 is that the modified alumina is replaced by alumina.

[0077] Specifically, in the preparation of the diaphragm coating slurry for solid-state batteries: S1, according to the mass percentage, weigh the raw material components of 28% aluminum oxide, 4.2% carboxymethyl cellulose, 0.8% dispersant, 1.4% silica sol, 1.8% calcined kaolin (4000 mesh), 0.6% interfacial compatibilizer and 63.2% water.

[0078] Comparative Example 9: The difference between this comparative example and Example 1 is that the modified alumina is replaced by alumina; and the mass percentage of carboxymethyl cellulose used is 6%.

[0079] Specifically, in the preparation of the diaphragm coating slurry for solid-state batteries: S1, according to the mass percentage, weigh the raw material components of 28% aluminum oxide, 6% carboxymethyl cellulose, 0.8% dispersant, 1.4% silica sol, 1.8% calcined kaolin (4000 mesh), 0.6% interfacial compatibilizer and 61.4% water.

[0080] Comparative Example 10: The difference between this comparative example and Example 1 is that the mass percentage of carboxymethyl cellulose used is 2.5%.

[0081] Specifically, in the preparation of the diaphragm coating slurry for solid-state batteries: S1, according to the mass percentage, weigh the raw material components of modified alumina 28%, carboxymethyl cellulose 2.5%, dispersant 0.8%, silica sol 1.4%, calcined kaolin (4000 mesh) 1.8%, interfacial compatibilizer 0.6% and water 64.9%.

[0082] Comparative Example 11: The difference between this comparative example and Example 1 is that the mass percentage of carboxymethyl cellulose used is 6%.

[0083] Specifically, in the preparation of the diaphragm coating slurry for solid-state batteries: S1. According to the mass percentage, weigh the raw material components of modified alumina 28%, carboxymethyl cellulose 6%, dispersant 0.8%, silica sol 1.4%, calcined kaolin (4000 mesh) 1.8%, interfacial compatibilizer 0.6% and water 61.4%.

[0084] Test example: Test object: Ceramic diaphragms were prepared according to Examples 1-6 and Comparative Examples 1-11.

[0085] Test items: ① Adhesion-peel strength of coating; ② Tensile strength of ceramic diaphragm.

[0086] Test basis: ① The peel strength is tested according to method 2 of the national standard GB / T 2792-2014 "Test method for peel strength of adhesive tape"; ② The tensile strength is tested according to the provisions of GB / T1040.3-2006, using a type 2 specimen with a width of 15 mm, an initial distance between the clamps of 100 mm, and a test speed of 250 mm / min.

[0087] Test results: See Table 1.

[0088] Table 1. Test data of the experimental example

[0089]

[0090] Result analysis: Analyze Examples 1-6 and Comparative Examples 1-11 and combine the data in Table 1 and Figure 1-2 It can be seen that the present invention can effectively improve the adhesion between the coating and the diaphragm substrate, with the measured peel strength reaching over 2.81 N / cm, effectively preventing it from falling off; at the same time, it can improve the tensile strength, with the measured tensile strength reaching over 50.2 MPa, effectively preventing the coating itself from being damaged by force; the long-term stability of the battery is excellent.

[0091] Analyze Comparative Examples 1-3 and combine the data in Table 1 and Figure 1-2 It can be seen that when alumina is not modified and the raw material components of the slurry do not contain silica sol and calcined kaolin (4000 mesh), the peel strength and tensile strength test data are all comparative example 1 (carboxymethyl cellulose 2.5%)> comparative example 2 (carboxymethyl cellulose 4.2%)> comparative example 3 (carboxymethyl cellulose 6%). This shows that when the content of carboxymethyl cellulose is low, the adhesion of the coating and the tensile strength of the diaphragm are greater. This is because when the content of carboxymethyl cellulose is low, the porosity of the coating is low and the bonding area between the coating and the substrate is larger.

[0092] Analyze Comparative Examples 1-3 and Comparative Examples 4-6 and combine the data in Table 1 and Figure 1-2 It can be seen that, compared with Comparative Examples 1-3, after the aluminum oxide is modified by the present invention, the peel strength and tensile strength test data are all Comparative Example 4 (carboxymethyl cellulose 2.5%)>Comparative Example 5 (carboxymethyl cellulose 4.2%)>Comparative Example 6 (carboxymethyl cellulose 6%). This shows that when the aluminum oxide is modified by the present invention, the effect is better when the carboxymethyl cellulose content is lower (2.5%).

[0093] In addition, in terms of peel strength, Comparative Example 4>Comparative Example 1, an increase of 0.43N / cm; Comparative Example 5>Comparative Example 2, an increase of 0.34N / cm; Comparative Example 6>Comparative Example 3, an increase of 0.26N / cm; in terms of tensile strength, Comparative Example 4>Comparative Example 1, an increase of 6MPa; Comparative Example 5>Comparative Example 2, an increase of 4.7MPa; Comparative Example 6>Comparative Example 3, an increase of 3.7MPa. It can be seen that after the aluminum oxide is modified by the present invention, the increase in the effect of 2.5% on carboxymethyl cellulose is greater than the increase in the effect of 4.2% on carboxymethyl cellulose, and the increase in the effect of 6% on carboxymethyl cellulose. This shows that when the content of carboxymethyl cellulose is low (2.5%), the modification of the aluminum oxide by the present invention is more conducive to improving the adhesion of the coating and the tensile strength of the diaphragm.

