Reslurrable anti-sticking liners and combination compositions for making same

The difficulty of reslurrying of the anti-adhesive liner is solved by using the first formulation of a vinyl functionalized polysiloxane and noble metal-siloxane composite catalyst in the anti-adhesive liner and an aqueous dispersion of an olefin (co)polymer. The problem of slurrying achieves excellent reslurrying properties and mechanical properties.

CN119013142APending Publication Date: 2024-11-22DOW GLOBAL TECHNOLOGIES LLC +2
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202280094847.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2022-05-13
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Existing anti-adhesive pads are difficult to reslurry after use, resulting in waste accumulation, affecting environmental protection, and existing solutions often compromise other properties such as adhesion strength, peeling ability and wear resistance.

Method used

A first formulation comprising a vinyl functionalized polysiloxane and noble metal-siloxane composite catalyst is used for the preparation of the anti-adhesion layer and an olefin (co)polymer and an olefin-(meth)acrylic acid copolymer are used. The aqueous dispersion acts as an intermediate layer to form a reslurry anti-stick liner.

Benefits of technology

The excellent reslurryability, wear resistance and mechanical strength of the anti-adhesive liner is achieved, while maintaining good bonding strength and peeling force, avoiding deterioration of performance properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119013142A_ABST
    Figure CN119013142A_ABST
Patent Text Reader

Abstract

The invention discloses a reslurrable anti-sticking pad and a combination composition for preparing the reslurrable anti-sticking pad. The combined composition comprises (A) a first formulation comprising a vinyl functionalized polysiloxane, a non-vinyl polysiloxane, and a noble metal-siloxane composite catalyst; (B) a second formulation comprising at least one olefin copolymer and at least one olefin-(meth) acrylic copolymer. The first formulation is independent of the second formulation. The anti-sticking pad prepared by using the combined composition shows excellent re-slurrying property, friction resistance, coating suitability of an anti-sticking coating layer with required release force, and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a unique repulpable release liner and a combination composition for preparing the same. The release liner and the combination composition are specially designed to achieve excellent performance properties, such as repulpability of the release liner, abrasion resistance, and coatability of a release coating with a desired release force. Background Art

[0002] Release liner is widely used in various commercial products, such as adhesive tape, self-adhesive label, protective film, packaging material, container etc., and these commercial products need temporary protection and peeling layer immediately before use. Release liner allows convenient transportation, storage and use of product, but still has some challenges in this field. Exemplary paper release liner coated with polyolefin is usually made of high-density polyethylene (HDPE), low-density polyethylene (LDPE) and polypropylene (PP) plastic resin. Another example comprises kraft paper coated with polyolefin, which is usually machined kraft (MFK) paper and can be coated on one side or both sides so that this kraft paper is very smooth, moisture-proof and dimensionally stable. Due to the existence of polyolefin extrusion coating, all these release liners can not be repulpable. Therefore, one of major challenges is that the use of these commercial products will produce a large amount of waste, particularly the release liner peeled off, which brings serious burden in terms of technology, economy and environmental protection, and therefore highly expects the complete and effective repulping of waste. Some solutions have been reported in the prior art, but they invariably compromise one or more additional performance properties, such as adhesion strength, peel ability, abrasion resistance, mechanical strength, etc. Therefore, there remains a long-felt need for a unique repulpable release liner that can be easily and completely repulped without causing degradation of any other performance properties, such as those mentioned above.

[0003] After continued exploration, we have surprisingly developed a unique repulpable release liner and a combined composition for preparing the release liner that can achieve the above-mentioned goals. Summary of the invention

[0004] The present disclosure provides a unique repulpable release liner and composite composition for making the same.

[0005] In a first aspect of the present disclosure, the present disclosure provides a combination composition for preparing a repulpable release liner, the combination composition comprising (A) a first formulation comprising a vinyl functionalized polysiloxane, a non-vinyl polysiloxane, and a noble metal-siloxane composite catalyst; and (B) a second formulation comprising at least one olefin (co)polymer and at least one olefin-(meth)acrylic acid copolymer; wherein the first formulation is independent of the second formulation. According to an embodiment of the present disclosure, the first formulation is used to prepare a release layer of a repulpable release liner, and the second formulation is used to prepare an intermediate layer sandwiched between the release layer and the backing paper layer. According to another embodiment of the present disclosure, the first formulation is solvent-free.

[0006] In a second aspect of the present disclosure, the present disclosure provides a repulpable release liner prepared with the combined composition of the present disclosure, the release liner comprising (I) a release layer formed with the first formulation; (II) an intermediate layer formed with the second formulation; and (III) a backing layer, which can be a backing paper layer.

[0007] Other features and aspects of the disclosure are discussed in more detail below.It is to be understood that both the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the invention, as claimed. BRIEF DESCRIPTION OF THE DRAWINGS

[0008] For the purpose of illustrating the invention, there are shown in the drawings exemplary embodiments. It should be understood, however, that the disclosure is not limited to the precise arrangements shown.

[0009] Figure 1 is a schematic cross-sectional view of a release liner according to an embodiment of the present disclosure;

[0010] Figure 2 is a schematic cross-sectional view of an adhesive tape roll prepared by using a release liner according to an embodiment of the present disclosure; and

[0011] Figure 3 is a schematic cross-sectional view of a different type of tape / label according to another embodiment of the present disclosure. DETAILED DESCRIPTION

[0012] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which the invention belongs. In addition, all publications, patent applications, patents, and other references mentioned herein are incorporated by reference.

[0013] As disclosed herein, "and / or" means "and, or as an alternative". Unless otherwise indicated, all ranges are inclusive. The terms "polysiloxane" and "siloxane" are interchangeable and refer to molecules having multiple Si-O-Si bonds. The term "(meth)acrylic" refers to acrylic or methacrylic, "(meth)acrylic" refers to acrylic or methacrylic, "(meth)acrylate" refers to acrylate or methacrylate, and "(meth)acrylamide" refers to acrylamide or methacrylamide.

[0014] Without being limited to any particular theory, the technical breakthrough of the present disclosure lies primarily in the specially designed combination of formulations for the release layer and the intermediate layer of the release liner. In particular, it was found that the combination of (A) a first formulation for the release layer and (B) a second formulation for the intermediate layer can produce a release liner that exhibits excellent performance properties such as repulpability, abrasion resistance, curing ability, and mechanical strength (e.g., tensile strength, elongation at break, bond strength between the release layer and the backing layer, etc.).

[0015] It has also been discovered that the types and relative amounts of ingredients used in each of the above components can be further varied to achieve further improvements in the performance properties of the release layer.

[0016] Preparation (A)

[0017] Formulation (A) comprises a vinyl-functional polysiloxane, a , and a noble metal-siloxane composite catalyst.

[0018] According to an embodiment of the present disclosure, the vinyl functionalized polysiloxane used in formulation (A) is a polysiloxane comprising at least one vinyl group per molecule. Specifically, the vinyl functionalized polysiloxane may comprise at least one ViSiO 3 / 2 ,ViR 1 SiO 2 / 2 , or Vi(R 2 )2SiO 1 / 2 units, and may further comprise at least one unit selected from the group consisting of: SiO 4 / 2 , R 3 SiO 3 / 2 , (R 4 )2SiO 2 / 2 , (R 5 )3SiO 1 / 2 and any combination thereof, wherein Vi represents a vinyl group (-CH=CH2), and R 1 , R 2 , R 3 , R 4 and R 5Each of which is independently selected from H, Cl-C 16 Alkyl groups and C1-C 16 Alkoxy groups and combinations thereof; According to an exemplary embodiment, R 1 , R 2 , R 3 , R 4 and R 5 Each of them is independently a C1-C6 alkyl group such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, etc., or a C1-C6 alkoxy group such as methoxy, ethoxy, propoxy, butoxy, etc.

