Thermoplastic elastomer composition for multilayer molding, multilayer molded article, and method for producing multilayer molded article
By combining hydrogenated block copolymers, polypropylene resins, and non-aromatic plasticizers in specific proportions, the problems of odor and coloring in thermoplastic elastomer compositions during heat processing are solved, the adhesion strength to polar thermoplastic resins is enhanced, and it is suitable for multilayer molded parts.
Patent Information
- Application Number
- CN202380031787.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-05-18
- Filing Date
- 2023-04-20
- Publication Date
- 2024-11-22
AI Technical Summary
Existing thermoplastic elastomer compositions produce irritating odors and discoloration problems during thermal processing, and their adhesion strength to thermoplastic resins containing polar groups is insufficient, affecting their application in fields such as medical and automotive interiors.
A combination of hydrogenated block copolymers, polypropylene resins, and non-aromatic plasticizers in a specific ratio is used to form a multilayer molded body through injection molding and hot-melting. The hydrogenated block copolymers do not contain modified groups to avoid odor and coloring, and enhance the bonding strength.
This invention achieves a thermoplastic elastomer composition with good odor and color, excellent formability and thermal bonding strength, suitable for multilayer moldings, and improves the bonding strength and mechanical strength with thermoplastic resins containing polar groups.
Smart Images

Figure BDA0005066719310000591 
Figure BDA0005066719310000601 
Figure BDA0005066719310000611
Abstract
Description
Technical Field
[0001] The present invention relates to a thermoplastic elastomer composition for multilayer molding, a multilayer molded body, and a method for producing the multilayer molded body. Background Art
[0002] Thermoplastic resins containing polar groups, which are called engineering plastics, have been used in various fields due to their excellent heat resistance and mechanical properties. For example, the thermoplastic resin containing polar groups is often used as a substrate, and a soft material is bonded to the surface or part of the substrate to form a multilayer molded body. Examples include automotive interior skins, handles, cushioning materials, gaskets and other sealing parts.
[0003] Examples of the bonding method for the soft material and the base material of the thermoplastic resin containing a polar group include a bonding method using an adhesive and a bonding method by thermal fusion during molding.
[0004] In the method using an adhesive, a soft material and a base material can be firmly bonded together by the adhesive, but a step of curing the adhesive is required in addition to the step of applying the adhesive, which has a problem of reducing production speed.
[0005] On the other hand, as a bonding method using heat fusion, there can be mentioned a bonding method using injection molding such as insert molding, two-color molding, etc. In these bonding methods based on injection molding, heat fusion can be performed simultaneously with molding, so the production speed can be greatly improved. In recent years, bonding methods using heat fusion using injection molding have increased.
[0006] However, in the bonding method based on thermal bonding, the affinity of the soft material to be bonded to the substrate of the thermoplastic resin containing a polar group becomes an important factor, and when a non-polar composition is used as the soft material, there is a problem that the bonding strength becomes weak. Therefore, in order to improve the bonding strength, a thermal bonding composition containing a modified component having a functional group as a soft material and a bonded body using the composition are proposed.
[0007] For example, Patent Document 1 discloses a thermoplastic elastomer composition containing a hydrogenated thermoplastic styrene elastomer, a hydrocarbon rubber softener, polypropylene, a thermoplastic polyurethane elastomer, and an acid-modified hydrogenated styrene elastomer.
[0008] Patent Document 2 discloses a thermoplastic polymer composition containing a thermoplastic elastomer, a polyvinyl acetal resin and / or a polypropylene resin containing a polar group, and a bonded body containing the thermoplastic polymer composition and an insert component.
[0009] Prior art literature
[0010] Patent Literature
[0011] Patent Document 1: Japanese Patent Application Publication No. 2009-209273
[0012] Patent Document 2: Japanese Patent Application Publication No. 2014-168940 Summary of the invention
[0013] Problems to be solved by the invention
[0014] However, the thermoplastic elastomer composition disclosed in Patent Document 1, although containing a maleic anhydride-modified styrene elastomer as the acid-modified hydrogenated styrene elastomer, generates irritating odor during heat processing or in a molded article thereafter. Therefore, it is not suitable for medical applications, automotive interior materials, residential materials, and other uses where people stay for a long time. In addition, when acid-modified, there are problems such as an increase in the number of modification steps or unreacted free maleic acid remaining as impurities, which in turn causes coloration due to oligomers of maleic acid.
[0015] In addition, the thermoplastic polymer composition disclosed in Patent Document 2 contains a polyvinyl acetal resin and / or a polypropylene resin containing a polar group. The side chain of the polyvinyl acetal resin is easily detached during heat processing, and a strong odor is generated due to its decomposition reaction, so there is a problem of a very bad working environment. In addition, the polypropylene resin containing a polar group is acid-modified with maleic anhydride, and has the problem of generating a pungent odor like the thermoplastic elastomer composition disclosed in Patent Document 1.
[0016] As described above, conventionally proposed thermoplastic elastomer compositions or thermal adhesive compositions composed of thermoplastic polymer compositions have problems that still need to be improved in terms of odor, coloration, and the like.
[0017] Therefore, in view of the above-mentioned problems of the prior art, an object of the present invention is to provide a thermoplastic elastomer composition and a multilayer molded product which are good in practical use in terms of odor and color tone and excellent in moldability, thermal adhesive strength and mechanical strength.
[0018] Means for solving problems
[0019] The present inventors have conducted intensive studies to solve the problems of the prior art and have found that a thermoplastic elastomer composition containing a hydrogenated block copolymer having a predetermined structure, a polypropylene resin, and a non-aromatic softener in a predetermined ratio can solve the problems of the prior art, thereby completing the present invention.
[0020] That is, the present invention is as follows. [1]
[0022] A thermoplastic elastomer composition for multilayer molding, which is a thermoplastic elastomer composition for multilayer molding that is heat-welded by injection molding, comprising:
[0023] 100 parts by mass of a hydrogenated block copolymer (a-1);
[0024] 10 to 100 parts by mass of a polypropylene resin (b); and
[0025] 50 to 300 parts by weight of a non-aromatic softener (c),
[0026] further comprising a hydrogenated block copolymer (a-2), wherein the hydrogenated block copolymer (a-1) and the hydrogenated block copolymer (a-2) are both unmodified hydrogenated block copolymers,
[0027] in,
[0028] The content of the hydrogenated block copolymer (a-2) is 5 to 70% by mass based on the total amount of the components (a-1), (a-2), (b), and (c).
[0029] The hydrogenated block copolymer (a-1) satisfies the following conditions (1-1) to (1-4),
[0030] The hydrogenated block copolymer (a-2) satisfies the following conditions (2-1) to (2-6).
[0031] (1-1): Contains one or more polymer blocks A1 mainly composed of vinyl aromatic monomer units, and one or more polymer blocks B1 mainly composed of conjugated diene monomer units.
[0032] (1-2): The content of all vinyl aromatic monomer units is 15% by mass or more and less than 35% by mass.
[0033] (1-3): The weight average molecular weight is 150,000 to 550,000.
[0034] (1-4): 50 mol% or more of the double bonds of the conjugated diene monomer units are hydrogenated.
[0035] (2-1): Contains one or more polymer blocks A2 mainly composed of vinyl aromatic monomer units and one or more polymer blocks B2 mainly composed of conjugated diene monomer units.
[0036] (2-2): The content of the vinyl aromatic monomer unit in the polymer block A2 is 50% by mass or more.
[0037] (2-3): The content of all vinyl aromatic monomer units is 35% to 70% by mass.
[0038] (2-4): The weight average molecular weight is 30,000 or more and less than 150,000.
[0039] (2-5): The amount of vinyl bonds in the conjugated diene monomer units in the polymer block B2 before hydrogenation is 60 mol% to 95 mol%.
[0040] (2-6): 50 mol% or more of the double bonds of the conjugated diene monomer units are hydrogenated. [2]
[0042] The thermoplastic elastomer composition for multilayer molding as described in [1] above, wherein
[0043] The above hydrogenated block copolymer (a-2):
[0044] It has at least two polymer blocks A2 mainly composed of vinyl aromatic monomer units, and at least two polymer blocks B2 mainly composed of conjugated diene monomer units,
[0045] At least one of the polymer blocks B2 is located at the terminal of the hydrogenated block copolymer (a-2), and the content of the polymer block B2 located at the terminal is 1 to 10% by mass in the hydrogenated block copolymer (a-2).
[0046] There is no peak having a weight average molecular weight of 250,000 or more. [3]
[0048] The thermoplastic elastomer composition for multilayer molding as described in [1] or [2] above, wherein the content of the vinyl aromatic monomer unit in the polymer block A2 of the hydrogenated block copolymer (a-2) is 90% by mass or more. [4]
[0050] The thermoplastic elastomer composition for multilayer molding as described in any one of the above [1] to [3], wherein the content of all vinyl aromatic monomer units in the hydrogenated block copolymer (a-2) is more than 40% by mass and not more than 70% by mass. [5]
[0052] The thermoplastic elastomer composition for multilayer molding as described in any one of the above [1] to [4], wherein in the hydrogenated block copolymer (a-1), the amount of vinyl bonds in the conjugated diene monomer units before hydrogenation is 30 mol% to 50 mol%. [6]
[0054] A multilayer molded body comprising:
[0055] A layer of the thermoplastic elastomer composition for multilayer molding according to any one of the above [1] to [5], and
[0056] A thermoplastic resin layer containing polar groups. [7]
[0058] A multilayer molded body comprising:
[0059] a thermoplastic resin layer containing polar groups; and
[0060] A thermoplastic elastomer composition layer comprising a hydrogenated block copolymer (a), a polypropylene resin (b) and a non-aromatic softener (c),
[0061] in,
[0062] The thermoplastic elastomer composition layer is provided in contact with the polar group-containing thermoplastic resin layer.
[0063] The hydrogenated block copolymer (a) does not contain a modifying group.
[0064] The above hydrogenated block copolymer (a):
[0065] A hydrogenated block copolymer which is a hydrogenated product of a block copolymer having a vinyl aromatic monomer unit and a conjugated diene monomer unit,
[0066] The molecular weight peaks based on GPC are 30,000 to less than 150,000 and 150,000 to 550,000, respectively, and there are at least one peak.
[0067] The hydrogenated block copolymer having a molecular weight peak of 30,000 to less than 150,000 based on GPC has a total vinyl aromatic monomer unit content of 35% to 70% by mass, and a vinyl bond content before hydrogenation in the conjugated diene monomer unit of 60% to 95% by mole.
[0068] The hydrogenated block copolymer having a molecular weight peak of 150,000 to 550,000 based on GPC has a total vinyl aromatic monomer unit content of 15% to less than 35% by mass.
[0069] The hydrogenation rate of double bonds in the conjugated diene monomer units is 50 mol% or more. [8]
[0071] The multilayer molded body as described in the above-mentioned [7], wherein
[0072] The hydrogenated block copolymer (a) is composed of a hydrogenated block copolymer (a-1) and a hydrogenated block copolymer (a-2).
[0073] The above (a-1) satisfies the following conditions (1-1) to (1-4),
[0074] The above (a-2) satisfies the following conditions (2-1) to (2-6),
[0075] The thermoplastic elastomer composition layer contains 100 parts by mass of the above (a-1), 10 to 100 parts by mass of the above (b), and 50 to 300 parts by mass of the above (c).
[0076] The content of the (a-2) in the thermoplastic elastomer composition layer is 5 to 70% by mass based on the total amount of the components (a-1), (a-2), (b), and (c).
[0077] (1-1): Contains one or more polymer blocks A1 mainly composed of vinyl aromatic monomer units, and one or more polymer blocks B1 mainly composed of conjugated diene monomer units.
[0078] (1-2): The content of all vinyl aromatic monomer units is 15% by mass or more and less than 35% by mass.
[0079] (1-3): The weight average molecular weight is 150,000 to 550,000.
[0080] (1-4): 50 mol% or more of the double bonds of the conjugated diene monomer units are hydrogenated.
[0081] (2-1): Contains one or more polymer blocks A2 mainly composed of vinyl aromatic monomer units and one or more polymer blocks B2 mainly composed of conjugated diene monomer units.
[0082] (2-2): The content of the vinyl aromatic monomer unit in the polymer block A2 is 50% by mass or more.
[0083] (2-3): The content of all vinyl aromatic monomer units is 35% to 70% by mass.
[0084] (2-4): The weight average molecular weight is 30,000 or more and less than 150,000.
[0085] (2-5): The amount of vinyl bonds in the conjugated diene monomer units in the polymer block B2 before hydrogenation is 60 mol% to 95 mol%.
[0086] (2-6): 50 mol% or more of the double bonds of the conjugated diene monomer units are hydrogenated. [9]
[0088] The multilayer molded article as described in the above [8], wherein the hydrogenated block copolymer (a-2) is:
[0089] The hydrogenated block copolymer (a-2) comprises at least two polymer blocks A2 mainly composed of vinyl aromatic monomer units and at least two polymer blocks B2 mainly composed of conjugated diene monomer units, at least one of the polymer blocks B2 is located at the end of the hydrogenated block copolymer (a-2), and the content of the polymer block B2 located at the end is 1 to 10% by mass in the hydrogenated block copolymer (a-2).
[0090] The content of all vinyl aromatic monomer units is greater than 40% by mass and less than 70% by mass,
[0091] There is no peak having a weight average molecular weight of 250,000 or more.
[10]
[0093] The multilayer molded product as described in [8] or [9] above, wherein the content of the vinyl aromatic monomer unit in the polymer block A2 of the hydrogenated block copolymer (a-2) is 90% by mass or more.
[11]
[0095] The multilayer molded body as described in any one of [6] to
[10] above, wherein the polar group-containing thermoplastic resin is at least one selected from the group consisting of polycarbonate resins, ABS resins, polyester resins, acrylic resins, and mixtures thereof.
[12]
[0097] The multilayer molded product as described in any one of [8] to
[11] above, wherein in the hydrogenated block copolymer (a-1), the amount of vinyl bonds in the conjugated diene monomer units before hydrogenation is 30 mol% to 50 mol%.
[13]
[0099] A thermoplastic elastomer composition, which is a thermoplastic elastomer composition used in the multilayer molded body described in any one of [6] to
[12] above, wherein in the multilayer molded body, the polar group-containing thermoplastic resin layer and the thermoplastic elastomer composition layer are heat-fused by injection molding.
[14]
[0101] A method for producing a multilayer molded body, which is the method for producing a multilayer molded body described in any one of [6] to
[13] above, comprising the following steps:
[0102] The step of molding the thermoplastic resin containing polar groups to obtain a molded body;
[0103] With the molded body placed in the mold, the thermoplastic elastomer composition described in
[13] is injected into the gap between the mold and the molded body to perform heat fusion bonding.
[0104] Effects of the Invention
[0105] According to the present invention, a thermoplastic elastomer composition and a multilayer laminate can be obtained which are practically good in terms of odor and color tone and are excellent in moldability, thermal adhesive strength and mechanical strength. DETAILED DESCRIPTION
[0106] A specific embodiment of the present invention (hereinafter referred to as “this embodiment”) will be described in detail below.
[0107] It should be noted that the following embodiments are examples for explaining the present invention, and the present invention is not limited to the following contents. The present invention can be implemented with various modifications within the scope of the gist thereof.
[0108] [Thermoplastic elastomer composition]
[0109] The thermoplastic elastomer composition of the present embodiment is a thermoplastic elastomer composition for multilayer molding to be heat-fused with other parts by injection molding, and contains:
[0110] 100 parts by mass of a hydrogenated block copolymer (a-1);
[0111] 10 to 100 parts by mass of a polypropylene resin (b); and
[0112] 50 to 300 parts by weight of a non-aromatic softener (c),
[0113] It further contains a hydrogenated block copolymer (a-2), and both the hydrogenated block copolymer (a-1) and the hydrogenated block copolymer (a-2) are unmodified hydrogenated block copolymers.