[0094] Analyze Comparative Examples 1-3 and Comparative Examples 7-9 and combine the data in Table 1 and Figure 1-2 It can be seen that compared with Comparative Examples 1-3, after adding silica sol and calcined kaolin (4000 mesh), the peel strength and tensile strength test data are all Comparative Example 7 (carboxymethyl cellulose 2.5%)> Comparative Example 8 (carboxymethyl cellulose 4.2%)> Comparative Example 9 (carboxymethyl cellulose 6%). This shows that adding silica sol and calcined kaolin (4000 mesh) with a lower carboxymethyl cellulose content (2.5%) has a better effect.

[0095] Analyze Comparative Examples 1-3 and Example 1, Comparative Examples 10-11 and combine the data in Table 1 and Figure 1-2 It can be seen that compared with Comparative Examples 1-3, after the aluminum oxide is modified by the present invention and silica sol and calcined kaolin (4000 mesh) are added, the two are synergistically effective, and the peel strength and tensile strength test data are all Example 1 (carboxymethyl cellulose 4.2%)> Comparative Example 10 (carboxymethyl cellulose 2.5%)> Comparative Example 11 (carboxymethyl cellulose 6%). This shows that the aluminum oxide is modified by the present invention, and silica sol and calcined kaolin (4000 mesh) are added, and the effect is best when the carboxymethyl cellulose content is 4.2%.

[0096] In addition, in terms of peel strength, Example 1>Comparative Example 2, an increase of 0.79N / cm; Comparative Example 10>Comparative Example 1, an increase of 0.50N / cm; Comparative Example 11>Comparative Example 3, an increase of 0.66N / cm; in terms of tensile strength, Example 1>Comparative Example 2, an increase of 10.9MPa; Comparative Example 10>Comparative Example 1, an increase of 7.1MPa; Comparative Example 11>Comparative Example 3, an increase of 6.8MPa. It can be seen that the alumina is modified by the present invention, and silica sol and calcined kaolin (4000 mesh) are added. In terms of peel strength, the increase in the effect of 4.2% carboxymethyl cellulose> the increase in the effect of 6% carboxymethyl cellulose> the increase in the effect of 2.5% carboxymethyl cellulose. In terms of tensile strength, the increase in the effect of 4.2% carboxymethyl cellulose> the increase in the effect of 2.5% carboxymethyl cellulose> the increase in the effect of 6% carboxymethyl cellulose. It shows that when the content of carboxymethyl cellulose is 4.2%, the aluminum oxide is modified by the present invention and silica sol and calcined kaolin (4000 mesh) are added, and the two work synergistically to achieve the best effect on improving the adhesion of the coating and the tensile strength of the diaphragm.

[0097] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.

[0098] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.

Claims

1. A solid-state battery separator coating slurry, characterized in that: The raw material components include, by mass percentage, 25-30% of modified alumina, 4-4.5% of carboxymethyl cellulose, 0.6-1% of dispersant, 1.3-1.5% of inorganic sol, 1.5-2% of nano filler, 0.5-0.8% of interfacial compatibilizer and the remainder of water; the modified alumina is prepared by acid-washing alumina and then surface-treating it with a silane coupling agent.

2. The solid-state battery separator coating slurry according to claim 1, characterized in that: The preparation method of the modified alumina is as follows: A1. Immerse the aluminum oxide in a 5-6% hydrofluoric acid aqueous solution, stir at 70-80r / min for 3-4 minutes at room temperature, then filter and wash with water until neutral to obtain roughened aluminum oxide; A2. Immerse the roughened alumina obtained in A1 in a 10-11% silane coupling agent n-butanol solution, heat to 80-85°C, stir at 55-65r / min for 4-4.5h, then filter and dry to obtain modified alumina.

3. The solid-state battery separator coating slurry according to claim 2, characterized in that: The silane coupling agent is γ-aminopropyltriethoxysilane.

4. The solid-state battery separator coating slurry according to claim 1, characterized in that: The inorganic sol includes silica sol and / or aluminum sol.

5. The solid-state battery separator coating slurry according to claim 1, characterized in that: The nano filler includes any one of nano silicate, carbon nano tube and graphene.

6. The solid-state battery separator coating slurry according to claim 5, characterized in that: The nano silicate includes any one of kaolin, calcium feldspar, quartz and tourmaline powder or a mixture of at least two of them.

7. The solid-state battery separator coating slurry according to claim 1, characterized in that: The dispersant is polyethylene glycol dioleate.

8. The solid-state battery separator coating slurry according to claim 1, characterized in that: The interfacial compatibilizer is maleic anhydride grafted polyethylene.

9. A method for preparing a solid-state battery separator coating slurry according to any one of claims 1 to 8, characterized in that: The steps include: S1. dissolving carboxymethyl cellulose in water to obtain a colloidal solution; S2, mixing the modified alumina and the nanofiller to obtain mixed particles; S3. Put the colloidal solution obtained in S1 and the mixed particles obtained in S2 into a blender, and then add a dispersant, an inorganic sol and an interfacial compatibilizer, stir and mix well to obtain a diaphragm coating slurry for a solid-state battery. The method for preparing a diaphragm coating slurry for a solid-state battery according to claim 9, characterized in that: In S3, the stirring speed is 1500-1700 r / min, and the stirring time is 50-60 min.

Citation Information

Patent Citations

  • Novel lithium ion battery diaphragm with inorganic coating and preparation method thereof

    CN103107301A

  • High-temperature resistant lithium battery separator and preparation method thereof

    CN107492620A

  • Composite polypropylene microporous membrane and preparation method thereof and lithium ion battery separator including composite polypropylene microporous membrane

    CN110343278A

  • Method for preparing composite polypropylene microporous membrane through interfacial polymerization method, and products and application of composite polypropylene microporous membrane

    CN110343279A

  • Preparation method of modified aluminum oxide and PMMA mixed slurry coated diaphragm

    CN114050375A

Cited By

  • Linear light lithium battery diaphragm and preparation method thereof

    CN119447703A