[0019] According to an embodiment of the present disclosure, the vinyl-functionalized polysiloxane comprises, based on the total weight of the vinyl-functionalized polysiloxane, 0.05 wt% to 8 wt%, such as 0.1 wt% to 6 wt%, or 0.2 wt% to 5 wt%, or 0.3 wt% to 3 wt%, or 0.35 wt% to 2 wt%, or 0.4 wt% to 1 wt%, or 0.5 wt% to 0.8 wt%, or 0.6 wt% to 0.7 wt% of vinyl groups; for example, the vinyl content can be within the range of values ​​obtained by combining any two of the following two endpoints: 0.1 wt%, 0.15 wt%, 0.2 wt%, 0.25 wt%, 0.3 wt%, 0.35 wt%, 0.4 wt%, 0.45 wt%, 0.5 wt%, 0.6 wt%, 0.7 wt%, 0.8 wt%, 0.9 wt%, 10 wt%, 11 wt%, 12 wt%, 13 wt%, 14 wt%, 15 wt%, 16 wt%, 17 wt%, 18 wt%, 19 wt%, 20 wt%, 21 wt%, 22 wt%, 23 wt%, 24 wt%, 25 wt%, 26 wt%, 27 wt%, 28 wt%, 29 wt%, 30 wt%, 31 wt%, 32 wt%, 34 wt%, 36 wt%, 37 wt%, 38 wt%, 39 wt%, 40 wt%, 41 wt%, 42 wt%, 43 wt%, 44 wt%, 45 wt%, 46 wt%, 47 wt%, 48 wt%, 49 wt%, 50 wt .5 weight %, 0.55 weight %, 0.6 weight %, 0.65 weight %, 0.7 weight %, 0.75 weight %, 0.8 weight %, 0.85 weight %, 0.9 weight %, 0.95 weight %, 1 weight %, 1.2 weight %, 1.5 weight %, 1.8 weight %, 2 weight %, 2.2 weight %, 2.5 weight %, 2.8 weight %, 3 weight %, 3.2 weight %, 3.5 weight %, 3.8 weight %, 4 weight %, 4.2 weight %, 4.5 weight %, 4.8 weight %, 5 weight %, 5.2 weight %, 5.5 weight %, 5.8 weight %, 6 weight %, 6.2 weight %, 6.5 weight %, 6.8 weight %, 7 weight %, 7.2 weight %, 7.5 weight %, 7.8 weight %, 8 weight %.

[0020] As is generally known in the art of polysiloxanes, oxygen atoms have subscripts such as "1 / 2", "2 / 2", "3 / 2" and "4 / 2" because each of these oxygen atoms is actually shared by two silicon atoms. For example, "Vi(R 2 )2SiO 1 / 2 " represents a unit having the formula

[0021]

[0022] The oxygen atom marked with an asterisk is further attached to another silicon atom.

[0023] According to an exemplary embodiment of the present disclosure, the vinyl-functionalized polysiloxane comprises, based on the total weight of the vinyl-functionalized polysiloxane, 0.01 wt % to 25 wt %, such as 0.1 wt % to 22 wt %, or 0.5 wt % to 20 wt %, or 1 wt % to 18 wt %, or 1.5 wt % to 15 wt %, or 2 wt % to 12 wt %, or 2.2 wt % to 10 wt %, or 2.5 wt % to 5 wt % of Vi(R 2 )2SiO 1 / 2 Unit; for example, Vi(R 2 )2SiO 1 / 2 The content of the unit can be in a numerical range obtained by combining any two of the following two endpoint values: 0.01 wt%, 0.05 wt%, 0.1 wt%, 0.15 wt%, 0.2 wt%, 0.25 wt%, 0.3 wt%, 0.35 wt%, 0.4 wt%, 0.45 wt%, 0.5 wt%, 0.55 wt%, 0.6 wt%, 0.65 wt%, 0.7 wt%, 0.75 wt%, 0.8 wt%, 0.85 wt%, 0.9 wt%, 0.95 wt%, 1 wt%, 1.2 wt%, 1.5 wt%, 1 .8 weight %, 2 weight %, 2.2 weight %, 2.5 weight %, 2.8 weight %, 3 weight %, 3.2 weight %, 3.5 weight %, 3.8 weight %, 4 weight %, 4.2 weight %, 4.5 weight %, 4.8 weight %, 5 weight %, 5.2 weight %, 5.5 weight %, 5.8 weight %, 6 weight %, 6.2 weight %, 6.5 weight %, 6.8 weight %, 7 weight %, 7.2 weight %, 7.5 weight %, 7.8 weight %, 8 weight %, 10 weight %, 12 weight %, 15 weight %, 18 weight %, 20 weight %, 22 weight %, 25 weight %.

[0024] According to an exemplary embodiment of the present disclosure, the vinyl-functionalized polysiloxane comprises, based on the total weight of the vinyl-functionalized polysiloxane, 0.01 wt % to 20 wt %, such as 0.1 wt % to 18 wt %, or 0.5 wt % to 16 wt %, or 1 wt % to 15 wt %, or 1.5 wt % to 12 wt %, or 2 wt % to 10 wt %, or 2.2 wt % to 8 wt %, or 2.5 wt % to 5 wt % of ViSiO 3 / 2 ; For example, ViSiO 3 / 2The content of the unit can be in a numerical range obtained by combining any two of the following two endpoint values: 0.01 wt%, 0.05 wt%, 0.1 wt%, 0.15 wt%, 0.2 wt%, 0.25 wt%, 0.3 wt%, 0.35 wt%, 0.4 wt%, 0.45 wt%, 0.5 wt%, 0.55 wt%, 0.6 wt%, 0.65 wt%, 0.7 wt%, 0.75 wt%, 0.8 wt%, 0.85 wt%, 0.9 wt%, 0.95 wt%, 1 wt%, 1.2 wt%, 1. 5 weight%, 1.8 weight%, 2 weight%, 2.2 weight%, 2.5 weight%, 2.8 weight%, 3 weight%, 3.2 weight%, 3.5 weight%, 3.8 weight%, 4 weight%, 4.2 weight%, 4.5 weight%, 4.8 weight%, 5 weight%, 5.2 weight%, 5.5 weight%, 5.8 weight%, 6 weight%, 6.2 weight%, 6.5 weight%, 6.8 weight%, 7 weight%, 7.2 weight%, 7.5 weight%, 7.8 weight%, 8 weight%, 10 weight%, 12 weight%, 15 weight%, 18 weight%, 20 weight%.