[0114] The content of the hydrogenated block copolymer (a-2) is 5 to 70% by mass based on the total amount of the components (a-1), (a-2), (b), and (c).
[0115] The hydrogenated block copolymer (a-1) satisfies the following conditions (1-1) to (1-4), and the hydrogenated block copolymer (a-2) satisfies the following conditions (2-1) to (2-6).
[0116] (1-1): Contains one or more polymer blocks A1 mainly composed of vinyl aromatic monomer units, and one or more polymer blocks B1 mainly composed of conjugated diene monomer units.
[0117] (1-2): The content of all vinyl aromatic monomer units is 15% by mass or more and less than 35% by mass.
[0118] (1-3): The weight average molecular weight is 150,000 to 550,000.
[0119] (1-4): 50 mol% or more of the double bonds of the conjugated diene monomer units are hydrogenated.
[0120] (2-1): Contains one or more polymer blocks A2 mainly composed of vinyl aromatic monomer units and one or more polymer blocks B2 mainly composed of conjugated diene monomer units.
[0121] (2-2): The content of the vinyl aromatic monomer unit in the polymer block A2 is 50% by mass or more.
[0122] (2-3): The content of all vinyl aromatic monomer units is 35% to 70% by mass.
[0123] (2-4): The weight average molecular weight is 30,000 or more and less than 150,000.
[0124] (2-5): The amount of vinyl bonds in the conjugated diene monomer units in the polymer block B2 before hydrogenation is 60 mol% to 95 mol%.
[0125] (2-6): 50 mol% or more of the double bonds of the conjugated diene monomer units are hydrogenated.
[0126] By having the above-mentioned constitution, it is possible to obtain a thermoplastic elastomer composition which is good in practical terms in terms of odor and color tone and is excellent in moldability, thermal adhesive strength, and mechanical strength.
[0127] Each component is described in detail below.
[0128] (Hydrogenated block copolymer (a-1))
[0129] The thermoplastic elastomer composition of the present embodiment contains the hydrogenated block copolymer (a-1).
[0130] The hydrogenated block copolymer (a-1) is obtained by hydrogenating a block copolymer comprising one or more polymer blocks A1 mainly composed of vinyl aromatic monomer units and one or more polymer blocks B1 mainly composed of conjugated diene monomer units (the above condition (1-1)).
[0131] The hydrogenated block copolymer (a-1) is a so-called "unmodified" copolymer having no functional group other than that derived from a vinyl aromatic compound or a conjugated diene compound. By being unmodified, impurities from unreacted products are not mixed in, and a copolymer with little odor can be obtained.
[0132] It should be noted that the term “unmodified” excludes the case where the hydrogenated block copolymer (a-1) contains a modified group formed by a predetermined modifier. In the case where the hydrogenated block copolymer (a-1) is a substance obtained by a coupling reaction using a coupling agent, it is deemed to satisfy the condition of “unmodified” if it has Si atoms and O atoms derived from the coupling agent.
[0133] Thus, in the present embodiment, the atomic group having heteroatoms is distinguished as existing in the form of a coupling agent residue or introduced by a modifier, and it is believed that the following tendency has an influence in this context, that is, the coupling agent residue is easily located in the center of the copolymer, and on the other hand, in the case of a modifier, it is easy to be introduced to the end or side chain of the copolymer. In order to provide a thermoplastic elastomer composition with good odor and color tone in practical use, it is preferred that the functional group is less free, but in the case of a residue introduced into the center in the form of a coupling agent, the polymer chain end will be bonded to the functional group due to the coupling reaction, and / or steric hindrance based on the copolymer chain will occur, so there is a tendency that the functional group is not easy to be free. In contrast, when the modifier is reacted with the end or side chain of the copolymer, the functional group is easily freed, and there is a tendency that it is easy to cause odor or color tone. In particular, in the case of so-called secondary modified products in which a copolymer and a modifier are mixed and reacted using an extruder, maleic anhydride, epoxy, and the like are often used to introduce a modifying group. In such cases, carboxyl-containing compounds and epoxy-containing compounds are easily separated, which tends to cause odor and color tone. In addition, in the case of a coupling reaction at the polymerization termination end, unreacted products can be largely removed in the subsequent finishing process of the copolymer such as desolvation. In contrast, in the case of secondary modified products, it is difficult to completely remove them, and there tends to be a large amount of unreacted residues. From this point of view, it is also easy to give odor and color tone.
[0134] Conventionally, modification was performed for the purpose of improving adhesion to other components, but the present inventors have conceived a scheme that the structure of the hydrogenated block copolymer can be designed so as to ensure good adhesion even without modification. The structure of the hydrogenated block copolymer (a-2) described later mainly exerts the effect of facilitating heat fusion with other components in multilayer molding.
[0135] The modified groups of the hydrogenated block copolymer can be confirmed by NMR analysis and IR analysis.
[0136] The above-mentioned polymer block A1 mainly composed of vinyl aromatic monomer units means that the content of vinyl aromatic monomer units in the polymer block A1 is greater than 50% by mass. From the perspective of mechanical strength and heat deformation resistance, it is preferably 60% by mass or more, more preferably 70% by mass or more, further preferably 80% by mass or more, and further more preferably 90% by mass or more.
[0137] Similarly, the polymer block B1 mainly composed of conjugated diene monomer units means that the content of the conjugated diene monomer units in the polymer block B1 is greater than 50% by mass, and is preferably 60% by mass or more, more preferably 70% by mass or more, further preferably 80% by mass or more, and further more preferably 90% by mass or more from the perspective of flexibility and softener retention.
[0138] It should be noted that, in the present embodiment, the naming of each monomer unit constituting the block copolymer is based on the naming of the monomer from which the monomer unit is derived. For example, a "vinyl aromatic monomer unit" refers to a structural unit of a polymer produced by polymerizing a vinyl aromatic compound as a monomer, and its structure is a molecular structure in which two carbon atoms of a substituted ethylene group derived from a substituted vinyl group serve as bonding sites.
[0139] The "conjugated diene monomer unit" refers to a structural unit of a polymer produced by polymerizing a conjugated diene compound as a monomer, and has a molecular structure in which two carbon atoms derived from an olefin of the conjugated diene compound serve as bonding sites.
[0140] In the present embodiment, the vinyl aromatic compound that can be used to form the vinyl aromatic monomer unit in the polymer block A1 refers to a compound having a vinyl group and an aromatic ring.
[0141] Examples of the vinyl aromatic compound include, but are not limited to, styrene, α-methylstyrene, p-methylstyrene, divinylbenzene, 1,1-diphenylethylene, N,N-dimethyl-p-aminoethylstyrene, N,N-diethyl-p-aminoethylstyrene, etc. Among these, styrene, α-methylstyrene, and divinylbenzene are preferably used from the perspective of polymerizability. These vinyl aromatic compounds may be used alone or in combination of two or more.
[0142] The conjugated diene compound that can be used to form the conjugated diene monomer unit in the polymer block B1 refers to a diene having one pair of conjugated double bonds (two double bonds bonded in a conjugated manner).
[0143] As conjugated diene compounds, for example, 1,3-butadiene, 2-methyl-1,3-butadiene (isoprene), 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, 2-methyl-1,3-pentadiene, 1,3-hexadiene, etc. can be cited but are not limited thereto. Among these, from the aspect of polymerizability, 1,3-butadiene and 2-methyl-1,3-butadiene (isoprene) are preferably used. These conjugated diene compounds can be used alone or in combination of two or more.
[0144] The hydrogenated block copolymer (a-1) has, but is not limited to, structures represented by the following general formulae (1) to (7). The hydrogenated block copolymer (a-1) may be a mixture of copolymers having structures represented by the following general formulae (1) to (7) in any proportion.
[0145] (A1-B1) n (1)
[0146] A1-(B1-A1) n (2)
[0147] B1-(A1-B1) n (3)
[0148] [(B1-A1) n ] m -Z(4)
[0149] [(A1-B1) n ] m -Z(5)
[0150] [(B1-A1) n -B1] m -Z(6)
[0151] [(A1-B1) n -A1] m -Z(7)
[0152] In general formulae (1) to (7), A1 is a polymer block mainly composed of vinyl aromatic monomer units, and B1 is a polymer block mainly composed of conjugated diene monomer units. The boundary between polymer block A1 and polymer block B1 does not necessarily need to be clearly distinguished.
[0153] In addition, n is an integer of 1 or more, and preferably an integer of 1-5.
[0154] m is an integer of 2 or more, preferably an integer of 2-11, and more preferably an integer of 2-8.
[0155] Z represents a coupling agent residue. Here, the coupling agent residue refers to the residue after bonding of a coupling agent used to bond a plurality of copolymers of conjugated diene monomer units and vinyl aromatic monomer units between polymer blocks A1-polymer blocks A1, between polymer blocks B1-polymer blocks B1, or between polymer blocks A1-polymer blocks B1. Examples of the coupling agent include, but are not limited to, halogenated silicon compounds and acid esters described below.
[0156] In the general formulae (1) to (7), the vinyl aromatic monomer units in the polymer block A1 and the polymer block B1 may be uniformly distributed or may be distributed in a tapered manner.
[0157] In addition, when polymer block A1 and polymer block B1 are copolymer blocks of vinyl aromatic monomer units and conjugated diene monomer units, the vinyl aromatic monomer units in the copolymer blocks may exist in a plurality of uniformly distributed portions and a portion distributed in a tapered manner. In addition, a plurality of portions having different contents of vinyl aromatic monomer units may coexist in the above copolymer block portion.
[0158] The content of all vinyl aromatic monomer units in the hydrogenated block copolymer (a-1) is 15% by mass or more and less than 35% by mass (the above condition (1-2)).
[0159] From the viewpoint of mechanical strength, flexibility, recovery and rebound resilience of the thermoplastic elastomer composition of the present embodiment, the content is preferably 17% by mass or more, more preferably 19% by mass or more, further preferably 21% by mass or more, and still further preferably 23% by mass or more.
[0160] Moreover, it is preferably 34 mass % or less, and more preferably 33 mass % or less.
[0161] Mechanical strength and resilience are properties required as material strength and prevention of deformation, and softness and rebound resilience are properties related to touch. Therefore, when the thermoplastic elastomer composition of the present embodiment is used for handles, skin materials, or sealing materials, the content of all vinyl aromatic monomer units in the hydrogenated block copolymer (a-1) is preferably designed to be within a range suitable for these uses.
[0162] When the content of all vinyl aromatic monomer units in the hydrogenated block copolymer (a-1) is 15% by mass or more, the mechanical strength and heat deformation resistance of the thermoplastic elastomer composition of the present embodiment tend to be improved, and when the content of all vinyl aromatic monomer units is less than 35% by mass, the flexibility, recovery and rebound resilience of the thermoplastic elastomer composition of the present embodiment tend to be improved. It should be noted that the content of all vinyl aromatic monomer units can be controlled within the above numerical range by adjusting the amount of monomers added in the polymerization step of the hydrogenated block copolymer (a-1), and can be calculated from the absorption intensity at 262 nm using an ultraviolet spectrophotometer by the method described in the Examples described later.
[0163] The weight average molecular weight of the hydrogenated block copolymer (a-1) is 150,000 to 550,000 (the above condition (1-3)). From the viewpoint of heat deformation resistance, it is 150,000 or more, preferably 170,000 or more, more preferably 190,000 or more, and further preferably 210,000 or more. In addition, it is preferably 500,000 or less, more preferably 450,000 or less, further preferably 400,000 or less, further more preferably 350,000 or less, and further preferably 300,000 or less.
[0164] When the weight average molecular weight of the hydrogenated block copolymer (a-1) is 150,000 or more, the thermoplastic elastomer composition of the present embodiment tends to have good heat deformation resistance and recovery. When the weight average molecular weight of the hydrogenated block copolymer (a-1) is 550,000 or less, the thermoplastic elastomer composition of the present embodiment exhibits good fluidity and sufficient molding processability can be obtained.
[0165] The molecular weight distribution (Mw / Mn) of the hydrogenated block copolymer (a-1) is preferably 1.01 to 5.0, more preferably 1.01 to 4.0, and even more preferably 1.01 to 3.0.
[0166] When the molecular weight distribution of the hydrogenated block copolymer (a-1) is 1.01 to 5.0, there is a tendency that better mechanical strength can be obtained.
[0167] The shape of the molecular weight distribution curve of the hydrogenated block copolymer (a-1) measured by gel permeation chromatography (hereinafter sometimes referred to as GPC) is not particularly limited, and may have a multimodal molecular weight distribution with two or more peaks or a unimodal molecular weight distribution with one peak.
[0168] It should be noted that the weight average molecular weight (Mw) and molecular weight distribution [Mw / Mn; ratio of weight average molecular weight (Mw) to number average molecular weight (Mn)] of the hydrogenated block copolymer (a-1) can be determined by the method described in the Examples below, based on the peak molecular weight of the chromatogram measured by gel permeation chromatography (GPC), using a calibration curve obtained by measurement of commercially available standard polystyrene (prepared using the peak molecular weight of standard polystyrene).
[0169] The microstructure (cis, trans, vinyl bond content) of the polymer block B1 in the hydrogenated block copolymer (a-1) can be arbitrarily controlled by using a regulator such as a polar compound in the polymerization step of the hydrogenated block copolymer (a-1).
[0170] The modifiers are described below.
[0171] The amount of vinyl bonds in the conjugated diene monomer units in the hydrogenated block copolymer (a-1) before hydrogenation is preferably 30 mol% or more, more preferably 31 mol% or more, further preferably 31 mol% or more, and further more preferably 32 mol% or more. The preferred upper limit is 50 mol% or less, more preferably 47 mol% or less, and further preferably 44 mol% or less.
[0172] When the amount of vinyl bonds in the conjugated diene monomer units before hydrogenation in the hydrogenated block copolymer (a-1) is 30 mol% or more, the compatibility of the hydrogenated block copolymer (a-1) with the polypropylene resin (b) described below tends to be further improved. When the amount of vinyl bonds in the conjugated diene monomer units before hydrogenation is 50 mol% or less, the mechanical strength of the thermoplastic elastomer composition of the present embodiment tends to be further improved.
[0173] It should be noted that the vinyl bond amount "before hydrogenation" in this specification is referred to as "vinyl bond" because it cannot be referred to as "vinyl bond" after hydrogenation, and it is not intended to be measured using the copolymer before hydrogenation. Since the bonding mode of the conjugated diene can also be determined by the structure after hydrogenation, the vinyl bond amount "before hydrogenation" can also be calculated by investigating the structure after hydrogenation.
[0174] It should be noted that in the present embodiment, the vinyl bond amount refers to, for example, in butadiene, before hydrogenation, the ratio of the total molar amount of the conjugated diene monomer units introduced in the bonding manner of 1,2-bond and 3,4-bond to the total molar amount of the conjugated diene monomer units introduced in the bonding manner of 1,2-bond, 3,4-bond and 1,4-bond.
[0175] It should be noted that after hydrogenation, the total molar amount of the conjugated diene monomer units introduced by the bonding mode of unhydrogenated 1,2-bond, hydrogenated 1,2-bond, unhydrogenated 3,4-bond, hydrogenated 3,4-bond, unhydrogenated 1,4-bond and hydrogenated 1,4-bond is equal to the total molar amount of the conjugated diene monomer units introduced by the bonding mode of unhydrogenated 1,2-bond, hydrogenated 1,2-bond, unhydrogenated 3,4-bond and hydrogenated 3,4-bond. Therefore, the vinyl bond amount of the conjugated diene monomer units before hydrogenation can be measured by nuclear magnetic resonance spectroscopy (NMR) using the block copolymer after hydrogenation, and specifically, it can be measured by the method described in the examples described later.
