Magnetic tunnel junction fixing layer, magnetic storage chip, magnetic sensing chip and manufacturing method of magnetic tunnel junction fixing layer

By adopting a combined structure of multi-layer ferromagnetic and antiferromagnetic materials in the magnetic tunnel junction, the problem of growth of double fixed layer structure is solved, the writing efficiency and durability of magnetic storage and magnetic sensing chips are improved, and information writing is reduced Energy consumption.

CN119012898APending Publication Date: 2024-11-22YANGTZE DEITA GRADUATE SCHOOI OF BEIJING INST OF TECH (JIAXING) +1

Patent Information

Application Number
CN202411082287.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The prior art is difficult to grow high-quality double-fixed layer structures, especially the upper fixed layer, in magnetic tunnel junctions, resulting in high write electrical energy, large information writing energy and poor durability of magnetic memory chips and magnetic sensing chips. question.

Method used

The combination structure is adopted, such as the ferromagnetic fixed layer structure, the antiparallel coupled ferromagnetic fixed layer structure, the antiparallel coupled ferromagnetic fixed layer structure containing antiferromagnetic magnets, and the combination of the oxide coupling layer and the ferromagnetic thin film structure, A fixed layer with high coercive force is formed and a ferromagnetic material with high spin polarization such as iron and boron alloy is used to reduce the exchange coupling magnetic field to the free layer.

Benefits of technology

The high coercive force and low exchange coupled magnetic field of the fixed layer are realized, which reduces the energy consumption of information writing, improves the durability of the magnetic tunnel junction, and makes the manufacturing process of the double fixed layer MTJ feasible.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119012898A_ABST
    Figure CN119012898A_ABST
Patent Text Reader

Abstract

The invention relates to a fixing layer of a core device magnetic tunnel junction applied to a magnetic storage chip and a magnetic sensing chip in an integrated circuit and a manufacturing method of the fixing layer. Generally, a magnetic tunnel junction uses a Co / Pt alternating multilayer thin film structure as a fixed layer of the magnetic tunnel junction, but the Co / Pt alternating multilayer thin film structure requires a substrate structure to have crystals matched with the substrate structure. In order to prepare a matched substrate, a fixed layer of a traditional magnetic tunnel junction is usually closer to a substrate than a free layer, and a double-fixed-layer junction magnetic tunnel junction needs to prepare a fixed layer above the free layer. According to the invention, the structure and process design of the fixed layer is carried out by utilizing the fact that a ferromagnetic film structure body is clamped by two ends of the MgO film to generate great magnetic anisotropy. The invention provides a fixed layer structure above a free layer of a magnetic tunnel junction and a manufacturing process thereof, wherein the fixed layer structure has larger coercive force and generates smaller exchange coupling to the free layer and can be used for the free layer of the magnetic tunnel junction.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of magnetic storage chips and magnetic sensor chips in integrated circuits, and in particular to a fixed layer of a magnetic tunnel junction, a core device used in both magnetic storage chips and magnetic sensor chips, a corresponding chip, and a manufacturing method thereof. Background Art

[0002] The magnetic tunnel junction (MTJ) consists of two ferromagnetic thin film structures (the so-called structure refers to a multilayer thin film) sandwiched by a tunneling layer insulator oxide (usually MgO). The spin direction (also called magnetization direction) of a ferromagnetic thin film structure (fixed layer) of the MTJ is fixed, and the spin direction of another ferromagnetic thin film (free layer) is changed. The two ferromagnetic thin film structures have different resistances in the parallel and anti-parallel states of the spin directions. Therefore, it can be used in magnetic storage chips (MRAM, also known as magnetic random access memory or random read memory) and magnetic sensor chips (such as magnetic sensors such as hard disk heads).

[0003] An important issue of MRAM based on spin transfer torque (STT) MTJ is that the write electric energy of MTJ device is high, which damages the insulator of tunnel layer. STT is to write information by changing the magnetization spin direction of free layer through the magnetic moment generated by spin polarization of transmitted current in fixed layer. The greater the difference between the number of spins facing up and down when the current is spin polarized in fixed layer, the smaller the write current from one state to another (for example, from parallel to antiparallel), while the write current from the opposite state (corresponding to from antiparallel to parallel) will be. And vice versa. Therefore, the STT-MTJ structure with double fixed layer structure (Chinese patent: 202410613679.5) was proposed.