[0025] According to an exemplary embodiment of the present disclosure, the vinyl functionalized polysiloxane comprises, based on the total weight of the vinyl functionalized polysiloxane, 0.01 wt % to 20 wt %, such as 0.1 wt % to 18 wt %, or 0.5 wt % to 16 wt %, or 1 wt % to 15 wt %, or 1.5 wt % to 12 wt %, or 2 wt % to 10 wt %, or 2.2 wt % to 8 wt %, or 2.5 wt % to 5 wt % of ViR 1 SiO 2 / 2 For example, ViR 1 SiO 2 / 2The content of the unit can be in a numerical range obtained by combining any two of the following two endpoint values: 0.01 wt%, 0.05 wt%, 0.1 wt%, 0.15 wt%, 0.2 wt%, 0.25 wt%, 0.3 wt%, 0.35 wt%, 0.4 wt%, 0.45 wt%, 0.5 wt%, 0.55 wt%, 0.6 wt%, 0.65 wt%, 0.7 wt%, 0.75 wt%, 0.8 wt%, 0.85 wt%, 0.9 wt%, 0.95 wt%, 1 wt%, 1.2 wt%, 1. 5 weight%, 1.8 weight%, 2 weight%, 2.2 weight%, 2.5 weight%, 2.8 weight%, 3 weight%, 3.2 weight%, 3.5 weight%, 3.8 weight%, 4 weight%, 4.2 weight%, 4.5 weight%, 4.8 weight%, 5 weight%, 5.2 weight%, 5.5 weight%, 5.8 weight%, 6 weight%, 6.2 weight%, 6.5 weight%, 6.8 weight%, 7 weight%, 7.2 weight%, 7.5 weight%, 7.8 weight%, 8 weight%, 10 weight%, 12 weight%, 15 weight%, 18 weight%, 20 weight%.

[0026] According to another embodiment of the present disclosure, based on the total weight of the vinyl-functionalized polysiloxane, SiO 4 / 2 , R 3 SiO 3 / 2 , (R 4 )2SiO 2 / 2 and R 5 SiO 1 / 2 The content of each of may be, for example, 0 wt % to 100 wt %, or 2 wt % to 95 wt %, or 5 wt % to 90 wt %, or 8 wt % to 85 wt %, or 10 wt % to 80 wt %, or 15 wt % to 75 wt %, or 20 wt % to 70 wt %, or 25 wt % to 65 wt %, or 30 wt % to 60 wt %, or 35 wt % to 55 wt %, or 40 wt % to 50 wt %, or 45 wt % to 48 wt %.

[0027] According to an exemplary embodiment of the present disclosure, the vinyl-functionalized polysiloxane may be represented by the general formula (1):

[0028] [Vi(R 2 )2SiO 1 / 2 ] m -(SiO 4 / 2 ) n -(R 3 SiO 3 / 2 ) p -[(R 4 )2SiO 2 / 2 ] q-[(R 5 )3SiO 1 / 2 ] r Formula (1) wherein each of the subscripts m, n, p, q and r is independently an integer from 0 to 500, such as from 1 to 400, or from 2 to 300, or within a numerical range obtained by combining any two of the following endpoint values: 0, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 12, 15, 18, 20, 22, 25, 30, 35, 40, 45, 50, 55, 60 , 70, 80, 90, 100, 110, 120, 130, 140, 150, 160, 170, 180, 190, 200, 220, 250, 300, 350, 400, 450, 500; for example, subscript m can be an integer from 1 to 100, each of subscripts n, p, q and r is independently an integer from 0 to 500, and 3≤n+p+q+r≤2000. According to another embodiment, R 1 , R 2 , R 3 , R 4 and R 5 Neither is hydrogen.

[0029] According to another embodiment of the present disclosure, the vinyl-functionalized polysiloxane is represented by the general formula (2):

[0030] (ViMe2SiO 1 / 2 ) m -(SiO 4 / 2 ) n -(Me 3 SiO 3 / 2 ) p -[Me2SiO 2 / 2 ] q -[Me3SiO 1 / 2 ] r Formula (2)

[0031] wherein each of the subscripts m, n, p, q and r are as defined above.

[0032] According to an embodiment of the present disclosure, the viscosity of the vinyl functionalized polysiloxane at 25° C. is about 80 mPa·s to 2000 mPa·s, such as 100 mPa·s to 1500 mPa·s, or 120 mPa·s to 1200 mPa·s, or 150 mPa·s to 1000 mPa·s, or 200 mPa·s to 800 mPa·s, or 220 mPa·s to 600 mPa·s, or 250 mPa·s to 400 mPa·s. s, or 280 mPa·s to 350 mPa·s, or in a numerical range obtained by combining any two of the following two endpoint values: 80 mPa·s, 100 mPa·s, 120 mPa·s, 150 mPa·s, 180 mPa·s, 200 mPa·s, 220 mPa·s, 250 mPa·s, 280 mPa·s, 300 mPa·s, 320 mPa·s, 350 mPa·s, 380 mPa·s a·s, 400mPa·s, 420mPa·s, 450mPa·s, 500mPa·s, 550mPa·s, 600mPa·s, 650mPa·s, 700mPa·s, 750mPa ·s, 800mPa·s, 850mPa·s, 900mPa·s, 950mPa·s, 1000mPa·s, 1050mPa·s, 1100mPa·s, 1150mPa·s, 1200 mPa·s, 1250mPa·s, 1300mPa·s, 1350mPa·s, 1400mPa·s, 1450mPa·s, 1500mPa·s, 1550mPa·s, 1600mPa ·s, 1650mPa·s, 1700mPa·s, 1750mPa·s, 1800mPa·s, 1850mPa·s, 1900mPa·s, 1950mPa·s, 2000mPa·s.

[0033] As used herein, all viscosities are reported in millipascals*seconds (mPa·s) unless otherwise stated and were measured using a cone-plate rheometer with a CP#52 spindle at a speed of 0.1 rpm (0.2 s -1 The low shear viscosity was measured at a shear rate of 10 rpm (20 s -1 High shear viscosity was measured at a shear rate of 1.5 %.

[0034] According to an embodiment of the present disclosure, the content of the vinyl-functionalized polysiloxane can be 80 wt % to 99 wt %, such as 82 wt % to 98.5 wt %, or 85 wt % to 98 wt %, or 87 wt % to 97.5 wt %, or 88 wt % to 97 wt %, or 90 wt % to 96.5 wt %, or 92 wt % to 96 wt %, based on the total weight of the first formulation, or within the numerical range obtained by combining any two of the following two endpoints: 80 wt %, 82 wt %, 85 wt %, 88 wt %, 90 wt %, 92 wt %, 93 wt %, 94 wt %, 95 wt %, 96 wt %, 97 wt %, 98 wt %, 99 wt %.

[0035] According to an embodiment of the present disclosure, the non-vinyl polysiloxane may be represented by the general formula (3):

[0036] [(R 6 )3SiO 1 / 2 ] a -(SiO 4 / 2 ) b -(R 7 SiO 3 / 2 ) c -[(R 8 )2SiO 2 / 2 ] d Formula (3)

[0037] Where R 6 , R 7 and R 8 Each of which is independently selected from the group consisting of: H, C1-C 16 Alkyl groups, and C1-C 16 Alkoxy groups and combinations thereof; According to an exemplary embodiment, R 6 , R 7 and R 8Each of the subscripts a, b, c and d is independently an integer from 0 to 300, such as 1 to 200, or 2 to 280, or in a numerical range obtained by combining any two of the following two endpoint values: 0, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, 31, 32, 33, 34, 35, 36, 37, 38, 39, 40, 41, 42, 43, 44, 45, 46, 47, 48, 50, 51, 52, 53, 54, 55, 56, 57, 58, 59, 60, 61, 62, 63, 64, 65, 66, 67, 68, 79, 80, 81, 82, 83, 84, 85, 86, 87, 88, 89, 90, 91, 92 , 9, 10, 12, 15, 18, 20, 22, 25, 30, 35, 40, 45, 50, 55, 60, 70, 80, 90, 100, 110, 120, 130, 140, 150, 160, 170, 180, 190, 200, 220, 250, 300; for example, subscript a can be an integer from 1 to 100, or 2 to 50, each of subscripts b, c and d is independently an integer from 0 to 200, and 3≤a+b+c+d≤800. According to an embodiment, the non-vinyl polysiloxane is represented by “(R 6 )3SiO 1 / 2 "Unit termination.