[0176] The hydrogenation rate of the aliphatic double bonds derived from the conjugated diene compound, i.e., the double bonds of the conjugated diene monomer units in the hydrogenated block copolymer (a-1) is 50% or more (the above condition (1-4)), preferably 60% or more, and more preferably 70% or more. If the hydrogenation rate is 50% or more, the thermoplastic elastomer composition of the present embodiment tends to be able to more effectively suppress the reduction of mechanical properties due to thermal degradation (oxidative degradation). In addition, if the hydrogenation rate is 70% or more, the thermoplastic elastomer composition of the present embodiment tends to obtain more excellent weather resistance. The upper limit of the hydrogenation rate is not particularly limited, but is preferably 100% or less, and more preferably 99% or less.
[0177] The hydrogenation rate of the double bonds of the conjugated diene monomer units of the hydrogenated block copolymer (a-1) can be controlled within the above numerical range by adjusting the type and amount of the hydrogenation catalyst and the hydrogenation conditions, and can be measured by the method described in the examples below.
[0178] In the thermoplastic elastomer composition of the present embodiment, by mixing the organic peroxide (e) described later, the thermoplastic elastomer composition can be partially crosslinked in the process of melt-kneading the thermoplastic elastomer composition using an extruder. The thermoplastic elastomer composition layer constituting the multilayer molded body of the present embodiment described later does not necessarily need to be crosslinked, but may be crosslinked in applications where the requirement for suppressing permanent strain is high. When the thermoplastic elastomer composition of the present embodiment is partially crosslinked using the organic peroxide (e), the hydrogenation rate of the aliphatic double bonds derived from the conjugated diene compound in the hydrogenated block copolymer (a-1) needs to be 50% or more, preferably 60% or more from the aspect of heat resistance, and preferably 90% or less, more preferably 85% or less from the aspects of processability and crosslinking reactivity.
[0179] The hydrogenation rate of the aromatic double bonds based on the vinyl aromatic monomer units in the hydrogenated block copolymer (a-1) is not particularly limited, but is preferably 50% or less, more preferably 30% or less, and even more preferably 20% or less.
[0180] (Hydrogenated block copolymer (a-2))
[0181] The thermoplastic elastomer composition of the present embodiment contains the hydrogenated block copolymer (a-2).
[0182] The hydrogenated block copolymer (a-2) is obtained by hydrogenating a block copolymer comprising one or more polymer blocks A2 mainly composed of vinyl aromatic monomer units and one or more polymer blocks B2 mainly composed of conjugated diene compound monomer units (the above condition (2-1)).
[0183] In the hydrogenated block copolymer (a-2), the content of all vinyl aromatic monomer units is 35% to 70% by mass (the above condition (2-3)). In addition, the weight average molecular weight of the hydrogenated block copolymer (a-2) is 30,000 or more and less than 150,000 (the above condition (2-4)). In addition, the amount of vinyl bonds before hydrogenation in the conjugated diene monomer units in the polymer block B2 is 60% to 95% by mole (the above condition (2-5)).
[0184] The hydrogenated block copolymer (a-2) is an unmodified block copolymer having no functional groups other than those derived from the vinyl aromatic compound and the conjugated diene compound. By making the hydrogenated block copolymer (a-2) unmodified, a thermoplastic elastomer composition having no odor or color tone and no impurities from unreacted products can be obtained.
[0185] It should be noted that the term “unmodified” excludes the case where the hydrogenated block copolymer (a-2) contains a modified group formed by a predetermined modifier. In the case where the hydrogenated block copolymer (a-2) is a substance obtained by a coupling reaction using a coupling agent, it is deemed to satisfy the condition of “unmodified” if it has Si atoms and O atoms derived from the coupling agent.
[0186] The thermoplastic elastomer composition of the present embodiment can be thermally bonded to a polar group-containing thermoplastic resin described later without using a modified copolymer by containing the hydrogenated block copolymer (a-2) having a specific structure satisfying the requirements (2-1) to (2-6).
[0187] The thermoplastic elastomer composition of the present embodiment contains a polypropylene-based resin (b) to adjust moldability and hardness. However, when thermally bonded to a thermoplastic resin containing a polar group described later, the polypropylene-based resin (b) has low affinity for the thermoplastic resin composition containing a polar group and substantially no bonding strength is exhibited.
[0188] The thermal adhesiveness of the thermoplastic elastomer composition of the present embodiment tends to be controllable by the amount of vinyl aromatic monomer units or the amount of vinyl bonds in the hydrogenated block copolymers (a-1) and (a-2). The content of the vinyl aromatic monomer in the hydrogenated block copolymer (a-2) is 35% by mass to 70% by mass (the above condition (2-3)). For example, as the amount of styrene in the hydrogenated block copolymer increases and the content of the component (a-2) in the thermoplastic elastomer composition of the present embodiment increases, the affinity with the polar group-containing thermoplastic resin described later tends to increase, and the adhesive strength tends to increase.
[0189] In the hydrogenated block copolymer (a-2), the vinyl bond content of the conjugated diene monomer unit in the polymer block B2 before hydrogenation is 60 mol% to 95 mol% (the above condition (2-5)). Within this range, the higher the vinyl bond content and the higher the ratio of the component (a-2) at the same vinyl bond content, the higher the compatibility with the polypropylene resin (b) and the more fine dispersion occurs, thereby compensating for the disadvantage of the polypropylene resin (b) that the affinity for the thermoplastic resin containing a polar group is low. That is, due to their synergistic effect, the thermal adhesiveness between the thermoplastic resin containing a polar group and the thermoplastic elastomer composition of the present embodiment is improved.
[0190] In the thermoplastic elastomer composition of the present embodiment, in addition to the hydrogenated block copolymer (a-1) and the hydrogenated block copolymer (a-2), one or more polypropylene resins (b) and non-aromatic softeners (c) are respectively contained from the aspect of improving the balance among mechanical strength, flexibility, recovery, moldability and thermal adhesiveness, and the content of the hydrogenated block copolymer (a-2) is 5 to 70% by mass relative to the total amount of the components (a-1), (a-2), (b) and (c). The preferred lower limit is 10% by mass or more, more preferably 15% by mass or more. The preferred upper limit is 65% by mass or less, more preferably 60% by mass or less.
[0191] In the hydrogenated block copolymer (a-2), the polymer block A2 mainly composed of vinyl aromatic monomer units is a polymer block A2 in which the content of the vinyl aromatic monomer units is 50% by mass or more (the above-mentioned condition (2-2)). From the viewpoint of the thermal fusion property between the thermoplastic elastomer composition of the present embodiment and the polar group-containing thermoplastic resin described later, the content is preferably 60% by mass or more, more preferably 70% by mass or more, further preferably 80% by mass or more, and further more preferably 90% by mass or more.
[0192] In the hydrogenated block copolymer (a-2), the polymer block B2 mainly composed of conjugated diene monomer units means that the content of the conjugated diene monomer units in the polymer block B2 is greater than 50% by mass, preferably 60% by mass or more, more preferably 70% by mass or more, further preferably 80% by mass or more, and further more preferably 90% by mass or more.
[0193] The vinyl aromatic compound used to form the vinyl aromatic monomer unit in the polymer block A2 refers to a compound having a vinyl group and an aromatic ring. Examples of the vinyl aromatic compound include, but are not limited to, styrene, α-methylstyrene, p-methylstyrene, divinylbenzene, 1,1-diphenylethylene, N,N-dimethyl-p-aminoethylstyrene, N,N-diethyl-p-aminoethylstyrene, etc. Among these, styrene, α-methylstyrene, and divinylbenzene are suitable from the perspective of polymerizability. These vinyl aromatic compounds may be used alone or in combination of two or more.
[0194] The conjugated diene compound used to form the conjugated diene monomer unit in the polymer block B2 refers to a diene having a pair of conjugated double bonds (two double bonds bonded in a conjugated manner). As the conjugated diene compound, for example, 1,3-butadiene, 2-methyl-1,3-butadiene (isoprene), 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, 2-methyl-1,3-pentadiene, 1,3-hexadiene, etc. can be cited but not limited to. Among these, from the aspect of polymerizability, 1,3-butadiene and 2-methyl-1,3-butadiene (isoprene) are suitable for use. These conjugated diene compounds can be used alone or in combination.
[0195] The hydrogenated block copolymer (a-2) has, but is not limited to, structures represented by the following general formulae (8) to (14). The hydrogenated block copolymer (a-2) may be a mixture containing a plurality of structures represented by the following general formulae (8) to (14) in any proportion.
[0196] (A2-B2) n (8)
[0197] A2-(B2-A2) n (9)
[0198] B2-(A2-B2) n (10)
[0199] [(B2-A2) n ] m -Z(11)
[0200] [(A2-B2) n ] m -Z(12)
[0201] [(B2-A2) n -B2] m -Z(13)
[0202] [(A2-B2) n -A2] m -Z(14)
[0203] In general formulae (8) to (14), A2 is a polymer block mainly composed of vinyl aromatic monomer units, and B2 is a polymer block mainly composed of conjugated diene monomer units. The boundary between polymer block A2 and polymer block B2 does not necessarily need to be clearly distinguished.
[0204] In addition, n is an integer of 1 or more, and preferably an integer of 1-5.
[0205] m is an integer of 2 or more, preferably an integer of 2-11, and more preferably an integer of 2-8.
[0206] Z represents a coupling agent residue. Here, the coupling agent residue refers to the residue after bonding of a coupling agent used to bond a plurality of copolymers of conjugated diene monomer units and vinyl aromatic monomer units between polymer block A2-polymer block A2, between polymer block B2-polymer block B2, or between polymer block A2-polymer block B2. Examples of the coupling agent include, but are not limited to, halogenated silicon compounds and acid esters described below.
[0207] The structural formula of the hydrogenated block copolymer (a-2) is preferably the above-mentioned formulas (8), (9) and (10), more preferably the above-mentioned formulas (8) and (10), and still more preferably the above-mentioned formula (8).
[0208] In general formulas (8) to (14), the vinyl aromatic monomer units in polymer blocks A2 and B2 may be uniformly distributed or distributed in a tapered manner. In addition, when polymer blocks A2 and B2 are copolymer blocks of vinyl aromatic monomer units and conjugated diene monomer units, the vinyl aromatic monomer units in the copolymer blocks may exist in a plurality of uniformly distributed portions and / or in a tapered distribution portion. In addition, a plurality of portions having different contents of vinyl aromatic monomer units may coexist in the above-mentioned copolymer block portion.
[0209] As described above, the content of all vinyl aromatic monomer units in the hydrogenated block copolymer (a-2) is 35% to 70% by mass (the above condition (2-3)). It is preferably 37% to 70% by mass, more preferably 40% to 70% by mass, further preferably greater than 40% to 70% by mass, further preferably greater than 40% to 68% by mass, further preferably greater than 40% to 66% by mass.
[0210] When the content of all vinyl aromatic monomer units in the hydrogenated block copolymer (a-2) is 35% by mass or more, the thermoplastic elastomer composition of the present embodiment has improved mechanical strength and affinity with the polar group-containing thermoplastic resin described later, and there is a tendency that sufficient thermal adhesive strength can be obtained. When the content of all vinyl aromatic monomer units in the hydrogenated block copolymer (a-2) is 70% by mass or less, there is a tendency that the thermoplastic elastomer composition of the present embodiment has further improved flexibility and recovery properties.
[0211] It should be noted that the content of all vinyl aromatic monomer units in the hydrogenated block copolymer (a-2) can be controlled within the above numerical range by adjusting the amount of monomer added in the polymerization step of the hydrogenated block copolymer (a-2), and can be calculated using an ultraviolet spectrophotometer based on the absorption intensity at a wavelength of 262 nm using the method described in the examples described later.
[0212] The weight average molecular weight of the hydrogenated block copolymer (a-2) is 30,000 or more and less than 150,000 (the above-mentioned condition (2-4)).
[0213] When the weight average molecular weight of the hydrogenated block copolymer (a-2) is 30,000 or more, the heat deformation resistance and recovery of the thermoplastic elastomer composition of the present embodiment tend to be improved. When the weight average molecular weight of the hydrogenated block copolymer (a-2) is less than 150,000, the fluidity of the thermoplastic elastomer composition of the present embodiment is improved, and the moldability and thermal adhesiveness of the thermoplastic elastomer composition of the present embodiment tend to be improved. From the same viewpoint, the weight average molecular weight of the hydrogenated block copolymer (a-2) is preferably 40,000 to 130,000, and more preferably 50,000 to 110,000.
[0214] The molecular weight distribution (Mw / Mn) of the hydrogenated block copolymer (a-2) is preferably 1.01 to 8.0, more preferably 1.01 to 6.0, and even more preferably 1.01 to 5.0. If the molecular weight distribution of the hydrogenated block copolymer (a-2) is within the above range, the thermoplastic elastomer composition of the present embodiment tends to have better recovery. It should be noted that the Mw and Mn of the hydrogenated block copolymer (a-2) can be measured by GPC, specifically, by the method described in the examples described later.
[0215] The shape of the molecular weight distribution curve of the hydrogenated block copolymer (a-2) is not particularly limited, and the molecular weight distribution curve may be a multimodal molecular weight distribution having two or more peaks, or a unimodal molecular weight distribution having one peak.
[0216] In the hydrogenated block copolymer (a-2), the vinyl bond content of the conjugated diene monomer units in the polymer block B2 before hydrogenation is 60 to 95 mol% (the above condition (2-5)), preferably 63 to 90 mol%, more preferably 65 to 85 mol%.
[0217] In the hydrogenated block copolymer (a-2), when the vinyl bond content before hydrogenation in the conjugated diene monomer unit in the polymer block B2 is 60 mol% or more, the compatibility with the polypropylene resin (b) described later tends to be improved, and the thermoplastic elastomer composition of the present embodiment tends to have good thermal adhesiveness. In addition, by making the molecular weight of the hydrogenated block copolymer (a-2) relatively small and further making the vinyl bond content as high as 60 mol% or more, the fluidity of the thermoplastic elastomer composition of the present embodiment is improved, and the wettability to follow the fine irregularities on the surface of the adherend is improved, and the thermoplastic elastomer composition of the present embodiment tends to have good thermal adhesiveness.
[0218] Furthermore, by setting the vinyl bond content of the conjugated diene monomer unit before hydrogenation to 95 mol% or less, the mechanical strength of the thermoplastic elastomer composition of the present embodiment tends to be ensured.
[0219] The vinyl bond content of the conjugated diene monomer unit can be measured by nuclear magnetic resonance spectroscopy (NMR) using the block copolymer, and specifically, can be measured by the method described in Examples below.
[0220] The vinyl bond content can be controlled within the above-mentioned numerical range by adjusting the type and amount of a regulator such as a tertiary amine described later.
[0221] As described above, from the viewpoint of the thermal adhesive strength of the thermoplastic elastomer composition of the present embodiment, and the flexibility and recovery of the thermoplastic elastomer composition, the hydrogenated block copolymer (a-2) contains 35 to 70% by mass of all vinyl aromatic monomer units (the above condition (2-3)), and from the viewpoint of the thermal adhesiveness and mechanical strength of the thermoplastic elastomer composition of the present embodiment, the amount of vinyl bonds in the conjugated diene monomer units before hydrogenation is 60 to 95% by mass (the above condition (2-5)).