[0004] The fixed layer that can be used in practice so far is a face-centered (fcc) Pt metal grown on a substrate with a (111) plane, and a multilayer film of alternating Co metal and Pt metal grown on the fcc (111) plane with the highest atomic density to serve as the fixed layer. The easy axis of magnetization of Co metal is perpendicular to the plane with the highest atomic density of its crystal, thus producing strong perpendicular magnetic anisotropy, so the Co / Pt alternating multilayer film structure is usually used as the fixed layer of the MTJ. However, before the growth of the above structure, the (111) plane of the face-centered Pt metal needs to be deposited on the substrate. For a double fixed layer structure, especially the upper fixed layer in a double fixed layer magnetic tunnel junction, that is, the fixed layer farther from the substrate, the fixed layer of the above Co / Pt alternating multilayer film structure is difficult to grow, so it is difficult to obtain a high-quality structure and the corresponding perpendicular magnetic anisotropy.

[0005] In addition to STT-MTJ, MTJ based on spin-orbit moment (SOT) writing and MTJ based on voltage-controlled magnetic anisotropy (VCMA) writing will also face the same problem if the fixed layer is not grown on the substrate (or when it grows freely). In addition, magnetic sensor chips including magnetic heads also face the same problem. Summary of the invention

[0006] In view of the above background and problems, the present invention provides a new structure of the MTJ fixed layer and its preparation method. The present invention uses the ferromagnetic thin film structure clamped at both ends of the MgO film to produce a large magnetic anisotropy. The design of the fixed layer above the free layer (that is, farther from the substrate than the free layer) is the main starting point of the present invention. The fixed layer of the present invention has a larger coercive force (H) than the free layer. c ), but it will generate an exchange coupling magnetic field on the free layer. In order to make the fixed layer have a larger coercive force and a smaller exchange coupling magnetic field on the free layer, a combination of four structures, namely, a ferromagnetic fixed layer structure (FP), an antiparallel coupled ferromagnetic fixed layer structure (APP), an antiparallel coupled ferromagnetic fixed layer containing antiferromagnets (AFFP), and an antiparallel coupled ferromagnetic fixed layer structure containing antiferromagnets (AFAPP), is used to form the final upper fixed layer. The specific structure is as follows:

[0007] FP: oxide coupling layer / ferromagnetic thin film structure / oxide coupling layer;

[0008] AFFP: oxide coupling layer / ferromagnetic thin film structure / antiferromagnetic thin film structure;

[0009] APP: oxide coupling layer / ferromagnetic thin film structure / antiparallel coupling layer / ferromagnetic thin film structure / oxide coupling layer;

[0010] AFAPP: oxide coupling layer / ferromagnetic thin film structure / antiparallel coupling layer / ferromagnetic thin film structure / antiferromagnetic thin film structure.

[0011] The results show that the fixed layer prepared by this method has a high coercive force, which can be achieved by adjusting and reducing the exchange coupling magnetic field to the free layer, and by selecting ferromagnetic materials with large spin polarization rate, such as iron-boron alloys. The details are as follows:

[0012] The present invention provides a magnetic tunnel junction for a magnetic storage chip and a magnetic sensor chip, and its characteristic structure is:

[0013] The device is composed of a ferromagnetic thin film structure serving as a free layer, a magnesium oxide thin film serving as a tunneling layer, and a ferromagnetic thin film structure serving as a fixed layer in order from near to far from the substrate;

[0014] The fixed layer ferromagnetic film structure is composed of an oxide coupling layer, a ferromagnetic film structure, and a ferromagnetic fixed layer structure composed of an oxide coupling layer, and an antiparallel coupling ferromagnetic fixed layer structure composed of an oxide coupling layer, a ferromagnetic film structure, an antiparallel coupling layer, a ferromagnetic film structure, and an oxide coupling layer, from near to far from the substrate. The two structures contain at least one and any one of the structures contains at least one structure.

[0015] A supplementary explanation of the above content: The starting point of the present invention is to solve the preparation method of the upper fixed layer of the double-fixed layer MTJ. The lower fixed layer is ignored here because for some single-fixed layer MTJs, such as MTJs based on the SOT writing method, the fixed layer is originally above the free layer. Note that the distance from the substrate mentioned in the present invention is from near to far. The substrate is usually regarded as the bottom, and then the thin film is grown layer by layer. Therefore, the later the growth order, the farther the distance from the substrate. A ferromagnetic thin film structure refers to a structure composed of one or more thin films containing at least one layer of ferromagnetism. The structure refers to a structure composed of one or more thin films. The coupling layer can also be a one-layer or multi-layer thin film structure.