[0038] According to another embodiment of the present disclosure, the non-vinyl polysiloxane is represented by formula (4):

[0039] [(Me)3SiO 1 / 2 ] a -(SiO 4 / 2 ) b -(MeSiO 3 / 2 ) c -[(Me)2SiO 2 / 2 ] d Formula (4)

[0040] wherein each of the subscripts a, b, c and d are as defined above.

[0041] According to an embodiment of the present disclosure, the viscosity of the non-vinyl polysiloxane at 25° C. is about 5 mPa·s to 100 mPa·s, such as 8 mPa·s to 90 mPa·s, or 10 mPa·s to 85 mPa·s, or 12 mPa·s to 80 mPa·s, or 15 mPa·s to 70 mPa·s, or 16 mPa·s to 60 mPa·s, or 17 mPa·s to 50 mPa·s, or 18 mPa·s to 40 mPa·s, or 20 mPa·s to 30 mPa·s, or by combining the following two The numerical range of any two endpoint values ​​is as follows: 5mPa·s, 8mPa·s, 10mPa·s, 12mPa·s, 15mPa·s, 20mPa·s, 25mPa·s, 30mPa·s, 35mPa·s, 40mPa·s, 45mPa·s, 50mPa·s, 55mPa·s, 60mPa·s, 65mPa·s, 70mPa·s, 75mPa·s, 80mPa·s, 90mPa·s, 95mPa·s, 100mPa·s.

[0042] According to an embodiment of the present disclosure, the content of the non-vinyl polysiloxane can be 0.05 wt% to 10 wt%, such as 0.1 wt% to 8 wt%, or 0.5 wt% to 7 wt%, or 0.8 wt% to 6 wt%, or 1 wt% to 5 wt%, or 1.2 wt% to 4 wt%, or 1.5 wt% to 3 wt%, or 2.5 wt% to 3 wt%, based on the total weight of the first formulation, or within a numerical range obtained by combining any two of the following two endpoint values: 0.05 wt%, 0.08 wt%, 0.1 wt%, 0.2 wt%, 0.3 wt%, 0.5 wt%, 0.8 wt%, 0.9 wt%, 1 wt%, 1.1 wt%, 1.2 wt%, 1.3 wt%, 1.4 wt%, 1.5 wt%, 1.6 wt%, or 1.7 wt%. %, 1.7 wt%, 1.8 wt%, 1.9 wt%, 2 wt%, 2.1 wt%, 2.2 wt%, 2.3 wt%, 2.5 wt%, 2.6 wt%, 2.7 wt%, 2.8 wt%, 2.9 wt%, 3 wt%, 3.2 wt%, 3.5 wt%, 3.8 wt%, 4 wt%, 4.2 wt%, 4.5 wt%, 4.8 wt%, 5 wt%, 5.2 wt%, 5.5 wt%, 5.8 wt%, 6 wt%, 6.2 wt%, 6.5 wt%, 6.8 wt%, 7 wt%, 7.2 wt%, 7.5 wt%, 7.8 wt%, 8 wt%, 8.2 wt%, 8.5 wt%, 8.8 wt%, 9 wt%, 9.2 wt%, 9.5 wt%, 9.8 wt%, 10 wt%.

[0043] According to an embodiment of the present disclosure, the noble metal-siloxane composite catalyst comprises or consists of at least one noble metal and a siloxane ligand, wherein the noble metal may be selected from the group consisting of Pt, Pd, Ru, Rh, Os, Ir, Ag, alloys thereof, and mixtures thereof, and the siloxane ligand may be optionally containing one or more substituent groups such as hydrogen, C1-C 16 Alkyl, C1-C 16 Alkoxy, C2-C 16 For example, the siloxane ligand may contain more than one C2-C 16 Alkenyl (e.g. vinyl) and more than one C1-C 16 Alkyl groups such as divinyl-tetramethyldisiloxane, especially 1,3-divinyl-1,1,3,3-tetramethyldisiloxane.

[0044] According to another embodiment of the present disclosure, the noble metal-siloxane composite catalyst can be used in the form of a dispersion, which comprises the noble metal-siloxane composite catalyst dispersed in a polysiloxane dispersant, wherein the polysiloxane dispersant can be represented by formula (5):

[0045] [Vi(R 9 )2SiO 1 / 2 ] A -(SiO 4 / 2 ) B -(R 10 SiO 3 / 2 ) C -[(R 11 )2SiO 2 / 2 ] D -[(R 12 )3SiO 1 / 2 ] E Formula (5) where R 9 , R 10 , R 11 and R 12 Each of which is independently selected from the group consisting of: H, C1-C 16 Alkyl groups, and C1-C 16 Alkoxy groups and combinations thereof; According to an exemplary embodiment, R 9 , R 10 , R 11 and R 12 Each of is independently a C1-C6 alkyl group, such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, etc., or a C1-C6 alkoxy group, such as methoxy, ethoxy, propoxy, butoxy, etc. According to another embodiment, R 9 , R10 , R 11 and R 12 None of them is hydrogen. Each of the subscripts A, B, C, D and E is independently an integer from 0 to 500, such as from 1 to 400, or from 2 to 300, or within a numerical range obtained by combining any two of the following endpoint values: 0, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 12, 15, 18, 20, 22, 25, 30, 35, 40, 45, 50, 55, 60, 70 , 80, 90, 100, 110, 120, 130, 140, 150, 160, 170, 180, 190, 200, 220, 250, 300, 350, 400, 450, 500; for example, subscript A can be an integer from 1 to 100, each of the subscripts B, C, D and E is independently an integer from 0 to 500, and 3≤B+C+D+E≤2000.

[0046] According to another embodiment of the present disclosure, the polysiloxane dispersant is represented by formula (6):

[0047] [ViMeSiO 1 / 2 ] A -(SiO 4 / 2 ) B -(MeSiO 3 / 2 ) C -[Me2SiO 2 / 2 ] D -[Me3SiO 1 / 2 ] E Formula (6)

[0048] wherein each of the subscripts A, B, C, D and E are as defined above.