[0222] The hydrogenation rate of the double bonds of the conjugated diene monomer units in the hydrogenated block copolymer (a-2) is 50 mol% or more (the above condition (2-6)), preferably 80% or more, and more preferably 90% or more. If the hydrogenation rate of the double bonds of the conjugated diene monomer units in the hydrogenated block copolymer (a-2) is 50 mol% or more, the thermoplastic elastomer composition of the present embodiment can be suppressed from deteriorating in mechanical properties due to thermal degradation, i.e., oxidative degradation. The upper limit of the hydrogenation rate is not limited, but is preferably 100% or less, and preferably 99% or less.
[0223] The hydrogenation rate of the double bonds of the conjugated diene monomer units of the hydrogenated block copolymer (a-2) can be controlled within the above numerical range by adjusting the type and amount of the hydrogenation catalyst and the hydrogenation conditions, and can be measured by the method described in the examples below.
[0224] The hydrogenation rate of the aromatic double bonds based on the vinyl aromatic monomer units in the hydrogenated block copolymer (a-2) is not particularly limited, but is preferably 50% or less, more preferably 30% or less, and even more preferably 20% or less.
[0225] When the hydrogenated block copolymer (a-2) has at least two polymer blocks A2 and at least two of the above polymer blocks B2, at least one polymer block B2 is located at the terminal of the above hydrogenated block copolymer (a-2), and the content of the polymer block B2 located at the terminal is preferably 1% by mass or more, more preferably 2% by mass or more, and even more preferably 3% by mass or more in the above hydrogenated block copolymer (a-2). The upper limit is preferably 10% by mass or less, more preferably 9% by mass or less, and even more preferably 8% by mass or less.
[0226] In this case, the hydrogenated block copolymer (a-2) preferably does not have a peak having a weight average molecular weight of 250,000 or more.
[0227] In the case of this configuration, the content of all vinyl aromatic monomer units in the hydrogenated block copolymer (a-2) is preferably more than 40% by mass and not more than 70% by mass.
[0228] When at least one polymer block B2 is located at the terminal of the hydrogenated block copolymer (a-2) and the content of the polymer block B2 located at the terminal is within the above numerical range, the thermoplastic elastomer composition of the present embodiment tends to have better flexibility and fluidity. The content of the polymer block B2 located at the terminal can be calculated by dividing the mass of the conjugated diene polymerized at the terminal from the mass of all monomers used in the polymerization reaction.
[0229] In the above configuration, since the hydrogenated block copolymer (a-2) does not have a peak with a weight average molecular weight of 250,000 or more, the fluidity of the thermoplastic elastomer composition of the present embodiment is improved, the wettability to the adherend surface is good, and the thermoplastic elastomer composition of the present embodiment tends to have good thermal adhesiveness.
[0230] In addition, in this configuration, by making the content of all vinyl aromatic monomer units of the hydrogenated block copolymer (a-2) greater than 40% by mass and less than 70% by mass, the thermoplastic elastomer composition of the present embodiment has a good balance between mechanical strength or thermal adhesive strength with a polar group-containing thermoplastic resin and flexibility or recovery properties.
[0231] In order to make at least one polymer block B2 in the hydrogenated block copolymer (a-2) located at the end; the content of the polymer block B2 located at the end is within the above numerical range; there is no peak with a weight average molecular weight of 250,000 or more; and further make the content of all vinyl aromatic monomer units in the hydrogenated block copolymer (a-2) within the above numerical range, it is effective to adjust the addition period and addition amount of the monomers in the polymerization step of the hydrogenated block copolymer (a-2).
[0232] (Method for producing hydrogenated block copolymer)
[0233] Examples of methods for producing the hydrogenated block copolymers (a-1) and (a-2) include, but are not limited to, methods described in JP-B-36-19286, JP-B-43-17979, JP-B-46-32415, JP-B-49-36957, JP-B-48-2423, JP-B-48-4106, JP-B-51-49567, and JP-A-59-166518.
[0234] The block copolymers containing conjugated diene monomer units and vinyl aromatic monomer units before hydrogenation of the hydrogenated block copolymers (a-1) and (a-2) can be obtained by, but not limited to, anionic living polymerization in a hydrocarbon solvent using a polymerization initiator such as an organic alkali metal compound.
[0235] The hydrocarbon solvent is not particularly limited, and examples thereof include aliphatic hydrocarbons such as n-butane, isobutane, n-pentane, n-hexane, n-heptane, and n-octane; alicyclic hydrocarbons such as cyclohexane, cycloheptane, and methylcycloheptane; and aromatic hydrocarbons such as benzene, toluene, xylene, and ethylbenzene.
[0236] The polymerization initiator is not particularly limited, and an organic alkali metal compound that is generally known to have anionic polymerization activity for conjugated diene compounds and vinyl aromatic compounds can be used. Examples of the organic alkali metal compound include, but are not limited to, aliphatic hydrocarbon alkali metal compounds having 1 to 20 carbon atoms, aromatic hydrocarbon alkali metal compounds having 1 to 20 carbon atoms, and organic amino alkali metal compounds having 1 to 20 carbon atoms.
[0237] Examples of the alkali metal contained in the polymerization initiator include, but are not limited to, lithium, sodium, potassium, etc. In addition, the alkali metal may be contained in one molecule, or in two or more kinds.
[0238] Specific examples of the polymerization initiator include n-propyllithium, n-butyllithium, sec-butyllithium, tert-butyllithium, n-pentyllithium, n-hexyllithium, benzyllithium, phenyllithium, tolyllithium, the reaction product of diisopropenylbenzene and sec-butyllithium, and the reaction product of divinylbenzene, sec-butyllithium and a small amount of 1,3-butadiene.
[0239] In addition, 1-(tert-butoxy)propyllithium disclosed in U.S. Patent No. 5,708,092 and lithium compounds into which one to several molecules of isoprene monomer are inserted to improve their solubility; alkyllithiums containing silyl groups such as 1-(tert-butyldimethylsilyloxy)hexyllithium disclosed in British Patent No. 2,241,239; alkyllithiums containing amino groups disclosed in U.S. Patent No. 5,527,753; and amides such as lithium diisopropylamide and lithium hexamethyldisilazide can be used as polymerization initiators.
[0240] When a conjugated diene compound and a vinyl aromatic compound are copolymerized using an organic alkali metal compound as a polymerization initiator, a tertiary amine compound, an ether compound, or a metal alkoxide compound may be added as a regulator in order to adjust the content of the vinyl bond (1,2-bond or 3,4-bond) brought by the conjugated diene compound introduced into the copolymer, or to adjust the random copolymerizability of the conjugated diene compound and the vinyl aromatic compound.
[0241] The adjusters may be used alone or in combination of two or more.
[0242] As the tertiary amine compound of the adjusting agent, a compound represented by the general formula R1R2R3N can be used.
[0243] Here, in the general formula, R1, R2, and R3 represent a hydrocarbon group having 1 to 20 carbon atoms or a hydrocarbon group having a tertiary amino group.
[0244] Examples of tertiary amine compounds include, but are not limited to, trimethylamine, triethylamine, tributylamine, N,N-dimethylaniline, N-ethylpiperidine, N-methylpyrrolidine, N,N,N',N'-tetramethylethylenediamine, N,N,N',N'-tetraethylethylenediamine, 1,2-dipiperidinylethane, trimethylaminoethylpiperazine, N,N,N',N",N"-pentamethylethylenetriamine, and N,N'-dioctyl-p-phenylenediamine.
[0245] As the ether compound of the adjusting agent, a linear ether compound, a cyclic ether compound, or the like can be used.
[0246] Examples of the linear ether compound include, but are not limited to, dimethyl ether, diethyl ether, diphenyl ether, dialkyl ether compounds of ethylene glycol such as ethylene glycol dimethyl ether, ethylene glycol diethyl ether, and ethylene glycol dibutyl ether, and dialkyl ether compounds of diethylene glycol such as diethylene glycol dimethyl ether, diethylene glycol diethyl ether, and diethylene glycol dibutyl ether.
[0247] Examples of the cyclic ether compound include, but are not limited to, tetrahydrofuran, dioxane, 2,5-dimethyltetrahydrofuran, 2,2,5,5-tetramethyltetrahydrofuran, 2,2-bis(2-tetrahydrofuryl)propane, and alkyl ethers of furfuryl alcohol.
[0248] Examples of the metal alkoxide compound as the adjusting agent include, but are not limited to, sodium tert-amylate, sodium tert-butylate, potassium tert-amylate, potassium tert-butylate and the like.
[0249] The method for copolymerizing the conjugated diene compound and the vinyl aromatic compound using the organic alkali metal compound as a polymerization initiator is not particularly limited, and may be batch polymerization, continuous polymerization, or a combination thereof.
[0250] From the viewpoint of adjusting the molecular weight distribution to a preferred appropriate range, a batch polymerization method is preferred.
[0251] The polymerization temperature is not particularly limited, but is usually 0 to 180°C, preferably 30 to 150°C.
[0252] The time required for the polymerization varies depending on the conditions, but is usually within 48 hours, preferably 0.1 to 10 hours.
[0253] The polymerization is preferably carried out in an atmosphere of an inert gas such as nitrogen. The polymerization pressure is not particularly limited as long as the polymerization is carried out within a pressure range sufficient to maintain the monomer and the solvent in a liquid phase within the above-mentioned polymerization temperature range.
[0254] Furthermore, at the end of the polymerization, a necessary amount of a coupling agent having two or more functional groups may be added to carry out a coupling reaction.
[0255] There is no particular limitation on the coupling agent having more than two functional groups, and known substances can be used. As the coupling agent having two functional groups, there can be mentioned, but not limited to, alkyl alkoxysilanes such as dimethyldimethoxysilane and dimethyldiethoxysilane, halogenated silicon compounds such as dimethyldichlorosilane and dimethyldibromosilane; acid esters such as methyl benzoate, ethyl benzoate, phenyl benzoate and phthalates, etc.
[0256] In addition, when the hydrogenated block copolymers (a-1) and (a-2) are copolymers obtained by coupling reaction using these coupling agents, the non-modification condition is not violated.
[0257] Examples of the polyfunctional coupling agent with three or more functional groups include, but are not limited to, trivalent or more polyols, epoxidized soybean oil, polycyclic epoxy compounds such as diglycidyl bisphenol A, alkyl alkoxysilanes such as methyltrimethoxysilane, tetramethoxysilane, methyltriethoxysilane, and tetraethoxysilane, and compounds of the general formula R 1 (4-n) SiX n The represented silicon halide compound.
[0258] Here, in the general formula, R 1 represents a hydrocarbon group having 1 to 20 carbon atoms, X represents a halogen, and n represents an integer of 3 or 4.
[0259] Examples of the silicon halide compound include, but are not limited to, methyltrichlorosilane, tert-butyltrichlorosilane, silicon tetrachloride, and bromides thereof.
[0260] The hydrogenation catalyst used for producing the hydrogenated block copolymer is not particularly limited, and for example, the hydrogenation catalysts described in JP-B-42-8704, JP-B-43-6636, JP-B-63-4841, JP-B-1-37970, JP-B-1-53851, JP-B-2-9041, etc. can be used.
[0261] Preferred hydrogenation catalysts include cyclopentadienyl titanium compounds and mixtures of the cyclopentadienyl titanium compounds and reducing organometallic compounds.
[0262] The cyclopentadienyl titanium compound is not particularly limited, and examples thereof include compounds described in Japanese Patent Application Laid-Open No. 8-109219, etc. Specifically, examples thereof include compounds having at least one ligand having a substituted or unsubstituted cyclopentadienyl structure, an indenyl structure, and a fluorenyl structure, such as dicyclopentadienyl titanium dichloride and monopentamethylcyclopentadienyl titanium trichloride.
[0263] Examples of the reducing organometallic compound include, but are not limited to, organoalkali metal compounds such as organolithium, organomagnesium compounds, organoaluminum compounds, organoboron compounds, and organozinc compounds.
[0264] The reaction temperature of the hydrogenation reaction is usually 0 to 200°C, preferably 30 to 150°C.
[0265] The pressure of hydrogen used in the hydrogenation reaction is preferably 0.1 to 15 MPa, more preferably 0.2 to 10 MPa, and even more preferably 0.3 to 5 MPa.
[0266] The reaction time of the hydrogenation reaction is usually 3 minutes to 10 hours, preferably 10 minutes to 5 hours.
[0267] It should be noted that the hydrogenation reaction can be carried out by a batch process, a continuous process, or a combination thereof.
[0268] The catalyst residue may be removed from the reaction solution after the hydrogenation reaction as needed.
[0269] Examples of methods for separating the hydrogenated block copolymer from the solvent include, but are not limited to: a method in which a polar solvent such as acetone or alcohol, which is a poor solvent for the hydrogenated block copolymer, is added to a solution of the hydrogenated block copolymer to precipitate the hydrogenated block copolymer for recovery; or a method in which a solution of the hydrogenated block copolymer is poured into hot water under stirring to remove the solvent by stripping for recovery; a method in which the solution of the hydrogenated block copolymer is directly heated to remove the solvent by distillation; and the like.
[0270] An antioxidant may be added to the reaction solution when producing the hydrogenated block copolymer (a).
[0271] Examples of the antioxidant include, but are not limited to, phenolic antioxidants, phosphorus antioxidants, sulfur antioxidants, and amine antioxidants.
[0272] Specific examples include 2,6-di-tert-butyl-4-methylphenol, 3-(4'-hydroxy-3',5'-di-tert-butylphenyl) propionate, tetrakis-[methylene-3-(3',5'-di-tert-butyl-4'-hydroxyphenyl) propionate]methane], tris-(3,5-di-tert-butyl-4-hydroxybenzyl) isocyanurate, 4,4'-butylenebis-(3-methyl-6-tert-butylphenol), 3,9-bis[2-{3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionyloxy}-1,1-dimethyl [ethyl]-2,4,8,10-tetraoxaspiro[5,5]undecane, triethylene glycol bis[3-(3-tert-butyl-5-methyl-4-hydroxyphenyl) propionate], 1,6-hexanediol bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate], 2,4-bis-(n-octylthio)-6-(4-hydroxy-3,5-di-tert-butylanilino)1,3,5-triazine, pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate], 2,2-thio-diethylene bis[3-(3,5-di-tert-butyl -4-hydroxyphenyl) propionate], N,N'-hexamethylenebis(3,5-di-tert-butyl-4-hydroxy-hydrocinnamic acid), diethyl 3,5-di-tert-butyl-4-hydroxybenzylphosphonate, 1,3,5-trimethyl-2,4,6-tri(3,5-di-tert-butyl-4-hydroxybenzyl)benzene, a mixture of calcium bis(ethyl 3,5-di-tert-butyl-4-hydroxybenzylphosphonate) and polyethylene wax (50%), octylated diphenylamine, 2,4-bis[(octylthio)methyl]-o-cresol, isooctyl-3-(3,5-di-tert-butyl-4- The invention also includes the following: 1,2-di-(tert-butyl-5-hydroxy-2,6-dimethylbenzyl)isocyanurate, 2-tert-butyl-6-(3'-tert-butyl-5'-methyl-2'-hydroxybenzyl)-4-methylphenyl-acrylate, and 2-[1-(2-hydroxy-3,5-di-tert-pentylphenyl)-ethyl]-4,6-di-tert-pentylphenyl acrylate.
[0273] (Polypropylene resin (b))
[0274] The thermoplastic elastomer composition of the present embodiment contains a polypropylene-based resin (b).
[0275] Examples of the polypropylene resin (b) include, but are not limited to, propylene homopolymers; block copolymers or random copolymers of propylene and an olefin other than propylene, preferably an α-olefin having 2 to 20 carbon atoms; or blends thereof.
[0276] Examples of the α-olefins having 2 to 20 carbon atoms include, but are not limited to, ethylene, 1-butene, 1-hexene, 4-methyl-1-pentene, 1-octene, 1-decene, etc., preferably α-olefins having 2 to 8 carbon atoms, more preferably ethylene, 1-butene, 1-hexene, 4-methyl-1-pentene.