[0016] It should be noted that when any one of the two structures of the ferromagnetic pinned layer structure (FP) and the antiparallel coupling ferromagnetic pinned layer structure (APP) or a single or multiple structures of the two structures are combined, the adjacent parts such as the oxide coupling layer can be shared. The MgO of the tunneling layer can also be shared.

[0017] On the basis of the magnetic tunnel junction device structure for magnetic storage chips and magnetic sensor chips with the above characteristics, its structural features are further defined as: its structural features are: the fixed layer is increased at the end farthest from the substrate by a ferromagnetic fixed layer structure containing an antiferromagnet composed of an oxide coupling layer, a ferromagnetic thin film structure, and an antiferromagnetic thin film structure from near to far away from the substrate, and any one of the structures of an antiparallel coupled ferromagnetic fixed layer structure containing an antiferromagnet composed of an oxide coupling layer, a ferromagnetic thin film structure, an antiparallel coupling layer, a ferromagnetic thin film structure, and an antiferromagnetic thin film structure from near to far away from the substrate.

[0018] To supplement the above content: the ferromagnetic fixed layer structure containing antiferromagnets (AFFP) and the antiparallel coupled ferromagnetic fixed layer structure containing antiferromagnets (AFAPP) can only be used as the layer structure farthest from the substrate in the fixed layer. When they are combined with the aforementioned ferromagnetic fixed layer structure or antiparallel coupled ferromagnetic fixed layer structure, the adjacent parts such as the oxide coupling layer can be shared. In addition, when adjacent to the free layer, the tunneling layer magnesium oxide can be shared as the oxide coupling layer.

[0019] Based on the above-mentioned magnetic tunnel junction device structure for magnetic storage chips and magnetic sensor chips, the characteristic structures of the following seven devices are further defined, namely:

[0020] (1.1) From near to far away from the substrate, it is composed of a ferromagnetic film structure acting as a free layer, a magnesium oxide film acting as a tunneling layer, and a ferromagnetic film structure acting as a fixed layer; and the fixed layer is composed of a first ferromagnetic film structure, an antiparallel coupling layer, a second ferromagnetic film structure, a first oxide coupling layer, a third ferromagnetic film structure, and a magnesium oxide film.

[0021] (1.2) From near to far away from the substrate, it is composed of a ferromagnetic film structure acting as a free layer, a magnesium oxide film acting as a tunneling layer, and a ferromagnetic film structure acting as a fixed layer; and the fixed layer is composed of a first ferromagnetic film structure, an antiparallel coupling layer, a second ferromagnetic film structure, a first oxide coupling layer, a third ferromagnetic film structure, a second oxide coupling layer, a fourth ferromagnetic film structure, and a magnesium oxide film.

[0022] (1.3) From near to far away from the substrate, it is composed of a ferromagnetic thin film structure acting as a free layer, a magnesium oxide thin film acting as a tunneling layer, and a ferromagnetic thin film structure acting as a fixed layer; and the fixed layer is composed of a first ferromagnetic thin film structure, a first oxide coupling layer, a second ferromagnetic thin film structure, an antiparallel coupling layer, a third ferromagnetic thin film structure, a second oxide coupling layer, a fourth ferromagnetic thin film structure, and a magnesium oxide thin film.

[0023] (1.4) From near to far away from the substrate, it is composed of a ferromagnetic thin film structure acting as a free layer, a magnesium oxide thin film acting as a tunneling layer, and a ferromagnetic thin film structure acting as a fixed layer; and the fixed layer is composed of a first ferromagnetic thin film structure, a first oxide coupling layer, a second ferromagnetic thin film structure, an antiparallel coupling layer, a third ferromagnetic thin film structure, a second oxide coupling layer, a fourth ferromagnetic thin film structure, a third oxide coupling layer, a fifth ferromagnetic thin film structure, and a magnesium oxide thin film.

[0024] (1.5) From near to far away from the substrate, it is composed of a ferromagnetic thin film structure acting as a free layer, a magnesium oxide thin film acting as a tunneling layer, and a ferromagnetic thin film structure acting as a fixed layer; and the fixed layer is composed of a first ferromagnetic thin film structure, a first antiparallel coupling layer, a second ferromagnetic thin film structure, a first oxide coupling layer, a third ferromagnetic thin film structure, a second antiparallel coupling layer, a fourth ferromagnetic thin film structure, and a magnesium oxide thin film.