[0049] According to another embodiment of the present disclosure, the dispersion comprises the above-mentioned noble metal-siloxane composite catalyst and a polysiloxane dispersant, wherein the content of the noble metal-siloxane composite catalyst can be based on the total weight of the dispersion, 0.01 wt % to 15 wt %, such as 0.1 wt % to 12 wt %, or 0.5 wt % to 10 wt %, or 0.8 wt % to 8 wt %, or 1 wt % to 7 wt %, or 1.2 wt % to 6 wt %, or 1.3 wt % to 5 wt %, or 1.5 wt % to 3 wt %, or within the numerical range obtained by combining any two of the following two endpoint values: 0.01 wt %, 0.02 wt %, 0.05 wt %, 0.08 wt %, 0.1 wt %, 0.2 wt %, 0.3 wt %, 0.5 wt %, 0.8 wt %, 0.9 wt %, 1 wt %, 1.1 wt %, 1.2 wt %, 1.3 wt %, 1.4 wt %, %, 1.5 wt%, 1.6 wt%, 1.7 wt%, 1.8 wt%, 1.9 wt%, 2 wt%, 2.1 wt%, 2.2 wt%, 2.3 wt%, 2.5 wt%, 2.6 wt%, 2.7 wt%, 2.8 wt%, 2.9 wt%, 3 wt%, 3.2 wt%, 3.5 wt%, 3.8 wt%, 4 wt%, 4.2 wt%, 4.5 wt%, 4.8 wt%, 5 wt%, 5. 2 weight%, 5.5 weight%, 5.8 weight%, 6 weight%, 6.2 weight%, 6.5 weight%, 6.8 weight%, 7 weight%, 7.2 weight%, 7.5 weight%, 7.8 weight%, 8 weight%, 8.2 weight%, 8.5 weight%, 8.8 weight%, 9 weight%, 9.2 weight%, 9.5 weight%, 9.8 weight%, 10 weight%, 11 weight%, 12 weight%, 13 weight%, 14 weight%, 15 weight%.According to an embodiment of the present disclosure, the viscosity of the dispersion of the catalyst at 25° C. is about 100 mPa·s to 3000 mPa·s, such as 150 mPa·s to 2500 mPa·s, or 180 mPa·s to 2200 mPa·s, or 200 mPa·s to 2000 mPa·s, or 220 mPa·s to 1800 mPa·s, or 250 mPa·s to 1500 mPa·s, or 280 mPa·s to 1200 mPa·s, or 300 mPa·s to 400 mPa·s. The range of the present invention is as follows: 100 mPa·s, 120 mPa·s, 150 mPa·s, 180 mPa·s, 200 mPa·s, 220 mPa·s, 250 mPa·s, 280 mPa·s, 300 mPa·s, 320 mPa·s, 350 mPa·s, 380 mPa·s, 400 mPa·s, 4 20mPa·s, 450mPa·s, 500mPa·s, 550mPa·s, 600mPa·s, 650mPa·s, 700mPa·s, 750mPa·s, 800mPa·s, 850mPa·s, 900mPa·s, 950mPa·s, 1000mPa·s, 1050mPa·s, 1100mPa·s, 1150mPa·s, 1200mPa·s, 1250mPa·s, 1300mPa·s, 1 350mPa·s, 1400mPa·s, 1450mPa·s, 1500mPa·s, 1550mPa·s, 1600mPa·s, 1650mPa·s, 1700mPa·s, 1750mPa·s, 1800mPa·s, 1850mPa·s, 1900mPa·s, 1950mPa·s, 2000mPa·s, 2200mPa·s, 2500mPa·s, 2800mPa·s, 3000mPa·s.

[0050] According to another embodiment of the present disclosure, the amount of the above-mentioned dispersion (of the catalyst) can be based on the total weight of the first formulation, 0.05 wt% to 10 wt%, such as 0.1 wt% to 8 wt%, or 0.5 wt% to 7 wt%, or 0.8 wt% to 6 wt%, or 1 wt% to 5 wt%, or 1.2 wt% to 4 wt%, or 1.5 wt% to 3 wt%, or in the numerical range obtained by combining any two of the following two endpoints: 0.05 wt%, 0.08 wt%, 0.1 wt%, 0.2 wt%, 0.3 wt%, 0.5 wt%, 0.8 wt%, 0.9 wt%, 1 wt%, 1.1 wt%, 1.2 wt%, 1.3 wt%, 1.4 wt%, 1.5 wt%, 1.6 wt% %, 1.7 wt%, 1.8 wt%, 1.9 wt%, 2 wt%, 2.1 wt%, 2.2 wt%, 2.3 wt%, 2.5 wt%, 2.6 wt%, 2.7 wt%, 2.8 wt%, 2.9 wt%, 3 wt%, 3.2 wt%, 3.5 wt%, 3.8 wt%, 4 wt%, 4.2 wt%, 4.5 wt%, 4.8 wt%, 5 wt%, 5.2 wt%, 5.5 wt%, 5.8 wt%, 6 wt%, 6.2 wt%, 6.5 wt%, 6.8 wt%, 7 wt%, 7.2 wt%, 7.5 wt%, 7.8 wt%, 8 wt%, 8.2 wt%, 8.5 wt%, 8.8 wt%, 9 wt%, 9.2 wt%, 9.5 wt%, 9.8 wt%, 10 wt%.

[0051] According to another embodiment of the present disclosure, the first preparation is solvent-free. As used herein, the term "solvent-free" means that solvents such as water and any common organic solvents (such as alkanes, halogenated hydrocarbons, ethers, alcohols, esters, aromatic hydrocarbons, ketones, tetrahydrofuran, dimethylformamide, N-methylpyrrolidone, carbon disulfide, etc.) are not intentionally incorporated therein, and preparations containing trace amounts of these solvents as inevitable impurities (such as impurities contained in raw materials) are also considered to be solvent-free. For example, the solvent content of the first solvent-free preparation can be based on the gross weight of the first preparation, less than 1 weight %, such as less than 0.9 weight %, or less than 0.8 weight %, or less than 0.7 weight %, or less than 0.6 weight %, or less than 0.5 weight %, or less than 0.4 weight %, or less than 0.3 weight %, or less than 0.25 weight %, or less than 0.2 weight %. According to embodiments of the present disclosure, the vinyl-functionalized polysiloxane, the non-vinyl polysiloxane, and the one noble metal-siloxane composite catalyst (as well as the above-mentioned dispersion containing the noble metal-siloxane composite catalyst) are solvent-free.

[0052] The first formulation may optionally contain one or more conventional additives, such as fillers, pigments, film formers, thickeners, anti-migration aids, curing agents, coalescing agents, lubricants, flame retardants, light stabilizers, heat stabilizers, biocides, plasticizers, waxes or antioxidants.

[0053] Preparation (B)

[0054] Preparation (B) is an aqueous dispersion comprising at least one olefin (co)polymer and at least one olefin-(meth)acrylic acid copolymer.

[0055] The olefin (co)polymer may be C2-C 16 Homopolymers of olefins, two or more C2-C 16 Copolymers of olefins, or at least one C2-C 16 The olefin (co)polymer can be a copolymer of ethylene and one or more C3-C 16 Copolymers of α-olefins (such as 1-propylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-nonene, 1-decene, 1-dodecene, butadiene, styrene, etc.). 16 )α-olefin copolymers, ethylene and (C3-C 16) The molar ratio between the α-olefins can be from 99:1 to 1:99, such as within the range of values ​​obtained by combining any two of the following endpoints: 95:1, 90:1, 85:1, 80:1, 75:1, 70:1, 65:1, 60:1, 55:1, 50:1, 45:1, 40:1, 35:1, 30:1, 25:1, 20:1, 15:1, 10:1, 5:1, 3:1, 2:1, 1:1, 1:2, 1:3, 1:5, 1:10, 1:15, 1:20, 1:25, 1:30, 1:35, 1:40, 1:45, 1:50, 1:55, 1:60, 1:65, 1:70, 1:80, 1:90. The olefin (co)polymer can have a melt flow rate (MFR) in the range of 0.1 g / 10 min to 50 g / 10 min, such as 0.1 to 50, or 0.2 to 45, or 0.5 to 45, or 0.5 to 40, or 0.5 to 35, or 0.8 to 35, or 1 to 35, or 2 to 35, measured according to ASTM D-1238 (at 190°C / 2.16Kg). The content of olefin (co)polymer can be 10 wt % to 50 wt %, such as 15 wt % to 45 wt %, or 20 wt % to 40 wt %, or 25 wt % to 35 wt %, or 28 wt % to 32 wt %, based on the total weight of formulation (B), for example within the range of values ​​obtained by combining any two of the following endpoint values: 10 wt %, 12 wt %, 14 wt %, 15 wt %, 18 wt %, 20 wt %, 22 wt %, 25 wt %, 28 wt %, 30 wt %, 32 wt %, 34 wt %, 35 wt %, 38 wt %, 40 wt %, 42 wt %, 45 wt %, 48 wt %, 50 wt %.