[0277] The polypropylene-based resin (b) may be used alone or in combination of two or more.
[0278] The melt flow rate (MFR) of the polypropylene resin (b) is preferably 0.1 to 50 g / 10 min at a temperature of 230° C. and a load of 2.16 kg. The lower limit is more preferably 0.5 g / 10 min or more, and further preferably 1.0 g / 10 min or more. The upper limit is more preferably 45 g / 10 min or less, and further preferably 40 g / 10 min or less. If the MFR of the polypropylene resin (b) is within the above range, the molding processability of the thermoplastic elastomer composition of the present embodiment tends to be further improved.
[0279] Examples of methods for producing the polypropylene resin (b) include, but are not limited to, a method of polymerizing the above-mentioned monomers using a Ziegler-Natta catalyst comprising a combination of a titanium-containing solid transition metal component and an organic metal component.
[0280] Examples of transition metal components used in Ziegler-Natta catalysts include, but are not limited to, solid components containing titanium, magnesium, and halogen as essential components and electron-donating compounds as optional components, or titanium trichloride. Examples of organic metal components include, but are not limited to, aluminum compounds.
[0281] Examples of the polymerization method for producing the polypropylene resin (b) include, but are not limited to, slurry polymerization, gas phase polymerization, bulk polymerization, solution polymerization, or a multi-stage polymerization method combining these.
[0282] In these polymerization methods, only propylene is polymerized when a propylene homopolymer is to be obtained, and propylene and a monomer other than propylene are polymerized when a copolymer is to be obtained.
[0283] In the thermoplastic elastomer composition of the present embodiment, the content of the polypropylene resin (b) is 10 parts by mass or more, preferably 20 parts by mass or more, and more preferably 30 parts by mass or more, relative to 100 parts by mass of the hydrogenated block copolymer (a-1). The upper limit is 100 parts by mass, preferably 90 parts by mass or less, and more preferably 80 parts by mass or less.
[0284] When the content of the polypropylene-based resin (b) is 10 parts by mass or more, good fluidity can be obtained in the thermoplastic elastomer composition of the present embodiment, and excellent molding processability can be obtained.
[0285] When the content of the polypropylene-based resin (b) is 100 parts by mass or less, good rebound resilience and flexibility can be obtained in the thermoplastic elastomer composition of the present embodiment.
[0286] (Non-aromatic softener (c))
[0287] The thermoplastic elastomer composition of the present embodiment contains a non-aromatic softener (c).
[0288] The non-aromatic softener (c) is not particularly limited as long as it does not exhibit aromaticity and can soften the thermoplastic elastomer composition of the present embodiment, and a known non-aromatic softener can be used.
[0289] The non-aromatic softener (c) includes, but is not limited to, paraffin oil, cycloparaffin oil, paraffin wax, liquid paraffin, white mineral oil, plant softeners, etc. Among these, paraffin oil, liquid paraffin, and white mineral oil are preferred from the viewpoints of low temperature properties, dissolution resistance, sanitation, etc. of the molded article including the thermoplastic elastomer composition of the present embodiment.
[0290] The kinematic viscosity of the non-aromatic softener (c) at 40° C. is preferably 10 to 500 mm 2 / Second.
[0291] If the non-aromatic softener (c) has a kinematic viscosity of 10 mm at 40°C 2 / sec or more, the heat deformation resistance and softener retention of the thermoplastic elastomer composition of the present embodiment tend to be further improved.
[0292] If the non-aromatic softener (c) has a kinematic viscosity of 500 mm at 40°C 2 / sec or less, the fluidity of the thermoplastic elastomer composition of the present embodiment tends to be further improved, and the molding processability tends to be further improved.
[0293] The kinematic viscosity of the non-aromatic softener (c) can be measured using a glass capillary viscometer.
[0294] In the thermoplastic elastomer composition of the present embodiment, the content of the non-aromatic softener (c) is 50 to 300 parts by mass, preferably 60 parts by mass or more, and more preferably 70 parts by mass or more, relative to 100 parts by mass of the hydrogenated block copolymer (a-1). The upper limit is 300 parts by mass or less, preferably 250 parts by mass or less, and more preferably 200 parts by mass or less.
[0295] When the content of the non-aromatic softener (d) is within the above range, the retention of the non-aromatic softener (c), i.e., the effect of suppressing bleed-out, can be further enhanced, and a thermoplastic elastomer composition having further excellent molding processability, flexibility, and recovery properties tends to be obtained.
[0296] (Inorganic filler (d))
[0297] The thermoplastic elastomer composition of the present embodiment may contain an inorganic filler (d) from the viewpoint of adjusting the molded appearance, surface texture and feel, and glossiness.
[0298] Examples of the inorganic filler (d) include, but are not limited to, talc, calcium carbonate, calcium oxide, zinc carbonate, wollastonite, zeolite, wollastonite, silicon oxide, aluminum oxide, clay, titanium oxide, magnesium hydroxide, magnesium oxide, sodium silicate, calcium silicate, magnesium silicate, sodium aluminate, calcium aluminate, sodium aluminosilicate, zinc oxide, potassium titanate, hydrotalcite, barium sulfate, titanium black, and carbon black such as furnace black, thermal black, and acetylene black.
[0299] These inorganic fillers may be used alone or in combination of two or more.
[0300] In addition, these inorganic fillers may be surface-treated from the viewpoint of improving dispersibility in the thermoplastic elastomer composition of the present embodiment.
[0301] Examples of the surface treatment agent include fatty acids, resin acids, oils and fats, surfactants, and coupling agents (silane-based, titanium-based, phosphoric acid-based, carboxylic acid-based, etc.), but are not limited to these agents as long as they can act on the surface of the inorganic filler.
[0302] (Organic peroxide (e))
[0303] The thermoplastic elastomer composition of the present embodiment is preferably partially crosslinked in the presence of an organic peroxide (e) from the viewpoint of heat deformation resistance and recovery properties.
[0304] Examples of the organic peroxide (e) include, but are not limited to, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, dicumyl peroxide, 2,5-dimethyl-2,5-di(benzoylperoxy)hexane, tert-butyl peroxybenzoate, tert-butylcumyl peroxide, diisopropylbenzene peroxide, 1,3-bis(tert-butylperoxyisopropyl)benzene, benzoyl peroxide, 1,1-di(tert-butylperoxy)-3,3, 5-trimethylcyclohexane, tert-butyl hydroperoxide, 1,1,3,3-tetramethylbutyl hydroperoxide, cumene hydroperoxide, di-tert-butyl peroxide, 1,1-di-tert-butyl peroxycyclohexane, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexyne-3, n-butyl-4,4-bis(tert-butylperoxy)valerate, tert-butyl peroxyisobutyrate, tert-butyl peroxy-2-ethylhexanoate, tert-butyl peroxyisopropyl carbonate, etc.
[0305] These organic peroxides may be used alone or in combination of two or more.
[0306] The amount of the organic peroxide (e) used is preferably 0.05 to 5 parts by mass, more preferably 0.1 to 4 parts by mass, and even more preferably 0.3 to 3 parts by mass, based on 100 parts by mass of the hydrogenated block copolymer (a-1).
[0307] When the amount of the organic peroxide (e) used is within the above range, there is a tendency to obtain a thermoplastic elastomer composition having further excellent heat deformation resistance and recovery properties without reducing processability.
[0308] (Crosslinking aid (f))
[0309] When the thermoplastic elastomer composition of the present embodiment is partially crosslinked, a crosslinking aid may be used as necessary to adjust the degree of crosslinking.
[0310] Examples of the crosslinking aid (f) include, but are not limited to, trimethylolpropane triacrylate, triallyl isocyanurate, triallyl cyanurate, triallyl formal, triallyl trimellitate, N,N'-m-phenylene bismaleimide, dipropynyl terephthalate, diallyl phthalate, tetraallyl terephthalamide, triallyl phosphate, divinylbenzene, ethylene dimethacrylate, diallyl phthalate, quinone dioxime, ethylene glycol dimethacrylate, polyfunctional methacrylate monomers, polyol methacrylates and acrylates, and unsaturated silane compounds (e.g., vinyl trimethoxysilane, vinyl triethoxysilane, etc.).
[0311] These cross-linking aids may be used alone or in combination of two or more as necessary.
[0312] The amount of the crosslinking aid (f) used is preferably 0.1 parts by mass or more, more preferably 0.2 parts by mass or more, and further preferably 0.5 parts by mass or more, relative to 100 parts by mass of the hydrogenated block copolymer (a-1). The preferred upper limit is 10 parts by mass or less, more preferably 8 parts by mass or less, and further preferably 7 parts by mass or less.
[0313] (Other ingredients)
[0314] The thermoplastic elastomer composition of the present embodiment may further contain other additives in addition to the above-mentioned components (a) to (f) within a range that does not impair the purpose of the present embodiment.
[0315] Examples of the other additives include heat stabilizers, antioxidants, ultraviolet absorbers, antioxidants, plasticizers, light stabilizers, crystal nucleating agents, impact modifiers, pigments, lubricants, antistatic agents, flame retardants, flame retardant aids, compatibilizers, and tackifiers.
[0316] In particular, when silicone oil is added as a lubricant, the sliding property is improved, which is effective in reducing the resistance during needle puncture and improving the chipping during needle puncture.
[0317] Examples of the silicone oil include common dimethyl polysiloxane and phenyl-methyl polysiloxane, and dimethyl polysiloxane is particularly preferred.
[0318] The amount of silicone oil added is preferably 0.5 parts by mass or more, more preferably 0.7 parts by mass or more, and further preferably 1.0 parts by mass or more, relative to 100 parts by mass of the hydrogenated block copolymer (a-1). The upper limit is preferably 10 parts by mass or less, more preferably 7 parts by mass or less, and further preferably 5 parts by mass or less.
[0319] The kinematic viscosity of the silicone oil is not particularly limited, but is preferably 10 to 10,000 mm 2 / sec, more preferably 50 to 7000 mm 2 / sec, more preferably 100 to 5000 mm 2 / Second.
[0320] The above-mentioned other additives may be used alone or in combination of two or more.
[0321] (Method for producing thermoplastic elastomer composition)
[0322] The method for producing the thermoplastic elastomer composition of the present embodiment or a molded product (for example, pellets) composed of the thermoplastic elastomer composition is not particularly limited, and a conventionally known method can be applied.
[0323] For example, there can be mentioned a melt kneading method using common mixers such as a pressure kneader, Banbury mixer, internal mixer, torque rheometer (LABOPLASTOMILL), Mix Labo, single-screw extruder, twin-screw extruder, worm kneader, multi-screw extruder, etc.; a method in which each component is dissolved or dispersed and mixed and then heated to remove the solvent; and the like.
[0324] When the thermoplastic elastomer composition of the present embodiment is partially crosslinked by the organic peroxide (e), the composite formation of the components (a) to (d) and the partial crosslinking by the organic peroxide (e) and the crosslinking aid (f) added as required may be performed simultaneously, or the organic peroxide (e) and the crosslinking aid (f) may be added after the components (a) to (d) are composited to perform partial crosslinking.
[0325] Alternatively, part of the components (a) to (d) may be mixed with the organic peroxide (e) and, if necessary, the crosslinking aid (f) to perform crosslinking, and then other components may be mixed.
[0326] Partial crosslinking can be performed at a temperature at which the organic peroxide (e) used decomposes, usually at 150 to 250°C.
[0327] When compounding of part or all of the components (a) to (d) and crosslinking by the organic peroxide (e) and the crosslinking aid (f) added as required are simultaneously performed, compounding can be performed by using the above-mentioned melt kneader at a temperature at which the organic peroxide (e) used decomposes.
[0328] [Multilayer Molded Body]
[0329] The multilayer molded product of the present embodiment comprises a thermoplastic elastomer composition layer of the present embodiment and a polar group-containing thermoplastic resin layer.
[0330] The multilayer molded body of the present embodiment is a multilayer molded body comprising: a thermoplastic resin layer containing a polar group; and a thermoplastic elastomer composition layer containing a hydrogenated block copolymer (a), a polypropylene resin (b) and a non-aromatic softener (c); the thermoplastic elastomer composition layer is arranged in contact with the thermoplastic resin layer containing a polar group.
[0331] The hydrogenated block copolymer (a) is an unmodified block copolymer not containing a modifying group. By making the hydrogenated block copolymer (a) unmodified, a thermoplastic elastomer composition having no odor or color tone and no impurities from unreacted products can be obtained.
[0332] It should be noted that the term “non-modified” excludes the case where the hydrogenated block copolymer (a) contains a modified group formed by a predetermined modifier.
[0333] Examples of the modified group include an amino group containing a N atom, a nitro group or an amide bond, an azo bond, a keto group in which an O atom is bonded to a C atom alone via a double bond, a carbonyl group, a carboxyl group, an aldehyde group, a hydroxyl group in which an O atom is bonded to an H atom, a sulfone group containing an S atom, and a compound group bonded to a halogen element such as an F atom, a Cl atom, or a Br atom.
[0334] When the hydrogenated block copolymer (a) is obtained by a coupling reaction using a coupling agent at the end of the polymerization reaction, the condition of "being unmodified" is satisfied if it has Si atoms derived from the coupling agent and O atoms adjacent thereto and bonded to a straight chain as residues.
[0335] The hydrogenated block copolymer (a) is a hydrogenated block copolymer having a vinyl aromatic monomer unit and a conjugated diene monomer unit, and has one or more molecular weight peaks (weight-equivalent molecular weight; PMw) based on GPC at 30,000 to less than 150,000, preferably 40,000 to 130,000, and more preferably 50,000 to 110,000.
[0336] When the peak molecular weight of the hydrogenated block copolymer (a) is 30,000 or more, the thermoplastic elastomer composition of the present embodiment tends to have improved heat deformation resistance and recovery. On the other hand, when the peak molecular weight is less than 150,000, the fluidity of the thermoplastic elastomer composition of the present embodiment is improved, and the moldability and thermal adhesiveness of the thermoplastic elastomer composition of the present embodiment tend to be improved.
[0337] It should be noted that PMw of the hydrogenated block copolymer can be measured by GPC, and specifically, can be measured by the method described in Examples below.
[0338] In the hydrogenated block copolymer having a molecular weight peak of 30,000 to less than 150,000 based on GPC, the content of all vinyl aromatic monomer units is 35% by mass or more, preferably 37% by mass or more, more preferably 40% by mass or more, further preferably more than 40% by mass and 66% by mass or less. The upper limit is 70% by mass or less, preferably 68% by mass or less, and more preferably 66% by mass or less.
[0339] When the content of all vinyl aromatic monomer units in the hydrogenated block copolymer having a molecular weight peak of 30,000 to less than 150,000 based on GPC is 35% by mass or more, the mechanical strength of the thermoplastic elastomer composition of the present embodiment and the affinity with the polar group-containing thermoplastic resin are improved, and sufficient thermal adhesive strength tends to be obtained. When the content of all vinyl aromatic monomer units is 70% by mass or less, the flexibility and recovery of the thermoplastic elastomer composition of the present embodiment tend to be further improved.
[0340] It should be noted that the content of all vinyl aromatic monomer units can be controlled within the above numerical range by adjusting the amount of monomers added in the polymerization step of the hydrogenated block copolymer, and can be calculated based on the absorption intensity at 262 nm using an ultraviolet spectrophotometer by the method described in the examples below.
[0341] The amount of vinyl bonds before hydrogenation in the conjugated diene monomer units of the hydrogenated block copolymer having a molecular weight peak of 30,000 to less than 150,000 based on GPC is 60 mol% or more, preferably 63 mol% or more, more preferably 65 mol% or more, and the upper limit is 95 mol% or less, preferably 90 mol% or less, more preferably 85 mol% or less.