[0025] (1.6) From near to far away from the substrate, it is composed of a ferromagnetic thin film structure acting as a free layer, a magnesium oxide film acting as a tunneling layer, and a ferromagnetic thin film structure acting as a fixed layer; and the fixed layer is composed of a first ferromagnetic thin film structure, a first antiparallel coupling layer, a second ferromagnetic thin film structure, a first oxide coupling layer, a third ferromagnetic thin film structure, a second antiparallel coupling layer, a fourth ferromagnetic thin film structure, and an antiferromagnetic thin film structure.

[0026] (1.7) From near to far away from the substrate, it is composed of a ferromagnetic thin film structure acting as a free layer, a magnesium oxide film acting as a tunneling layer, and a ferromagnetic thin film structure acting as a fixed layer; and the fixed layer is composed of a first ferromagnetic thin film structure, a first oxide coupling layer, a second ferromagnetic thin film structure, an antiparallel coupling layer, a third ferromagnetic thin film structure, a second oxide coupling layer, a fourth ferromagnetic thin film structure, and an antiferromagnetic thin film structure.

[0027] To supplement the above content: the experimental and simulation results of the magnetic coercivity of the upper fixed layer of the magnetic tunnel junction devices containing the above 7 structures and the coupling magnetic field to the free layer show that they can be used in magnetic tunnel junctions and are expected to reduce the energy consumption of information writing in magnetic tunnel junctions, while improving the durability of magnetic tunnel junctions, and the manufacturing process is feasible.

[0028] On the basis of the above-mentioned magnetic tunnel junction device structure for magnetic storage chips and magnetic sensor chips, the characteristic structure of its fixed layer is further defined as follows: the antiferromagnetic film structure contains at least one antiferromagnetic material of manganese-platinum alloy or manganese-iridium alloy; the ferromagnetic film structure is mainly an alloy containing iron and boron; the antiparallel coupling layer material is usually made of either metal ruthenium or metal iridium; the oxide coupling layer is composed of any one of the following three: magnesium oxide containing any one of iron and cobalt elements plus boron and thicker than the tunneling layer magnesium oxide, iron oxide, and oxide containing iron and cobalt.

[0029] To supplement the above content: the antiferromagnetic film structure contains at least one of the antiferromagnetic materials, manganese-platinum alloy or manganese-iridium alloy, or both alloys; the antiferromagnetic film structure formed by some other non-magnetic films and manganese-platinum alloy or manganese-iridium alloy can also be used for the antiferromagnetic film structure. Current experiments and simulations show that the main method is to add ferromagnetic materials iron, cobalt and boron to magnesium oxide to form an oxide coupling layer, but iron oxide and iron-cobalt oxide or their combination may also achieve good parallel coupling ability, even if the spin directions of the ferromagnetic film structures at both ends are parallel.

[0030] The manufacturing method of the magnetic storage chip and the magnetic sensor chip having all the above structural features is defined to contain the following characteristic steps:

[0031] (2.1) Preparing peripheral circuits of magnetic storage chips and magnetic sensor chips on a substrate;

[0032] (2.2) Preparing the portion below the free layer of the magnetic tunnel junction on the metal connection layer of the peripheral circuit;

[0033] (2.3) preparing a ferromagnetic thin film structure serving as a free layer;

[0034] (2.4) preparing a tunneling layer magnesium oxide film;

[0035] (2.5) preparing the fixed layer;

[0036] (2.6) Patterning the thin film to form devices of magnetic storage chips and magnetic sensor chips;

[0037] (2.7) Connect and package the devices to form a chip.

[0038] To supplement the above content: the part below the free layer in (2.2) above corresponds to the magnetic transmission moment magnetic tunnel junction of the double fixed layer structure, mainly referring to the lower fixed layer. For the magnetic orbit moment magnetic tunnel junction, the part below the free layer refers to the spin Hall orbit that generates spin polarization.

[0039] The effect of the present invention is that it can realize the growth of a fixed layer on the MTJ free layer which cannot be realized by conventional technology; the grown fixed layer has a large coercive force and reduces the exchange coupling magnetic field generated on the free layer. The present invention can realize a double fixed layer MTJ with fixed layers at both ends of the free layer, so both the fixed layer and the free layer can use ferromagnetic materials with high spin polarization rate. As a result, the current of the free layer can be reduced when the spin direction of the free layer relative to the lower fixed layer is parallel to antiparallel or antiparallel to parallel, and the durability of the tunneling layer MgO is increased while reducing the energy consumption of information writing.