[0056] The olefin-(meth)acrylic acid copolymer may be at least one C2-C 16 A copolymer of an olefin and at least one (meth) acrylic acid monomer, wherein the C2-C 16 Olefins may include C2-C 12 olefins or C2-C6 olefins, such as ethylene, propylene, butene, pentene, hexene, heptene, octene, nonene or styrene; the (meth) acrylic acid monomer may include methacrylic acid, acrylic acid, methacrylamide, acrylamide, methacrylonitrile, acrylonitrile, methacrylic acid (C1-C 12 ) alkyl esters (e.g., methyl methacrylate, ethyl methacrylate, propyl methacrylate, butyl methacrylate, pentyl methacrylate, hexyl methacrylate, etc.), acrylic acid (C1-C 12) alkyl esters (e.g., methyl acrylate, ethyl acrylate, propyl acrylate, butyl acrylate, pentyl acrylate, hexyl acrylate, etc.), and any combination thereof. The molar ratio between the olefin and the (meth)acrylic acid monomer can be from 99:1 to 1:99, such as within the range of values ​​obtained by combining any two of the following endpoints: 95:1, 90:1, 85:1, 80:1, 75:1, 70:1, 65:1, 60:1, 55:1, 50:1, 45:1, 40:1, 35:1, 30:1, 25:1, 20:1, 15:1, 10:1, 5:1, 3:1, 2:1, 1:1, 1:2, 1:3, 1:5, 1:10, 1:15, 1:20, 1:25, 1:30, 1:35, 1:40, 1:45, 1:50, 1:55, 1:60, 1:65, 1:70, 1:80, 1:90. The olefin-(meth)acrylic acid copolymer may have a melt flow rate (MFR) in the range of 0.1 g / 10 min to 50 g / 10 min, such as 0.1 to 50, or 0.2 to 45, or 0.5 to 45, or 0.5 to 40, or 0.5 to 35, or 0.8 to 35, or 1 to 35, or 2 to 35, measured according to ASTM D-1238 (at 190° C. / 2.16 Kg). The content of the olefin-(meth)acrylic acid copolymer can be 2% to 30% by weight, such as 5% to 28% by weight, or 8% to 25% by weight, or 10% to 20% by weight, or 12% to 15% by weight, based on the total weight of the formulation (B), such as within the range of values ​​obtained by combining any two of the following endpoint values: 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 20%, 22%, 25%, 28%, 30% by weight.

[0057] Preparation (B) may contain one or more conventional additives such as surfactants, emulsifiers, fillers, film formers, colorants, pigments, thickeners, anti-migration aids, curing agents, coalescing agents, biocides, plasticizers, waxes, anti-aging agents or antioxidants.

[0058] Furthermore, in addition to the above-mentioned components, formulation (B) may contain a balance of water, such as having a water content of about 30% to 75% by weight, or 40% to 65% by weight, or 45% to 60% by weight, or 50% to 58% by weight, based on the total weight of formulation (B), such as within the range of values ​​obtained by combining any two of the following endpoint values: 30%, 32%, 35%, 38%, 40%, 42%, 45%, 48%, 50%, 52%, 55%, 58%, 60%, 62%, 65%, 68%, 70%, 72%, 75% by weight.

[0059] The above-mentioned formulation (A) and formulation (B) can be used independently to form individual components of the release liner of the present disclosure. Figure 1 A cross section of an exemplary release liner is shown, the cross section including, from bottom to top, a backing layer, an intermediate layer, and a release layer, wherein the intermediate layer is formed with formulation (B), and the release layer is formed with formulation (A).

[0060] According to an embodiment of the present disclosure, the backing layer may be made of a material selected from the group consisting of: paper, such as kraft paper, coated kraft paper, pressure-sensitive paper, glassine paper, coated glassine paper, adhesive tape, recycled paper, etc.; degradable polymers or natural materials, such as polylactic acid, polybutylene succinate / hexanoate, polyhydroxybutyrate / valerate, polyvinyl succinate, polycaprolactone, starch, modified cellulose; and any combination thereof. According to another embodiment, the backing layer may be made of kraft paper. According to a preferred embodiment of the present disclosure, the backing layer is not made of a non-repulpable material. For example, in various adhesive tapes or label products, polyethylene-coated kraft (PEK) paper, which is generally used as a backing layer or release liner after siliconization on the PE-coated side, cannot achieve the desired repulpability and is therefore completely unsuitable for the backing layer of the present disclosure.

[0061] According to an embodiment of the present disclosure, the backing layer is repulpable. As used herein, the term "repulpable" or "repulpability" means that the object can be fully degraded and disintegrated under common pulping (disintegration) conditions (e.g., treated in a warm aqueous solution stirred at a specific pH), so that the content of the remaining large fragments and debris (e.g., those having a size greater than 0.01 inches or about 0.254 mm) is minimized to the original weight (solid weight) of the object before the repulping process, such as less than 14 wt %, or less than 12 wt %, or less than 10 wt %, or less than 8 wt %, or less than 6 wt %. According to an embodiment of the present disclosure, the anti-adhesive layer, the intermediate layer and the backing layer are all repulpable. According to another embodiment of the present disclosure, the entire anti-adhesive layer is repulpable.

[0062] like Figure 1 As shown, the release liner can be prepared by applying the formulation (B) to one or both surfaces of the backing layer by any suitable coating technique such as gravure coating, roller coating, rod coating, knife coating, cast coating, spray coating, dip coating, die coating, blade coating, printing, etc., and the coating weight of this layer can be about 1 g / m 2 Up to 30g / m 2 , such as 2g / m 2 Up to 20g / m 2 , or 2g / m 2 Up to 10g / m 2 , or 2g / m 2 Up to 5g / m 2 The coated layer may then be cured at a temperature from ambient temperature to 200°C, such as from 50°C to 180°C, or from 60°C to 160°C, or from 80°C to 150°C, or from 90°C to 130°C, or from 100°C to 130°C. After curing and drying of the intermediate layer, a release layer may be formed on the surface of the intermediate layer by combining each component of formulation (A) to form a blend (e.g., a paste), and applying this blend to the outer surface of the intermediate layer by any of the above-mentioned coating techniques, and the coating weight of the release layer (wet) may be about 0.5 g / m 2 Up to 20g / m 2 , such as 0.5g / m 2 Up to 15g / m 2 , or 0.5g / m 2 Up to 10g / m 2 , or 0.8g / m 2 Up to 10g / m 2 The coated release layer may then be cured at a temperature of from ambient to 200°C, such as from 50°C to 180°C, or from 60°C to 170°C, or from 80°C to 160°C, or from 100°C to 150°C, or from 120°C to 150°C.

[0063] Release liners can be cut into different sizes and used for different applications, such as adhesive sheets for release sheets or continuous adhesive tapes. Figure 2 A schematic diagram of a continuous adhesive tape in roll form is shown, wherein the laminate formed by the release liner and the adhesive layer is wound into a roll. The adhesive tape roll can be unrolled for a specific purpose, and the release liner can be easily peeled off before or after the adhesive layer is bonded to the surface of an object. The peeled release liner has excellent repulpability and can therefore be easily repulped and recycled.

[0064] Figure 3A label or tape comprising an adhesive layer sandwiched between the release liner of the present invention and a carrier layer is shown, wherein the bond strength between the carrier layer and the adhesive layer is much higher, and the two layers are applied to the surface of an object as a whole while the release liner is previously peeled off and repulped. The carrier layer may have printed images, letters or symbols.