[0342] If the amount of vinyl bonds before hydrogenation in the conjugated diene monomer units of the hydrogenated block copolymer having a molecular weight peak of 30,000 to less than 150,000 based on GPC is 60 mol% or more, the compatibility with the polypropylene resin (b) tends to be improved, and the thermoplastic elastomer composition of the present embodiment tends to have good thermal adhesiveness. Furthermore, the fluidity is improved, and the wettability to follow the fine irregularities on the surface of the adherend is good, and the thermoplastic elastomer composition of the present embodiment tends to have good thermal adhesiveness.
[0343] When the amount of vinyl bonds before hydrogenation in the conjugated diene monomer units of the hydrogenated block copolymer having a molecular weight peak of 30,000 to less than 150,000 by GPC is 95 mol % or less, the thermoplastic elastomer composition of the present embodiment tends to have sufficient mechanical strength.
[0344] The vinyl bond amount of the conjugated diene monomer unit can be measured by nuclear magnetic resonance spectroscopy (NMR) using a block copolymer, and specifically, can be measured by the method described in the examples described later. In addition, the vinyl bond amount can be controlled within the above-mentioned numerical range by adjusting the type and addition amount of the adjusting agent such as the tertiary amine described later.
[0345] As described above, the hydrogenated block copolymer (a) constituting the thermoplastic elastomer composition is a hydrogenated polymer of a block copolymer having a vinyl aromatic monomer unit and a conjugated diene monomer unit. The hydrogenated block copolymer (a) further has one or more peaks of the molecular weight based on GPC (weight-converted molecular weight; PMw) in the range of 150,000 to 550,000. The molecular weight having the peak is preferably 170,000 or more, more preferably 190,000 or more, and further preferably 210,000 or more. In addition, it is preferably 500,000 or less, more preferably 450,000 or less, further preferably 400,000 or less, further more preferably 350,000 or less, and further preferably 300,000 or less.
[0346] When the peak molecular weight of the hydrogenated block copolymer is 150,000 or more, the thermoplastic elastomer composition of the present embodiment tends to have good heat deformation resistance and recovery. When the peak molecular weight of the hydrogenated block copolymer is 550,000 or less, the thermoplastic elastomer composition exhibits good fluidity, and thus tends to have sufficient molding processability.
[0347] It should be noted that PMw of the hydrogenated block copolymer can be measured by GPC, and specifically, can be measured by the method described in Examples below.
[0348] The hydrogenated block copolymer having a molecular weight peak of 150,000 to 550,000 by GPC contains 15% to less than 35% by mass, preferably 17% by mass or more, more preferably 19% by mass or more, further preferably 21% by mass or more, and further more preferably 23% by mass or more of all vinyl aromatic monomer units.
[0349] Moreover, it is preferably 34 mass % or less, and more preferably 33 mass % or less.
[0350] When the content of all vinyl aromatic monomer units in the hydrogenated block copolymer having a molecular weight peak of 150,000 to 550,000 based on GPC is 15% by mass or more, the mechanical strength and heat deformation resistance of the thermoplastic elastomer composition of the present embodiment tend to be improved. When the content of all vinyl aromatic monomer units in the hydrogenated block copolymer having a molecular weight peak of 150,000 to 550,000 based on GPC is less than 35% by mass, the flexibility, recovery and rebound resilience of the thermoplastic elastomer composition of the present embodiment tend to be improved.
[0351] It should be noted that the content of all vinyl aromatic monomer units can be controlled within the above numerical range by adjusting the amount of monomers added in the polymerization step of the hydrogenated block copolymer, and can be calculated based on the absorption intensity at a wavelength of 262 nm using an ultraviolet spectrophotometer by the method described in the examples below.
[0352] The hydrogenation rate of the aliphatic double bonds from the conjugated diene compound, i.e., the double bonds of the conjugated diene monomer unit in the hydrogenated block copolymer having a molecular weight peak of 150,000 to 550,000 based on GPC is 50 mol% or more, preferably 60 mol% or more, and more preferably 70 mol% or more. If the hydrogenation rate is 50 mol% or more, there is a tendency to more effectively suppress the reduction of mechanical properties due to thermal degradation (oxidative degradation). In addition, if the hydrogenation rate is 70 mol% or more, there is a tendency to obtain better weather resistance. The upper limit of the hydrogenation rate is not particularly limited, but is preferably 100% or less, and more preferably 99% or less.
[0353] The hydrogenation rate of the double bonds of the conjugated diene monomer units of the hydrogenated block copolymer having a molecular weight peak of 150,000 to 550,000 based on GPC can be controlled within the above numerical range by adjusting the type and amount of the hydrogenation catalyst and the hydrogenation conditions, and can be measured by the method described in the examples below.
[0354] The multilayer molded product of the present embodiment preferably has a structure in which the thermoplastic elastomer composition layer and the polar group-containing thermoplastic resin composition layer are heat-fused.
[0355] That is, the thermoplastic elastomer composition of the present embodiment constitutes a thermoplastic elastomer composition layer heat-fused to the polar group-containing thermoplastic resin composition layer constituting the multilayer molded body.
[0356] In the multilayer molded body of the present embodiment described above, the following configuration is a preferred aspect.
[0357] That is, the multilayer molded body of the present embodiment is preferably the following multilayer molded body:
[0358] The hydrogenated block copolymer (a) is composed of a hydrogenated block copolymer (a-1) and a hydrogenated block copolymer (a-2).
[0359] The above (a-1) satisfies the following conditions (1-1) to (1-4),
[0360] The above (a-2) satisfies the following conditions (2-1) to (2-6),
[0361] The thermoplastic elastomer composition layer contains 100 parts by mass of the above-mentioned (a-1), 10 to 100 parts by mass of the above-mentioned (b), and 50 to 300 parts by mass of the above-mentioned (c), wherein the content of the above-mentioned (a-2) in the thermoplastic elastomer composition layer is 5 to 70% by mass relative to the total amount of the above-mentioned components (a-1), (a-2), (b), and (c).
[0362] (1-1): Contains one or more polymer blocks A1 mainly composed of vinyl aromatic monomer units, and one or more polymer blocks B1 mainly composed of conjugated diene monomer units.
[0363] (1-2): The content of all vinyl aromatic monomer units is 15% by mass or more and less than 35% by mass.
[0364] (1-3): The weight average molecular weight is 150,000 to 550,000.
[0365] (1-4): 50 mol% or more of the double bonds of the conjugated diene monomer units are hydrogenated.
[0366] (2-1): Contains one or more polymer blocks A2 mainly composed of vinyl aromatic monomer units and one or more polymer blocks B2 mainly composed of conjugated diene monomer units.
[0367] (2-2): The content of the vinyl aromatic monomer unit in the polymer block A2 is 50% by mass or more.
[0368] (2-3): The content of all vinyl aromatic monomer units is 35% to 70% by mass.
[0369] (2-4): The weight average molecular weight is 30,000 or more and less than 150,000.
[0370] (2-5): The amount of vinyl bonds in the conjugated diene monomer units in the polymer block B2 before hydrogenation is 60 mol% to 95 mol%.
[0371] (2-6): 50 mol% or more of the double bonds of the conjugated diene monomer units are hydrogenated.
[0372] By having the above-mentioned structure, a multilayer molded body can be obtained which is good in odor and color tone from a practical point of view and is excellent in moldability, thermal adhesive strength, recovery property, and mechanical strength.
[0373] In addition, in the multilayer laminate of the present embodiment, the preferred aspects of the hydrogenated block copolymers (a-1) and (a-2) are common to the thermoplastic elastomer composition of the present embodiment.
[0374] (Thermoplastic resin containing polar groups)
[0375] As described above, the multilayer laminate of the present embodiment has a thermoplastic resin layer containing a polar group.
[0376] The polar group-containing thermoplastic resin constituting the polar group-containing thermoplastic resin layer contains one or more polar groups in its molecule.
[0377] Examples of the polar group-containing thermoplastic resin include, but are not limited to, polyamide resins, polyphenylene sulfide resins, polyester resins, polycarbonate resins, acrylonitrile-butadiene-styrene copolymer (ABS) resins (hereinafter also referred to as "ABS"), acrylic resins, and polyacetal resins.
[0378] These may be used alone or as a mixture of two or more.
[0379] The polyamide resin has an amino group, a carboxyl group, and an amide group in the main chain.
[0380] The polyphenylene sulfide resin has a carboxylic acid group at the terminal of the polymer chain.
[0381] The polyester resin has an ester structure in the main chain and a hydroxyl group or a carboxyl group at the terminal.
[0382] The polycarbonate resin has carbonate in the main chain and hydroxyl groups at the terminals.
[0383] ABS resin has a nitrile group.
[0384] Acrylic resin is a general term for polyacrylic acid, polyacrylate, polymethacrylic acid, and polymethacrylate, and has a carboxyl group and / or an ester group.
[0385] Polyacetal resin has an ether structure.
[0386] (use)
[0387] The multilayer molded body of this embodiment can be suitably used for sealing parts requiring softness and resilience in household appliance parts, industrial products, automobile parts / interior materials, medical instruments / equipment, building materials, tools, toys, sundries, etc., handles requiring a comfortable feel and tactile sensation when held by a person, or applications requiring impact protection when in contact with or colliding with the human body.
[0388] (Method for producing a multilayer molded body)
[0389] The method for manufacturing a multilayer molded body of the present embodiment comprises the following steps: a step of molding the above-mentioned thermoplastic resin containing polar groups to obtain a molded body; and a step of injecting the thermoplastic elastomer composition of the present embodiment into the gap between the above-mentioned mold and the above-mentioned molded body while the above-mentioned molded body is placed in a mold to perform heat welding.
[0390] Generally, a method is preferred in which a molded body of a polar group-containing thermoplastic resin is prepared, the molded body is inserted into a mold, and pellets of a thermoplastic elastomer composition are filled into the gap of the mold and heat-fused.
[0391] In addition, in the method for manufacturing a multilayer molded body, an insert molding method having the following steps can also be cited as a preferred method. The process is to first mold a molded body of a thermoplastic resin containing a polar group, then insert it into another mold, inject a thermoplastic elastomer composition into the gap, and perform heat welding.
[0392] In addition, the following two-color molding method is also a preferred method: using a molding machine having a structure of two or more barrels in one injection molding machine, first a thermoplastic resin containing a polar group is molded, and then a part of the mold is changed to generate a gap portion between the thermoplastic resin containing a polar group and the mold, and a thermoplastic elastomer composition is injected into the gap portion from another barrel.
[0393] The multilayer molded body of the present embodiment having the thermoplastic elastomer composition layer and the polar group-containing thermoplastic resin layer can be produced by any molding method.
[0394] The molding temperature is not particularly limited, but is preferably 150°C to 280°C.
[0395] Example
[0396] The present embodiment will be described in detail below with reference to specific examples and comparative examples, but the present invention is not limited to the following examples and comparative examples.
[0397] First, evaluation methods and methods for measuring physical properties applied to Examples and Comparative Examples are described below.
[0398] [Evaluation method of hydrogenated block copolymers (a-1) and (a-2)]
[0399] ((1) Weight average molecular weight, number average molecular weight, peak molecular weight, molecular weight distribution)
[0400] The weight average molecular weight (Mw), number average molecular weight (Mn), peak molecular weight (weight-converted molecular weight at the peak position; PMw), and molecular weight distribution (Mw / Mn) of the hydrogenated block copolymers (a-1) and (a-2) were determined based on the molecular weight of the peak in the chromatogram using a calibration curve obtained by measurement of commercially available standard polystyrene (prepared using the peak molecular weight of standard polystyrene).
[0401] HLC-8320ECOSEC Collection was used as the measurement software, and HLC-8320ECOSEC Analysis was used as the analysis software.
[0402] (Measurement conditions)
[0403] GPC: HLC-8320GPC (manufactured by Tosoh Corporation)
[0404] Detector: RI
[0405] Detection sensitivity: 3MV / minute
[0406] Sampling interval: 600MSEC
[0407] Column: TSKGEL SUPERHZM-N (6MMI.D×15CM) 4 pieces (manufactured by Tosoh Corporation)
[0408] Solvent: THF
[0409] Flow rate: 0.6ML / min
[0410] Concentration: 0.5MG / ML
[0411] Column temperature: 40°C
[0412] Injection volume: 20ML
[0413] ((2) Content of all vinyl aromatic monomer units (total styrene content))
[0414] A certain amount of the hydrogenated block copolymer was dissolved in chloroform and measured using an ultraviolet spectrophotometer (UV-2450 manufactured by Shimadzu Corporation). The styrene content was calculated from the peak intensity at the absorption wavelength (262 nm) due to styrene using a calibration curve.
[0415] ((3) Styrene Content in Polystyrene Block A in Hydrogenated Block Copolymers (a-1) and (a-2))
[0416] The styrene content in the polystyrene block A in the hydrogenated block copolymer is determined as follows: the hydrogenated block copolymer described later is oxidatively decomposed using tert-butyl hydroperoxide with osmium tetroxide as a catalyst, followed by precipitation with methanol, solid-liquid separation, and the precipitate is measured using an ultraviolet spectrophotometer (manufactured by Shimadzu Corporation, UV-2450). The peak intensity at the absorption wavelength (262 nm) due to styrene is calculated using a calibration curve, and the styrene content in the polystyrene block A is calculated based on the weight ratio of the calculated value to the amount added during production.
[0417] ((4) Styrene Content in Polystyrene Block A' in Hydrogenated Block Copolymer (a-2))
[0418] The styrene content in the polystyrene block A' in the hydrogenated block copolymer (a-2) is calculated by the following calculation formula.
[0419] (Calculation formula)
[0420] Styrene content in polystyrene block A' = ((total styrene content - styrene content in polystyrene block A) / amount of styrene and butadiene added during production of block A') × 100
[0421] ((5) Vinyl bond amount)
[0422] The amount of vinyl bonds in the polybutadiene block in the block copolymer was measured using a nuclear magnetic resonance apparatus (NMR) under the following conditions.
[0423] In the following tables, B represents a polybutadiene block.
[0424] The block copolymer was precipitated and recovered by adding a large amount of methanol to the reaction solution after the polymerization reaction. Next, the block copolymer was extracted with acetone, and the extract was vacuum dried and used as 1 H-NMR measurement of the sample. 1 The conditions for H-NMR measurement are as follows.
[0425] (Measurement conditions)
[0426] Measuring equipment: JNM-LA400 (manufactured by JEOL)
[0427] Solvent: deuterated chloroform
[0428] Sample concentration: 50MG / ML
[0429] Observation frequency: 400MHZ
[0430] Chemical shift standard: TMS (tetramethylsilane)
[0431] Pulse delay: 2.904 seconds
[0432] Scan times: 64 times
[0433] Pulse width: 45°
[0434] Measurement temperature: 26℃
[0435] The vinyl bond content was determined from the ratio of the total area of the peaks of 1,2-bond and 3,4-bond to the total area of all peaks related to the conjugated diene monomer unit (1,2-bond, 3,4-bond, 1,4-bond).
[0436] ((6) Hydrogenation rate)
[0437] The hydrogenation rate of the double bonds of the conjugated diene monomer units in the block copolymer was measured using a nuclear magnetic resonance apparatus (NMR) under the same conditions as in the above ((5) Vinyl bond amount).
[0438] The hydrogenation rate was determined by calculating the ratio of the total peak area of hydrogenated 1,2-bonds, hydrogenated 3,4-bonds, and hydrogenated 1,4-bonds to the total peak area of all peaks (1,2-bonds, 3,4-bonds, and 1,4-bonds) related to double bonds in the conjugated diene monomer units.