[0040] In addition, the structure of the present invention can also be used for MTJ based on SOT writing method or SOT and STT mixed writing method, and magnetic sensor including hard disk head based on MTJ. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] Figure 1 This is one of the embodiments of the present invention, and is the basic structure of the MTJ device of the present invention, in which the fixed layer (Pin) is on the top of the free layer. The antiparallel coupled ferromagnetic fixed layer structure (APP) is close to the free layer (FL), and the ferromagnetic fixed layer structure (FP) adjacent to the top thereof constitutes the fixed layer Pin on the top of the free layer.

[0042] Figure 2This is one of the embodiments of the present invention, and is the basic structure of the MTJ device with the fixed layer on the top of the free layer of the present invention, wherein the APP is close to the free layer FL, and the two FPs adjacent to the top of the APP constitute the fixed layer Pin on the top of the free layer.

[0043] Figure 3 This is one of the embodiments of the present invention, and is the basic structure of the MTJ device with the fixed layer on the free layer of the present invention, wherein the FP is close to the free layer FL, and the APP adjacent to the upper part thereof and the FP above it constitute the fixed layer Pin on the free layer.

[0044] Figure 4 This is one of the embodiments of the present invention, and is the basic structure of the MTJ device in which the fixed layer is on the free layer. Figure 4 is Figure 3 An additional FP is added on the top of the free layer to form a fixed layer Pin on the top of the free layer.

[0045] Figure 5 This is one of the embodiments of the present invention, and is the basic structure of the MTJ device with the fixed layer on the top of the free layer, wherein the APP is close to the free layer, and another APP adjacent to the top of the APP constitutes the fixed layer Pin on the top of the free layer.

[0046] Figure 6 This is one of the embodiments of the present invention, and is the basic structure of the MTJ device with the fixed layer on the free layer of the present invention, wherein the APP is close to the free layer, and the antiparallel coupled ferromagnetic fixed layer (AFAPP) containing antiferromagnets adjacent to the APP on the free layer constitutes the fixed layer Pin on the free layer.

[0047] Figure 7 One of the embodiments of the present invention is a fixed layer of five structures (a, b, c, d, e) composed of a combination of FP and AFP, wherein the upward and downward arrows represent the direction of spin or magnetization.

[0048] Figure 8 (A) Yes Figure 7 The coercivity of the films prepared by the five combinations in a certain way; Figure 8 (B) is a schematic diagram of the structure after the fixed layer is prepared on the free layer according to five methods and a schematic diagram of the hysteresis loop of the exchange coupling generated by the fixed layer to the free layer; Figure 8 (C) is a graph showing the relationship between the exchange coupling magnetic field and the device diameter for the five structures measured.

[0049] Fig. 9 One of the embodiments of the present invention is a fixed layer of four structures (f, g, h, i) composed of FP, AFFP and APP, wherein the upward and downward arrows represent the direction of spin or magnetization.

[0050] Fig.10 (A) Yes Fig. 9 The coercivity of the films prepared by the four combinations in a certain way; Fig.10 (B) is a graph showing the relationship between the exchange coupling magnetic field and the device diameter in the four structures measured.

[0051] Fig.11 One of the embodiments of the present invention is Figure 3 The difference is that the FP on the top is replaced by an antiparallel coupled ferromagnetic pinned layer (AFFP) containing an antiferromagnet.

[0052] Explanation of symbols:

[0053] 1: Free layer ferromagnetic thin film structure;

[0054] 2: Tunneling layer MgO film;

[0055] 1X (X=1, 2, 3, 4...): ferromagnetic thin film structure, a component of FP or AFFP;

[0056] 2X (X=1, 2, 3, 4...): ferromagnetic thin film structure, which is a component of APP or AFAPP;

[0057] 3X (X=1, 2, 3, 4…): antiparallel coupling layer, partially represented as APC;

[0058] 4X (X=1, 2, 3, 4…): oxide coupling layer, some figures show Oxide or Mid Oxide;

[0059] 5: magnesium oxide film layer;

[0060] 6: Antiferromagnetic magnetic thin film structure. DETAILED DESCRIPTION

[0061] The present invention will be described below with reference to the accompanying drawings and by way of examples of implementation.