[0065] Example

[0066] Some embodiments of the present invention will now be described in the following examples, wherein all parts and percentages are by weight, unless otherwise indicated. However, the scope of the present disclosure is certainly not limited to the formulations described in these examples. On the contrary, the examples are merely for illustration of the present disclosure.

[0067] The information of the raw materials used in the examples is listed in Table 1 below:

[0068] Table 1. Raw materials used in the examples

[0069]

[0070]

[0071] Example 1

[0072] In this embodiment, the basis weight is 70 g / m 2 A piece of 297 mm × 210 mm kraft paper was used as the backing layer, and Hypod 8501 was directly coated onto the surface of the backing layer using a Meyer rod to a density of 5 g / m 2 The target coating weight was set at 100°C and the coated kraft paper was then heated in a Mathis oven at 130°C for 3 minutes to form an intermediate layer on the backing layer. 2.8 g of non-vinyl polysiloxane (SYL-OFF TM SL 7028) was slowly added to 100 g of solvent-free vinyl functionalized polysiloxane (SYL-OFF TM SL 200), and then 1.5 g of Pt-siloxane composite catalyst SYL-OFF was added under vigorous stirring. TM 4000. The thus formed mixture was applied to the outer surface of the intermediate layer by using a Meyer rod, and then heated in an oven at 120° C. for 30 seconds, thereby forming a dry coating weight of 2 g / m 2 Anti-stick layer.

[0073] Example 2 to Example 3

[0074] In these examples, the procedure of Example 1 was repeated, intending to vary the formulations for the release layer according to those shown in Table 2.

[0075] Comparative Example 1

[0076] Comparative Example 1 A piece of uncoated kraft paper measuring 297 mm x 210 mm was provided.

[0077] Comparative Example 2

[0078] In this comparative example, a 10 μm PE coating is applied (by extrusion coating technology) to the surface of a piece of 297 mm×210 mm kraft paper to produce PEK (PE coated kraft paper). PEK has been widely used in the prior art as a backing layer or release liner in many commercially available products (such as adhesive tapes or adhesive labels), and is therefore used in Comparative Examples 2 and 3 to illustrate the technical effects of the embodiments of the present invention.

[0079] Comparative Example 3

[0080] In Comparative Example 3, 2.8 g of non-vinyl polysiloxane (SYL-OFF TM SL 7028) was slowly added to 100 g of solvent-free vinyl functionalized polysiloxane (SYL-OFF TM SL 200), and then 1.5 g of Pt-siloxane composite catalyst SYL-OFF was added under vigorous stirring. TM 4000. The thus formed mixture was applied to the outer surface of PEK by using a Meyer rod, and then heated in an oven at 120° C. for 30 seconds, thereby forming a dry coating weight of 2 g / m 2 Anti-stick layer.

[0081] Comparative Example 4

[0082] In Comparative Example 4, a 297 mm×210 mm piece of PEK prepared from Comparative Document 2 was used as a backing layer, and Hypod 8501 was directly coated onto the surface of the backing layer to a thickness of 5 g / m 2 by using a Meyer rod. 2 The target coating weight was 200 Å and the coated PEK was then heated in a Mathis oven at a temperature of 130° C. for 3 minutes. No release layer was applied.

[0083] Comparative Examples 5 to 15

[0084] In these examples, the procedure of Example 1 was repeated, the formulations of the intended release layers were varied according to those shown in Table 2, and the dry coating weight of all release layers was 2 g / m 2 .

[0085] Table 2: Formulations used in Examples (Ex.) 1 to 3 and Comparative Examples 1 to 15

[0086]

[0087]

[0088] The release liners prepared in the above-described inventive examples and comparative examples were characterized by the following techniques.

[0089] Paintability

[0090] The coatability of Examples 1 to 3 of the present invention and Comparative Examples 3 and Comparative Examples 4 to 15 was characterized by the following procedure: A bath of Formulation (A) was applied to paper (Kraft or PEK) with or without an intermediate layer as described in Table 2. If the bath can be evenly distributed and a film is formed on the surface within 5 seconds, the coatability should be reported as "Pass", otherwise the sample will be reported as "Fail".

[0091] The characterization results summarized in Table 2 show that only Examples 1 to 3 of the present invention and Comparative Examples 11 and 13 have good coatability, which indicates good compatibility between the intermediate layer and the release layer. Comparative Files 1 to 3 and Comparative File 4 were not characterized because they had no release layer or no intermediate layer.

[0092] As can be seen from the characterization results shown in Table 2, the release layer prepared with the aqueous formulation exhibited poor compatibility with the intermediate layer, and by using RHOBARR having a composition beyond the present disclosure TM The interlayer produced with 320 also exhibited poor compatibility. The comparative examples with poor coatability were not impractically usable, so they were not further characterized.

[0093] Abrasion resistance

[0094] The abrasion resistance of Examples 1 to 3 of the present invention and Comparative Examples 3, 11 and 13 is characterized by the following process:

[0095] Offline rubbing with thumb: This test is performed immediately after the release liner is prepared. Rub the release liner 10 times with a clean thumb at the center of the release layer with moderate force, then visually inspect the release layer to check if there is any scattered powder on the release layer, and draw a straight line on the surface with a marker pen to reveal any difference between the rubbed area and the unrubbed area. Samples that show neither powder nor a different appearance are given a "pass" result, otherwise they will be reported as "failed".

[0096] Rub off with thumb after curing: The release liners prepared in Examples 1 to 3 of the present invention and Comparative Examples 3, 11 and 13 were aged at ambient temperature for two days, and then rubbed 60 times with a clean thumb at a moderate force on the center of the release layer, after which the release layer was visually observed to check if there was any scattered powder on the release layer, and a straight line was drawn on the surface with a marker pen to reveal any difference between the rubbed area and the unrubbed area. Samples that showed neither powder nor a different appearance were given a "pass" result, otherwise they would be reported as "failed".

[0097] Machine rub off: This test is performed immediately after the release liner is prepared. Three φ30 mm samples are cut from the release liner, and a blank sample (without release layer) of the same size is also cut. The release coating weight of the sample is measured with an Oxford 8000 with the blank sample calibrated, and the measurement data is recorded as the coating weight before rubbing (in g / m 2 The sample was fixed on a platen and rubbed with a friction head for 30 cycles under a load of 1 kg. The anti-stick coating weight was then measured again with Oxford 8000 and recorded as the coating weight before rubbing (in g / m 2 The retention rate percentage (RO) can be calculated by the following equation:

[0098] Retention rate (%) = (coating weight after friction / coating weight before friction) × 100%

[0099] The measurement of each Example or Comparative Example was repeated three times, and the average results are summarized in Table 3 below.

[0100] Subsequent bond strength (SAS)

[0101] Characterize SAS according to Finat standard test method FTM 11.

[0102] Specifically, the pressure-sensitive adhesive tape Nitto 31B was laminated to the release layer of the release liner, and the laminated sample was pressed twice with a FINAT roller at a rolling rate of 10 mm / sec. The sample was placed on glass and 2The laminate was covered with a flat metal plate under a load of , and then kept at a temperature of 70 ° C for 20 hours to ensure close contact between the adhesive and the release layer. The sample was taken out and kept at ambient temperature for 1 hour. The Nitto 31B adhesive tape was peeled off from the release liner, laminated to a PET film, and pressed twice with a FINAT roller at a rolling rate of 10 mm / second. The laminate was kept under ambient conditions for 1.5 hours, after which the laminate was fixed to an AR-1500 tensile tester, and the peel strength was measured by peeling the sample at an angle of 180 ° at a clamp separation rate of 300 mm / minute. The above procedure was repeated three times, and the average result was reported as the "average adhesion on the test sample".