[0439] ((7) Content of terminal polybutadiene block)
[0440] The content of the terminal polybutadiene block in the block copolymer was determined by checking the amount of monomer added during production and the polymerization reaction rate of each block by gas chromatography (hereinafter referred to as GC).
[0441] <Confirmation of the Polymerization Reaction Rate of Each Polymer Block in the Block Copolymer>
[0442] About 20 mL of the polymer solution sampled at each step of the polymerization process of the block copolymer before hydrogenation was injected into a 100 mL bottle sealed with 0.50 mL of n-propylbenzene as an internal standard and about 20 mL of toluene to prepare a sample.
[0443] The sample was measured using a gas chromatograph (GC-14B manufactured by Shimadzu Corporation) equipped with a packed column loaded with apizone resin, and the amount of residual monomers in the polymer solution was calculated based on the calibration curve of butadiene monomer and styrene monomer obtained in advance, confirming that the polymerization rate of butadiene monomer and styrene monomer was 100%.
[0444] The polymerization rate of butadiene was measured under a constant condition of 90°C, and the polymerization rate of styrene was measured under a temperature increase condition of 90°C (maintained for 10 minutes) to 150°C (10°C / min).
[0445] ((8) Amount of anhydride group added)
[0446] The amount of added acid anhydride groups is the amount (mass %) of acid anhydride groups added to the entire hydrogenated block copolymer.
[0447] As a determination method, the block copolymer is first boiled in acetone for 60 minutes, then vacuum dried, and the dried product is dissolved in toluene. Next, phenolphthalein indicator is added, and titration is performed using a methanol solution of sodium methoxide (CH3ONa), and the amount of anhydride group added is calculated based on the amount of sodium methoxide added to the anhydride group.
[0448] [Production of Thermoplastic Elastomer Composition]
[0449] (Examples 1 to 25), (Comparative Examples 1 to 15)
[0450] The thermoplastic elastomer composition pellets were obtained by melt kneading at a set temperature of 230° C. using a twin-screw extruder (“TEX-30αII” manufactured by The Nippon Steel Works, Ltd., barrel diameter 30 mm) at the compounding ratios (parts by mass) shown in the table below.
[0451] [Evaluation method of thermoplastic elastomer composition]
[0452] ((9) Melt flow rate (MFR))
[0453] The melt flow rate (MFR) of the pellets of the thermoplastic elastomer composition obtained above was measured under the conditions of a temperature of 230° C. and a load of 2.16 kg in accordance with ASTM D1238.
[0454] ((10) Odor sensory test)
[0455] 100 g of the pellets of the thermoplastic elastomer composition were placed in a 500 mL pressure-resistant glass bottle, which was sealed, heated at 70° C. for 1 hour, and then left at room temperature for 48 hours.
[0456] Thereafter, 10 subjects confirmed the odor from the mouth of the glass bottle.
[0457] The judgment was made using the average value of the following odor intensity index.
[0458] ○: The odor intensity index is less than 3, ×: The odor intensity index is 3 or more, and ○ is evaluated as being good in practical use.
[0459] <Odor Intensity Index>
[0460] 0: no odor; 1: barely perceptible odor; 2: faint odor, but you can tell what it is; 2.5: between 2 and 3; 3: easily perceptible odor; 3.5: between 3 and 4; 4: relatively strong odor; 5: strong odor
[0461] [Preparation of pressed sheets]
[0462] The pellets of the thermoplastic elastomer composition obtained as described above were subjected to a 50 t electric hot press manufactured by Toho Press Mfg. Co., Ltd. using a die (size: 110 mm×220 mm×2 mm thick) at 200°C and 0.5 kgf / cm 2 Preheat for 5 minutes under pressure at 200℃, 100kgf / cm 2 The pressed sheet was prepared under a pressure of 2 mm for 2 minutes.
[0463] Using the obtained pressed sheet, physical properties were measured according to the following measurement methods.
[0464] [Evaluation method of pressed sheet]
[0465] ((11) Hardness)
[0466] The hardness was measured using a type A durometer in accordance with JIS K6253.
[0467] When the Shore A hardness is 90 or less, it is judged that the material has flexibility that does not cause problems in use, and when it is 80 or less, it is judged that the material has sufficient flexibility.
[0468] ((12) Tensile stress, tensile stress, tensile breaking strength, tensile breaking elongation)
[0469] According to JIS K6251, a tensile test was performed as follows at a crosshead speed of 500 mm / min using a No. 3 dumbbell-shaped specimen.
[0470] Tensile stress (M300): The stress at 300% elongation was measured.
[0471] Tensile strength at break (Tb): The stress at break was measured. If Tb was 2 MPa or more, it was judged that the material had mechanical strength sufficient for use, and if it was 4 MPa or more, it was judged that the material had sufficient mechanical strength.
[0472] Tensile elongation at break (Eb): The elongation at break was measured. If Eb is 500% or more, the material is judged to have sufficient flexibility.
[0473] ((13) Dunlop rebound)
[0474] The Dunlop rebound resilience was measured at 23°C using a Dunlop rebound resilience tester in accordance with BS903.
[0475] When the content is 30% or more, the film is judged to have a practically good touch.
[0476] ((14) 40℃ compression set)
[0477] According to the JIS K6301 compression set test, a 2 mm thick pressed sheet is punched into a circle with a diameter of 29 mm, and 6 circular sheets are stacked. The thickness of the initial stacking is measured at 23°C, and then placed in a 40°C oven for 22 hours under a 25% compression state, then taken out, released from compression, and the strain residual rate after being placed at 23°C for 30 minutes is calculated. If the strain residual rate is 70% or less, it is judged to have a sufficient deformation recovery force for practical use.
[0478] ((15) Color difference)
[0479] The b* value (yellow tint) of the pressed sheet of the thermoplastic elastomer composition obtained in the above [Production of Thermoplastic Elastomer] was measured using a colorimeter [manufactured by Nippon Denshoku Kogyo Co., Ltd., color meter ZE6000 (product name)] in accordance with JIS Z8781-4.
[0480] The measurement method is a reflection method, and the sheet is placed on a 30 mm Φ sample stand, and a white sample pressing piece is placed thereon for measurement.
[0481] The determination was performed using the following criteria.
[0482] ○: b* value is less than 10, ×: b* value is 10 or more, and ○ is evaluated as being good in practical use.
[0483] ((16) Transparency)
[0484] The haze value of a 2 mm thick pressed sheet of the thermoplastic elastomer composition obtained in the above [Production of Thermoplastic Elastomer] was measured using a haze meter [HZ-V3 (product name) manufactured by SUGA TEST INSTRUMENTS CO., LTD.] in accordance with JIS K7136 to evaluate transparency.
[0485] A haze value of more than 85% was judged to be non-transparent, and a haze value of 85% or less was judged to be transparent.
[0486] [Manufacturing of Multilayer Molded Body]
[0487] Using the pellets of the thermoplastic elastomer composition obtained in the above-mentioned [Manufacture of Thermoplastic Elastomer], a pre-molded thermoplastic resin molded product containing a polar group of 95 mm × 145 mm × thickness 2 mm is inserted into the mold cavity using an injection molding machine FNX110III-18A (manufactured by Nissei Plastic Industry Co., Ltd.), and a thermoplastic elastomer composition of 100 mm × 150 mm × thickness 2 mm is injection molded on its surface.
[0488] In addition, the conditions of injection molding are resin temperature: 240° C., injection speed: 40 mm / sec., extrusion time: 10 sec., mold temperature: 40° C., and cooling time: 30 sec.
[0489] [Evaluation method of multilayer molded body]
[0490] ((16) Thermal fusion strength)
[0491] Using the above-mentioned multilayer molded body, the heat fusion strength of the thermoplastic elastomer composition and the thermoplastic resin containing a polar group was measured by a 90-degree peel test. A notch with a width of 10 mm was cut on the surface of the thermoplastic elastomer composition side of the multilayer molded body, and the end thereof was peeled off several cm in advance. At the peeled portion, the layer composed of the thermoplastic elastomer composition and the layer composed of the thermoplastic resin containing a polar group were separately fixed to the chuck of a tensile testing machine [TGE-500N (product name) manufactured by Minebea Mitsumi Co., Ltd.]. The layer composed of the thermoplastic elastomer composition and the layer composed of the thermoplastic resin containing a polar group were stretched at 300 mm / min in the 90°C direction, thereby peeling the two layers. The tensile stress applied during the peeling was used as the heat fusion strength (N / cm) of the multilayer molded body of the thermoplastic elastomer composition and the thermoplastic resin containing a polar group, and the evaluation was performed according to the following evaluation criteria.
[0492] The evaluation was made into the following 1 to 5, 5 was evaluated as very excellent, and 4 was evaluated as practically good.
[0493] <Evaluation Criteria for Thermal Weld Strength>
[0494] 5: 20N / cm or more
[0495] 4: 10N / cm or more and less than 20N / cm
[0496] 3: 5N / cm or more and less than 10N / cm
[0497] 2: 1N / cm or more and less than 5N / cm
[0498] 1: Less than 1N / cm
[0499] [Components used in production of thermoplastic elastomer composition]
[0500] Hereinafter, each component used for producing the thermoplastic elastomer composition will be described.
[0501] (Preparation of Hydrogenation Catalyst)
[0502] The hydrogenation catalyst used in producing the hydrogenated block copolymer described below was prepared by the following method.
[0503] A reaction container equipped with a stirring device was purged with nitrogen in advance, and 1 L of dried and purified cyclohexane was added thereto.
[0504] Next, 100 mmol of bis(η5-cyclopentadienyl)titanium dichloride was added.
[0505] While the mixture was sufficiently stirred, a n-hexane solution containing 200 mmol of trimethylaluminum was added, and the mixture was reacted at room temperature for about 3 days to obtain a hydrogenation catalyst.
[0506] (Hydrogenated block copolymer (1))
[0507] A tank-type reactor with an internal volume of 100 L and equipped with a stirring device and a jacket was cleaned, dried, and replaced with nitrogen to carry out batch polymerization.
[0508] First, a cyclohexane solution containing 16 parts by mass of styrene monomer was charged, and then 0.062 parts by mass of n-butyl lithium per 100 parts by mass of all monomers and 0.34 mol of tetramethylethylenediamine (hereinafter referred to as TMEDA) per 1 mol of n-butyl lithium were added, and polymerization was carried out at 70° C. for 25 minutes.
[0509] Next, a cyclohexane solution containing 68 parts by mass of 1,3-butadiene monomer was added, and polymerization was carried out at 70° C. for 40 minutes.
[0510] Finally, a cyclohexane solution containing 16 parts by mass of styrene monomer was added and polymerized at 70° C. for 25 minutes.
[0511] After the polymerization reaction was completed, 0.95 mol of methanol was added to 1 mol of n-butyl lithium to deactivate the reaction catalyst, thereby obtaining a block copolymer.
[0512] Next, the above-mentioned hydrogenation catalyst was added to the obtained block copolymer in an amount of 100 ppm in terms of titanium per 100 parts by mass of the block copolymer, and a hydrogenation reaction was carried out under the conditions of a hydrogen pressure of 0.8 MPa and a temperature of 85°C.
[0513] After the hydrogenation reaction was completed, 0.3 parts by mass of octadecyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate was added as a stabilizer based on 100 parts by mass of the block copolymer to obtain a hydrogenated block copolymer (1).
[0514] The obtained hydrogenated block copolymer (1) had a total styrene content of 31.8% by mass, a styrene content in the polystyrene block A of 98.7% by mass, a vinyl bond content in the polybutadiene block before hydrogenation of 35.5 mol%, a weight average molecular weight of the entire polymer of 296,000, and a molecular weight distribution of 1.21. In addition, the hydrogenation rate of the aliphatic double bonds derived from 1,3-butadiene was 99.5%.
[0515] (Hydrogenated block copolymer (2))
[0516] A tank-type reactor with an internal volume of 100 L and equipped with a stirring device and a jacket was cleaned, dried, and replaced with nitrogen to carry out batch polymerization.
[0517] First, a cyclohexane solution containing 16 parts by mass of styrene monomer was charged, and then 0.088 parts by mass of n-butyl lithium per 100 parts by mass of all monomers and 0.34 mol of tetramethylethylenediamine (hereinafter referred to as TMEDA) per 1 mol of n-butyl lithium were added, and polymerization was carried out at 70° C. for 25 minutes.
[0518] Next, a cyclohexane solution containing 68 parts by mass of 1,3-butadiene monomer was added, and polymerization was carried out at 70° C. for 40 minutes.
[0519] Finally, a cyclohexane solution containing 16 parts by mass of styrene monomer was added and polymerized at 70° C. for 25 minutes.
[0520] After the polymerization reaction was completed, 0.95 mol of methanol was added to 1 mol of n-butyl lithium to deactivate the reaction catalyst, thereby obtaining a block copolymer.
[0521] Next, the above-mentioned hydrogenation catalyst was added to the obtained block copolymer in an amount of 100 ppm in terms of titanium per 100 parts by mass of the block copolymer, and a hydrogenation reaction was carried out under the conditions of a hydrogen pressure of 0.8 MPa and a temperature of 85°C.
[0522] After the hydrogenation reaction was completed, 0.3 parts by mass of octadecyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate was added as a stabilizer based on 100 parts by mass of the block copolymer to obtain a hydrogenated block copolymer (2).
[0523] The obtained hydrogenated block copolymer (2) had a total styrene content of 32.3% by mass, a styrene content in the polystyrene block A of 99.2% by mass, a vinyl bond content in the polybutadiene block before hydrogenation of 34.6 mol%, a weight average molecular weight of the entire polymer of 176,000, and a molecular weight distribution of 1.23. In addition, the hydrogenation rate of the aliphatic double bonds derived from 1,3-butadiene was 99.2%.
[0524] (Hydrogenated block copolymer (3))
[0525] A tank-type reactor with an internal volume of 100 L and equipped with a stirring device and a jacket was cleaned, dried, and replaced with nitrogen to carry out batch polymerization.
[0526] First, a cyclohexane solution containing 16 parts by mass of styrene monomer was charged, and then 0.062 parts by mass of n-butyl lithium per 100 parts by mass of all monomers and 0.34 mol of tetramethylethylenediamine (hereinafter referred to as TMEDA) per 1 mol of n-butyl lithium were added, and polymerization was carried out at 70° C. for 25 minutes.
[0527] Next, a cyclohexane solution containing 68 parts by mass of 1,3-butadiene monomer was added, and polymerization was carried out at 70° C. for 40 minutes.
[0528] Finally, a cyclohexane solution containing 16 parts by mass of styrene monomer was added and polymerized at 70° C. for 25 minutes.
[0529] After the polymerization reaction was completed, 0.95 mol of methanol was added to 1 mol of n-butyl lithium to deactivate the reaction catalyst, thereby obtaining a block copolymer.
[0530] Next, the above-mentioned hydrogenation catalyst was added to the obtained block copolymer in an amount of 70 ppm in terms of titanium per 100 parts by mass of the block copolymer, and a hydrogenation reaction was carried out under the conditions of a hydrogen pressure of 0.8 MPa and a temperature of 85°C.
[0531] After the hydrogenation reaction was completed, 0.3 parts by mass of octadecyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate was added as a stabilizer based on 100 parts by mass of the block copolymer to obtain a hydrogenated block copolymer (3).
[0532] The obtained hydrogenated block copolymer (3) had a total styrene content of 32.1% by mass, a styrene content in the polystyrene block A of 99.1% by mass, a vinyl bond content in the polybutadiene block before hydrogenation of 35.1% by mole, a weight average molecular weight of the entire polymer of 293,000, and a molecular weight distribution of 1.19. In addition, the hydrogenation rate of the aliphatic double bonds derived from 1,3-butadiene was 70.8%.