[0062] Embodiment 1:

[0063] Figures 1 to 6 The six types of structural devices are composed of four structures: ferromagnetic fixed layer structure (FP), antiparallel coupled ferromagnetic fixed layer structure (APP), ferromagnetic fixed layer structure containing antiferromagnets (AFFP), and antiparallel coupled ferromagnetic fixed layer structure containing antiferromagnets (AFAPP). When combined, any two structures are connected through a common oxide coupling layer, and a tunneling layer can also be used.

[0064] Embodiment 2:

[0065] Figure 7Five structures of fixed layers (a), (b), (c), (d), and (e) are proposed. Among them, (a) and (b) are basic structures. (a) is a ferromagnetic thin film structure sandwiched between two oxide coupling layers (usually MgO), which is called a ferromagnetic fixed layer structure (FP). (b) is a ferromagnetic thin film structure sandwiched between two oxide coupling layers (usually MgO). The antiparallel coupling layer (APC) is usually implemented by a metal thin film layer such as ruthenium or iridium with a thickness of about 0.1 to 1.5 nanometers, which is called an antiparallel coupling ferromagnetic fixed layer structure (APP). Among them, the ferromagnetic thin film structure used for FP is usually an alloy of iron and boron, an alloy of iron, cobalt, and boron, and the above alloys doped with molybdenum and tungsten, with a total thickness of about 1 to 4 nanometers. The ferromagnetic thin film structure used for APP is usually an alloy of iron and boron, an alloy of iron, cobalt, and boron, and the above alloys doped with molybdenum and tungsten, with a thickness of about 0.5 to 4 nanometers. The antiparallel coupling layer makes the spins of the two ferromagnetic thin film structures of APP arranged in antiparallel.

[0066] Generally, the coercivity of the free layer of an MTJ device is about 1000 Oe to 2000 Oe, while the coercivity of the pinned layer is preferably above 4000 Oe. Figure 8 (A) Figure 7 The coercivity values ​​of the fixed layers of the five MTJ devices with a diameter of 30 nanometers show that the coercivity of the single FP (a) and the single APP (b) are less than 3000Oe, which are not suitable for the fixed layer. However, the coercivity of the fixed layers of the three structures (c) two FPs, (d) APP and FP, and (e) APP and two FPs above it are all greater than 4000Oe when the device diameter is 30 nanometers, and can be used as fixed layers.

[0067] Another important characteristic of the fixed layer is that Figure 8 (B) shows the coupling magnetic field (H) generated by the fixed layer on the free layer bias ). Figure 8 (C) Yes Figure 7 The relationship between the coupling magnetic field generated by the five fixed layer structures on the free layer and the diameter of the magnetic tunnel junction. It is found that the coupling magnetic field of the fixed layer on the free layer increases for all devices as the diameter decreases. For the three structures (c), (d), and (e) where the coercivity satisfies the fixed layer, the H of (c) when the device diameter is 20 nanometers bias The coercivity of the free layer (c) is 2000Oe, which is greater than the coercivity of the free layer (c). The free layer cannot record the two states of "0" and "1", so (c) cannot be used as a fixed layer. (d) and (e) H of (c) when the device diameter is 20 nanometers bias They are negative 59 Oe and negative 401 Oe respectively, which are smaller than the coercivity of the free layer and can be easily adjusted to 0. Both structures (d) and (e) can be used as fixed layers.

[0068] Embodiment 3:

[0069] Fig. 9 It represents other combination structures of FP and APP. (f) is a structure in which APP is formed on FP, and then FP is formed on top of it. (g) is a structure in which APP is formed on FP, and then two FPs are formed on top of it. (h) is a structure in which two APPs are superimposed. (i) is a structure in which an antiparallel coupled ferromagnetic fixed layer structure (AFAPP) containing an antiferromagnet is superimposed on APP. As mentioned above, AFAPP is actually a structure in which the oxide coupling layer on the upper layer of APP is replaced with an antiferromagnetic thin film structure. An antiferromagnetic thin film structure containing MnPt alloy or MnIr alloy is usually used as the antiferromagnetic thin film structure of AFAPP. Figure 7 same, Fig. 9 The internal oxide coupling layer in the structure uses a Mid Oxide structure, which is used to make the spin directions of the ferromagnetic thin film structures at both ends parallel, thereby integrating the multi-layer ferromagnetic thin film structure and increasing the coercive force.