[0103] Additionally, the above procedure was further repeated three times by laminating the Nitto 31B adhesive tape onto blank Teflon, and the average result was reported as "Average Adhesion on Blank Teflon".

[0104] SAS can calculate it by the following equation

[0105] SAS (%) = (average adhesion on the test sample / average adhesion on the blank Teflon) x 100%.

[0106] The SAS characterization results are summarized in Table 3.

[0107] Peel force

[0108] The peel force was measured according to Finat standard test method FTM 10.

[0109] The release liners prepared in the above examples and comparative examples were kept at 23°C or 70°C for two days. Tesa7475 adhesive tape was laminated to the release layer of the release liner, and the laminated sample was pressed twice with a FINAT roller at a rolling rate of 10 mm / sec. The sample was placed on glass and 2 The laminate was covered with a flat metal plate under a load of , and then kept at a temperature of 70°C for 20 hours to ensure close contact between the adhesive and the release layer. The sample was taken out and kept at ambient temperature for 1 hour, after which the laminate was fixed on an AR-1500 tensile tester and the peel force was measured by peeling the sample at an angle of 180° at a clamp separation rate of 300 mm / min. The above procedure was repeated three times, and the average result was reported as "peel force at 23°C" or "peel force at 70°C" in g / inch.

[0110] Table 3: Friction resistance of Examples (Ex.) 1 to 3 and Comparative Examples (Co.Ex.) 3, 11, and 13 and adhesion / peel properties

[0111]

[0112] From the characterization results summarized in Table 3, it can be seen that all of the inventive examples can exhibit excellent abrasion resistance, suitable adhesion / peeling properties of adhesive tapes, and good anti-aging properties compared to the comparative examples.

[0113] Repulpability

[0114] The repulpability of each release liner is measured by weighing 25 grams of release liner sample and adding it to 2 liters of water. The sample is blended and disintegrated with conventional blender blades at a stirring rate of 3000rpm and a temperature of 50°C for 10 minutes. The dispersion is then filtered through a sieve with a mesh size of 0.010 inches. The solid residue captured on the sieve is rinsed with a small amount of deionized (DI) water, dried at 60°C for 2 hours, and weighed to calculate the percentage of insolubles. The results are recorded in Table 4 as sieving residue %, wherein higher percentage values ​​indicate more insoluble and poorer repulpability.

[0115] Table 4 Repulpability of Examples (Ex.) 1 to 3 and Comparative Examples 2 to 3, Comparative Example 11, and Comparative Example 13 Chemical .

[0116]

[0117] From the results shown in Table 4, it can be seen that all the release liners prepared using Examples 1 to 3 of the present invention exhibited better repulpability than the comparative examples.

[0118] In summary, the present disclosure has developed formulations for release layers and intermediate layers of release liners, and the combination of these two layers has achieved excellent repulpability, coatability, and good mechanical properties such as friction resistance, adhesive strength, peel force, etc.

Claims

1. A composite composition for preparing a repulpable release liner, the composite composition comprising: (A) a first formulation comprising a vinyl-functionalized polysiloxane, a non-vinyl polysiloxane, and a noble metal-siloxane composite catalyst; and (B) a second formulation comprising at least one olefin (co)polymer and at least one olefin-(meth)acrylic acid copolymer; wherein the first formulation is independent of the second formulation.

2. The combined composition according to claim 1, wherein the first formulation is solvent-free.

3. The combined composition according to claim 1, wherein the vinyl functionalized polysiloxane is represented by formula (1): [Vi(R 2 )2SiO 1 / 2 ] m -(SiO 4 / 2 ) n -(R 3 SiO 3 / 2 ) p -[(R 4 )2SiO 2 / 2 ] q -[(R 5 )3SiO 1 / 2 ] r Formula (1) Where R 2 , R 3 , R 4 and R 5 Each of which is independently selected from the group consisting of: H, C1-C 16 Alkyl groups and C1-C 16 Alkoxy groups and combinations thereof, subscript m is an integer from 1 to 100, each of subscripts n, p, q and r is independently an integer from 0 to 500, and 3≤n+p+q+r≤2000.

4. The combination composition according to claim 1, wherein the non-vinyl polysiloxane is represented by formula (3): [(R 6 )3SiO 1 / 2 ] a -(SiO 4 / 2 ) b -(R 7 SiO 3 / 2 ) c -[(R 8 )2SiO 2 / 2 ] d Formula (3) Where R6 , R 7 and R 8 Each of which is independently selected from the group consisting of: H, C1-C 16 Alkyl groups, C1-C 16 Alkoxy groups and combinations thereof; subscript a is an integer from 2 to 100, each of subscripts b, c and d is independently an integer from 0 to 200, and 3≤a+b+c+d≤800.

5. The composite composition according to claim 1, wherein the noble metal-siloxane composite catalyst comprises at least one noble metal and a siloxane ligand, wherein the noble metal is selected from the group consisting of Pt, Pd, Ru, Rh, Os, Ir, Ag, alloys thereof and mixtures thereof, and the siloxane ligand is optionally one or more selected from hydrogen, C1-C 16 Alkyl, C1-C 16 Alkoxy, C2-C 16 The substituent group is a monosiloxane, a disiloxane, a trisiloxane or a tetrasiloxane.

6. The combination composition according to claim 1, wherein the first formulation comprises, based on the total weight of the first formulation, 80 wt % to 99 wt % of the vinyl-functionalized polysiloxane, 0.05 wt % to 10 wt % of the non-vinyl polysiloxane, and 0.05 wt % to 10 wt % of the noble metal-siloxane composite catalyst.

7. The combination composition according to claim 1, wherein The olefin (co)polymer is C2-C 16 Homopolymers of olefins, two or more C2-C 16 Copolymers of olefins or at least one C2-C 16 A copolymer of an olefin and at least one vinyl comonomer; and The olefin-(meth)acrylic acid copolymer is at least one C2-C 16 The copolymer of olefin and at least one (meth) acrylic acid monomer, and the (meth) acrylic acid monomer includes methacrylic acid, acrylic acid, methacrylamide, acrylamide, methacrylonitrile, acrylonitrile, methacrylic acid (C1-C 12 ) alkyl esters, acrylic acid (C1-C 12 ) alkyl esters and any combination thereof.

8. The combination composition according to claim 1, wherein the second formulation comprises, based on the total weight of the second formulation, 10-50 wt% of the olefin (co)polymer, 2-30 wt% of the olefin-(meth)acrylic acid copolymer and 30-75 wt% of water.

9. A repulpable release liner prepared using the combined composition according to any one of claims 1 to 8, the repulpable release liner comprising (I) a release layer formed using the first preparation; (II) an intermediate layer formed with the second formulation; as well as (III) Backing layer.

10. The repulpable release liner of claim 9, wherein The backing layer is made of a repulpable material selected from the group consisting of kraft paper, coated kraft paper, pressure sensitive paper, glassine paper, coated glassine paper, gummed paper, recycled paper, polylactic acid, polybutylene succinate / caproate, polyhydroxybutyrate / valerate, polyvinyl succinate, polycaprolactone, starch, modified cellulose, and any combination thereof.

Citation Information

Patent Citations

  • Thick film pressure sensitive adhesive and laminated structure made therefrom

    CN103764784A

  • Improvements relating to adherent surfaces

    CN1042170A

  • Adhesive tape

    CN1732241A

  • Silicone-Self-Adhesives, Method of Production, Complexes Using Them and Their Uses

    US20110189422A1

  • Pressure-sensitive adhesive release liner

    US5084317A