[0070] Fig.10 (A) is the coercive force of the four fixed layers (f) to (i) when the diameter is 30 nanometers. The numbers are all greater than 4000 Oe, which means that they can all be used as fixed layers in terms of coercive force. Fig.10 (B) is a graph showing the relationship between the coupling magnetic field generated by the four fixed layer structures on the free layer and the diameter of the magnetic tunnel junction. Figure 8 (C) As the diameter of all devices decreases, the coupling magnetic field between the fixed layer and the free layer increases. bias They are (f) 780Oe, (g) 590Oe, (h) 200Oe, and (i) 200Oe, respectively. They are smaller than the coercive force of the free layer and can be easily adjusted to 0, so the four structures from (f) to (i) can all be used as fixed layers. The (i) structure actually replaces the oxide coupling layer with the antiferromagnetic film MnPt on the top layer of (h). The use of MnPt can more stably form the upward and downward alternating magnetization in the structures (i) and (h), thereby improving the performance of the device. For the same reason, the (f) structure uses an antiferromagnetic film structure on the top, that is, forming an antiparallel coupled ferromagnetic fixed layer (AFFP) containing an antiferromagnet, that is Fig.11 structure.

[0071] All the above embodiments only express certain implementation methods of the present invention, and the description is relatively specific, but it cannot be understood as limiting the scope of the invention patent. It should be pointed out that for ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be based on the attached claims.

Claims

1. A magnetic tunnel junction for a magnetic storage chip and a magnetic sensor chip, wherein the characteristic structure is: The device is composed of a ferromagnetic thin film structure serving as a free layer, a magnesium oxide thin film serving as a tunneling layer, and a ferromagnetic thin film structure serving as a fixed layer in order from near to far from the substrate; The fixed layer ferromagnetic film structure is composed of an oxide coupling layer, a ferromagnetic film structure, and a ferromagnetic fixed layer structure composed of an oxide coupling layer, and an antiparallel coupling ferromagnetic fixed layer structure composed of an oxide coupling layer, a ferromagnetic film structure, an antiparallel coupling layer, a ferromagnetic film structure, and an oxide coupling layer, from near to far from the substrate. The two structures contain at least one and any one of the structures contains at least one structure.

2. The magnetic tunnel junction for magnetic storage chips and magnetic sensor chips as described in claim 1, wherein the fixed layer is increased at the end farthest from the substrate by a ferromagnetic fixed layer structure containing an antiferromagnet, which is composed of an oxide coupling layer, a ferromagnetic thin film structure, and an antiferromagnetic thin film structure from near to far from the substrate, and an antiparallel coupled ferromagnetic fixed layer structure containing an antiferromagnet, which is composed of an oxide coupling layer, a ferromagnetic thin film structure, an antiparallel coupling layer, a ferromagnetic thin film structure, and an antiferromagnetic thin film structure from near to far from the substrate.

3. The magnetic tunnel junction for a magnetic storage chip and a magnetic sensor chip as claimed in claims 1 to 2, Its characteristic structure is: From near to far from the substrate, it is composed of a ferromagnetic thin film structure acting as a free layer, a magnesium oxide thin film acting as a tunneling layer, and a ferromagnetic thin film structure acting as a fixed layer; and the fixed layer is composed of a first ferromagnetic thin film structure, an antiparallel coupling layer, a second ferromagnetic thin film structure, a first oxide coupling layer, a third ferromagnetic thin film structure, and a magnesium oxide thin film.

4. The magnetic tunnel junction for a magnetic storage chip and a magnetic sensor chip as claimed in claims 1 to 2, Its characteristic structure is: From near to far from the substrate, it is composed of a ferromagnetic film structure acting as a free layer, a magnesium oxide film acting as a tunneling layer, and a ferromagnetic film structure acting as a fixed layer; and the fixed layer is composed of a first ferromagnetic film structure, an antiparallel coupling layer, a second ferromagnetic film structure, a first oxide coupling layer, a third ferromagnetic film structure, a second oxide coupling layer, a fourth ferromagnetic film structure, and a magnesium oxide film.

5. The magnetic tunnel junction for a magnetic storage chip and a magnetic sensor chip as claimed in claims 1 to 2, Its characteristic structure is: From near to far from the substrate, it is composed of a ferromagnetic thin film structure acting as a free layer, a magnesium oxide film acting as a tunneling layer, and a ferromagnetic thin film structure acting as a fixed layer; and the fixed layer is composed of a first ferromagnetic thin film structure, a first oxide coupling layer, a second ferromagnetic thin film structure, an antiparallel coupling layer, a third ferromagnetic thin film structure, a second oxide coupling layer, a fourth ferromagnetic thin film structure, and a magnesium oxide film.

6. The magnetic tunnel junction for a magnetic storage chip and a magnetic sensor chip as claimed in claims 1 to 2, Its characteristic structure is: From near to far from the substrate, it is composed of a ferromagnetic thin film structure acting as a free layer, a magnesium oxide film acting as a tunneling layer, and a ferromagnetic thin film structure acting as a fixed layer; and the fixed layer is composed of a first ferromagnetic thin film structure, a first oxide coupling layer, a second ferromagnetic thin film structure, an antiparallel coupling layer, a third ferromagnetic thin film structure, a second oxide coupling layer, a fourth ferromagnetic thin film structure, a third oxide coupling layer, a fifth ferromagnetic thin film structure, and a magnesium oxide film.

7. The magnetic tunnel junction for a magnetic storage chip and a magnetic sensor chip as claimed in claims 1 to 2, Its characteristic structure is: From near to far from the substrate, it is composed of a ferromagnetic thin film structure acting as a free layer, a magnesium oxide film acting as a tunneling layer, and a ferromagnetic thin film structure acting as a fixed layer; and the fixed layer is composed of a first ferromagnetic thin film structure, a first antiparallel coupling layer, a second ferromagnetic thin film structure, a first oxide coupling layer, a third ferromagnetic thin film structure, a second antiparallel coupling layer, a fourth ferromagnetic thin film structure, and a magnesium oxide film.

8. The magnetic tunnel junction for a magnetic storage chip and a magnetic sensor chip as claimed in claims 1 to 2, Its characteristic structure is: From near to far from the substrate, it is composed of a ferromagnetic thin film structure acting as a free layer, a magnesium oxide film acting as a tunneling layer, and a ferromagnetic thin film structure acting as a fixed layer; and the fixed layer is composed of a first ferromagnetic thin film structure, a first antiparallel coupling layer, a second ferromagnetic thin film structure, a first oxide coupling layer, a third ferromagnetic thin film structure, a second antiparallel coupling layer, a fourth ferromagnetic thin film structure, and an antiferromagnetic thin film structure.

9. The magnetic tunnel junction for a magnetic storage chip and a magnetic sensor chip as claimed in claims 1 to 2, Its characteristic structure is: From near to far from the substrate, it is composed of a ferromagnetic thin film structure acting as a free layer, a magnesium oxide film acting as a tunneling layer, and a ferromagnetic thin film structure acting as a fixed layer; and the fixed layer is composed of a first ferromagnetic thin film structure, a first oxide coupling layer, a second ferromagnetic thin film structure, an antiparallel coupling layer, a third ferromagnetic thin film structure, a second oxide coupling layer, a fourth ferromagnetic thin film structure, and an antiferromagnetic thin film structure.

10. The magnetic tunnel junction for a magnetic storage chip and a magnetic sensor chip as claimed in claims 1 to 9, Its characteristic structure is: The antiferromagnetic film structure contains at least one antiferromagnetic material, manganese-platinum alloy or manganese-iridium alloy; the ferromagnetic film structure is mainly an alloy containing iron and boron; the antiparallel coupling layer material usually uses either metal ruthenium or metal iridium; the oxide coupling layer is composed of magnesium oxide containing either iron and cobalt plus boron and thicker than the tunneling layer magnesium oxide, iron oxide, and oxide containing iron and cobalt.

11. The method for manufacturing a magnetic tunnel junction for a magnetic storage chip and a magnetic sensor chip according to claims 1 to 10, comprising the following characteristic steps: (1) Preparing peripheral circuits of a magnetic storage chip and a magnetic sensor chip on a substrate; (2) preparing the portion below the free layer of the magnetic tunnel junction on the metal connection layer of the peripheral circuit; (3) preparing a ferromagnetic thin film structure serving as a free layer; (4) preparing a tunneling layer magnesium oxide film; (5) preparing the fixed layer; (6) patterning the thin film to form devices of magnetic storage chips and magnetic sensor chips; (7) Connect and package the devices to form a chip.

Citation Information

Patent Citations

  • Magnetic tunnel junction fixing layer, magnetic memory chip and manufacturing method of magnetic tunnel junction fixing layer

    CN118541014A

Cited By

  • Pinned layer of magnetic tunnel junction, magnetic memory chip and magnetic sensor chip and manufacturing methods therefor

    WO2026031443A1