[0533] (Hydrogenated block copolymer (4))
[0534] A tank-type reactor with an internal volume of 100 L and equipped with a stirring device and a jacket was cleaned, dried, and replaced with nitrogen to carry out batch polymerization.
[0535] First, a cyclohexane solution containing 16 parts by mass of styrene monomer was charged, and then 0.062 parts by mass of n-butyl lithium per 100 parts by mass of all monomers and 0.25 mol of tetramethylethylenediamine (hereinafter referred to as TMEDA) per 1 mol of n-butyl lithium were added, and polymerization was carried out at 70° C. for 25 minutes.
[0536] Next, a cyclohexane solution containing 68 parts by mass of 1,3-butadiene monomer was added, and polymerization was carried out at 70° C. for 40 minutes.
[0537] Finally, a cyclohexane solution containing 16 parts by mass of styrene monomer was added and polymerized at 70° C. for 25 minutes.
[0538] After the polymerization reaction was completed, 0.95 mol of methanol was added to 1 mol of n-butyl lithium to deactivate the reaction catalyst, thereby obtaining a block copolymer.
[0539] Next, the above-mentioned hydrogenation catalyst was added to the obtained block copolymer in an amount of 100 ppm in terms of titanium per 100 parts by mass of the block copolymer, and a hydrogenation reaction was carried out under the conditions of a hydrogen pressure of 0.8 MPa and a temperature of 85°C.
[0540] After the hydrogenation reaction was completed, 0.3 parts by mass of octadecyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate was added as a stabilizer based on 100 parts by mass of the polymer to obtain a hydrogenated block copolymer (4).
[0541] The obtained hydrogenated block copolymer (4) had a total styrene content of 31.9 mass %, a styrene content in the polystyrene block A of 98.9 mass %, a vinyl bond content in the polybutadiene block before hydrogenation of 28.2 mol %, a weight average molecular weight of the entire polymer of 289,000, and a molecular weight distribution of 1.21. In addition, the hydrogenation rate of the aliphatic double bonds derived from 1,3-butadiene was 99.3%.
[0542] (Hydrogenated block copolymer (5))
[0543] A tank-type reactor with an internal volume of 100 L and equipped with a stirring device and a jacket was cleaned, dried, and replaced with nitrogen to carry out batch polymerization.
[0544] First, a cyclohexane solution containing 16 parts by mass of styrene monomer was charged, and then 0.060 parts by mass of n-butyl lithium per 100 parts by mass of all monomers and 0.55 mol of tetramethylethylenediamine (hereinafter referred to as TMEDA) per 1 mol of n-butyl lithium were added, and polymerization was carried out at 70° C. for 25 minutes.
[0545] Next, a cyclohexane solution containing 68 parts by mass of 1,3-butadiene monomer was added, and polymerization was carried out at 70° C. for 40 minutes.
[0546] Finally, a cyclohexane solution containing 16 parts by mass of styrene monomer was added and polymerized at 70° C. for 25 minutes.
[0547] After the polymerization reaction was completed, 0.95 mol of methanol was added to 1 mol of n-butyl lithium to deactivate the reaction catalyst, thereby obtaining a block copolymer.
[0548] Next, the above-mentioned hydrogenation catalyst was added to the obtained block copolymer in an amount of 100 ppm in terms of titanium per 100 parts by mass of the block copolymer, and a hydrogenation reaction was carried out under the conditions of a hydrogen pressure of 0.8 MPa and a temperature of 85°C.
[0549] After the hydrogenation reaction was completed, 0.3 parts by mass of octadecyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate was added as a stabilizer based on 100 parts by mass of the polymer to obtain a hydrogenated block copolymer (5).
[0550] The obtained hydrogenated block copolymer (5) had a total styrene content of 32.2% by mass, a styrene content in the polystyrene block A of 98.8% by mass, a vinyl bond content in the polybutadiene block before hydrogenation of 48.7 mol%, a weight average molecular weight of the entire polymer of 302,000, and a molecular weight distribution of 1.24. In addition, the hydrogenation rate of the aliphatic double bonds derived from 1,3-butadiene was 99.4%.
[0551] (Hydrogenated block copolymer (6))
[0552] A tank-type reactor with an internal volume of 100 L and equipped with a stirring device and a jacket was cleaned, dried, and replaced with nitrogen to carry out batch polymerization.
[0553] First, a cyclohexane solution containing 20 parts by mass of styrene monomer was charged, and then 0.080 parts by mass of n-butyl lithium per 100 parts by mass of all monomers and 1.2 mol of TMEDA per 1 mol of n-butyl lithium were added, followed by polymerization at 70° C. for 25 minutes.
[0554] Next, a cyclohexane solution containing 80 parts by mass of 1,3-butadiene monomer was added, and polymerization was carried out at 70° C. for 40 minutes.
[0555] After the polymerization reaction was completed, tetramethoxysilane (hereinafter also referred to as "TMS") was added so that the molar ratio of Si to Li (Si / Li) was 0.24 mol. After stirring for 20 minutes, 0.1 mol of methanol was added relative to 1 mol of n-butyl lithium to deactivate the reaction catalyst and obtain a block copolymer.
[0556] Next, the above-mentioned hydrogenation catalyst was added to the obtained block copolymer in an amount of 100 ppm in terms of titanium per 100 parts by mass of the block copolymer, and a hydrogenation reaction was carried out under the conditions of a hydrogen pressure of 0.8 MPa and a temperature of 85° C. After the hydrogenation reaction was completed, 0.3 parts by mass of octadecyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate as a stabilizer was added per 100 parts by mass of the polymer to obtain a hydrogenated block copolymer (6).
[0557] The obtained hydrogenated block copolymer (6) had a total styrene content of 20.3% by mass, a styrene content in the polystyrene block A of 98.5% by mass, a vinyl bond content in the polybutadiene block before hydrogenation of 58.6 mol%, a weight average molecular weight of the entire polymer of 453,000, and a molecular weight distribution of 1.28. In addition, the hydrogenation rate of the aliphatic double bonds derived from 1,3-butadiene was 99.3%.
[0558] (Hydrogenated block copolymer (7))
[0559] A tank-type reactor with an internal volume of 100 L and equipped with a stirring device and a jacket was cleaned, dried, and replaced with nitrogen to carry out batch polymerization.
[0560] First, a cyclohexane solution containing 5 parts by mass of 1,3-butadiene monomer was added, and then 0.109 parts by mass of n-butyl lithium per 100 parts by mass of all monomers, 1.6 mol of TMEDA per 1 mol of n-butyl lithium, and 0.04 mol of sodium tert-amyl alcohol per 1 mol of n-butyl lithium were added, and polymerization was carried out at 60° C. for 20 minutes.
[0561] Next, a cyclohexane solution containing 18 parts by mass of a styrene monomer was added, and polymerization was carried out at 70° C. for 25 minutes. Further, a cyclohexane solution containing 59 parts by mass of a 1,3-butadiene monomer was added, and polymerization was carried out at 60° C. for 1 hour.
[0562] Finally, a cyclohexane solution containing 18 parts by mass of styrene monomer was added and polymerized for 25 minutes at 70° C. After the polymerization reaction, 0.95 mol of methanol was added per 1 mol of n-butyl lithium to deactivate the reaction catalyst, thereby obtaining a block copolymer.
[0563] Next, the above-mentioned hydrogenation catalyst was added to the obtained block copolymer in an amount of 100 ppm in terms of titanium per 100 parts by mass of the block copolymer, and a hydrogenation reaction was carried out under the conditions of a hydrogen pressure of 0.8 MPa and a temperature of 85° C. After the hydrogenation reaction was completed, 0.3 parts by mass of octadecyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate as a stabilizer was added per 100 parts by mass of the polymer to obtain a hydrogenated block copolymer (7).
[0564] The obtained hydrogenated block copolymer (7) had a total styrene content of 36.2% by mass, a styrene content in the polystyrene block A of 99.1% by mass, a vinyl bond content in the polybutadiene block before hydrogenation of 76.2% by mole, a weight average molecular weight of the entire polymer of 137,000, and a molecular weight distribution of 1.18. In addition, the hydrogenation rate of the aliphatic double bonds derived from 1,3-butadiene was 99.4%.
[0565] (Hydrogenated block copolymer (8))
[0566] A tank-type reactor with an internal volume of 100 L and equipped with a stirring device and a jacket was cleaned, dried, and replaced with nitrogen to carry out batch polymerization.
[0567] First, a cyclohexane solution containing 5 parts by mass of 1,3-butadiene monomer was added, and then 0.125 parts by mass of n-butyl lithium per 100 parts by mass of all monomers, 1.6 mol of TMEDA per 1 mol of n-butyl lithium, and 0.04 mol of sodium tert-amyl alcohol per 1 mol of n-butyl lithium were added, and polymerization was carried out at 60° C. for 20 minutes.
[0568] Next, a cyclohexane solution containing 22 parts by mass of a styrene monomer was added, and polymerization was carried out at 70° C. for 25 minutes. Further, a cyclohexane solution containing 52 parts by mass of a 1,3-butadiene monomer was added, and polymerization was carried out at 60° C. for 1 hour.
[0569] Finally, a cyclohexane solution containing 21 parts by mass of styrene monomer was added and polymerized for 25 minutes at 70° C. After the polymerization reaction was completed, 0.95 mol of methanol was added per 1 mol of n-butyl lithium to deactivate the reaction catalyst, thereby obtaining a block copolymer.
[0570] Next, the above-mentioned hydrogenation catalyst was added to the obtained block copolymer in an amount of 100 ppm in terms of titanium per 100 parts by mass of the block copolymer, and a hydrogenation reaction was carried out under the conditions of a hydrogen pressure of 0.8 MPa and a temperature of 85° C. After the hydrogenation reaction was completed, 0.3 parts by mass of octadecyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate as a stabilizer was added per 100 parts by mass of the polymer to obtain a hydrogenated block copolymer (8).
[0571] The obtained hydrogenated block copolymer (8) had a total styrene content of 43.2% by mass, a styrene content in the polystyrene block A of 99.2% by mass, a vinyl bond content in the polybutadiene block before hydrogenation of 77.8% by mole, a weight average molecular weight of the entire polymer of 108,000, and a molecular weight distribution of 1.19. In addition, the hydrogenation rate of the aliphatic double bonds derived from 1,3-butadiene was 99.5%.
[0572] (Hydrogenated block copolymer (9))
[0573] A tank-type reactor with an internal volume of 100 L and equipped with a stirring device and a jacket was cleaned, dried, and replaced with nitrogen to carry out batch polymerization.
[0574] First, a cyclohexane solution containing 5 parts by mass of 1,3-butadiene monomer was added, and then 0.125 parts by mass of n-butyl lithium relative to 100 parts by mass of all monomers, 1.4 mol of TMEDA relative to 1 mol of n-butyl lithium, and 0.04 mol of sodium tert-amyl alcohol relative to 1 mol of n-butyl lithium were added, and polymerization was carried out at 60° C. for 20 minutes.
[0575] Next, a cyclohexane solution containing 22 parts by mass of a styrene monomer was added, and polymerization was carried out at 70° C. for 25 minutes. Further, a cyclohexane solution containing 52 parts by mass of a 1,3-butadiene monomer was added, and polymerization was carried out at 60° C. for 1 hour.
[0576] Finally, a cyclohexane solution containing 21 parts by mass of styrene monomer was added and polymerized for 25 minutes at 70° C. After the polymerization reaction was completed, 0.95 mol of methanol was added per 1 mol of n-butyl lithium to deactivate the reaction catalyst, thereby obtaining a block copolymer.
[0577] Next, the above-mentioned hydrogenation catalyst was added in an amount of 70 ppm in terms of titanium per 100 parts by mass of the polymer, and a hydrogenation reaction was carried out under the conditions of a hydrogen pressure of 0.8 MPa and a temperature of 85° C. After the hydrogenation reaction was completed, 0.3 parts by mass of octadecyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate was added as a stabilizer per 100 parts by mass of the polymer to obtain a hydrogenated block copolymer (9).
[0578] The obtained hydrogenated block copolymer (9) had a total styrene content of 42.6% by mass, a styrene content in the polystyrene block A of 98.9% by mass, a vinyl bond content in the polybutadiene block before hydrogenation of 73.2 mol%, a weight average molecular weight of the entire polymer of 113,000, and a molecular weight distribution of 1.20. In addition, the hydrogenation rate of the aliphatic double bonds derived from 1,3-butadiene was 75.7%.
[0579] (Hydrogenated block copolymer (10))
[0580] A tank-type reactor with an internal volume of 100 L and equipped with a stirring device and a jacket was cleaned, dried, and replaced with nitrogen to carry out batch polymerization.
[0581] First, a cyclohexane solution containing 5 parts by mass of 1,3-butadiene monomer was added, and then 0.25 parts by mass of n-butyl lithium per 100 parts by mass of all monomers, 1.6 mol of TMEDA per 1 mol of n-butyl lithium, and 0.04 mol of sodium tert-amyl alcohol per 1 mol of n-butyl lithium were added, and polymerization was carried out at 60° C. for 20 minutes.
[0582] Next, a cyclohexane solution containing 28 parts by mass of a styrene monomer was added, and polymerization was carried out at 70° C. for 30 minutes. Furthermore, a cyclohexane solution containing 40 parts by mass of a 1,3-butadiene monomer was added, and polymerization was carried out at 60° C. for 1 hour.
[0583] Finally, a cyclohexane solution containing 27 parts by mass of styrene monomer was added and polymerized for 30 minutes at 70° C. After the polymerization reaction was completed, 0.95 mol of methanol was added per 1 mol of n-butyl lithium to deactivate the reaction catalyst, thereby obtaining a block copolymer.
[0584] Next, the above-mentioned hydrogenation catalyst was added to the obtained block copolymer in an amount of 100 ppm in terms of titanium per 100 parts by mass of the block copolymer, and a hydrogenation reaction was carried out under the conditions of a hydrogen pressure of 0.8 MPa and a temperature of 85° C. After the hydrogenation reaction was completed, 0.3 parts by mass of octadecyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate as a stabilizer was added per 100 parts by mass of the polymer to obtain a hydrogenated block copolymer (10).
[0585] The obtained hydrogenated block copolymer (10) had a total styrene content of 54.7% by mass, a styrene content in the polystyrene block A of 99.4% by mass, a vinyl bond content in the polybutadiene block before hydrogenation of 77.3% by mole, a weight average molecular weight of the entire polymer of 41,000, and a molecular weight distribution of 1.15. In addition, the hydrogenation rate of the aliphatic double bonds derived from 1,3-butadiene was 99.3%.
[0586] (Hydrogenated block copolymer (11))
[0587] A tank-type reactor with an internal volume of 100 L and equipped with a stirring device and a jacket was cleaned, dried, and replaced with nitrogen to carry out batch polymerization.
[0588] First, a cyclohexane solution containing 22 parts by mass of styrene monomer was added, and then 0.125 parts by mass of n-butyl lithium relative to 100 parts by mass of all monomers, 1.6 mol of TMEDA relative to 1 mol of n-butyl lithium, and 0.04 mol of sodium tert-amyl alcohol relative to 1 mol of n-butyl lithium were added, and polymerization was carried out at 70° C. for 25 minutes.
[0589] Next, a cyclohexane solution containing 57 parts by mass of a 1,3-butadiene monomer was added, and polymerization was carried out at 60° C. for 1 hour.
[0590] Finally, a cyclohexane solution containing 21 parts by mass of styrene monomer was added and polymerized for 25 minutes at 70° C. After the polymerization reaction was completed, 0.95 mol of methanol was added per 1 mol of n-butyl lithium to deactivate the reaction catalyst, thereby obtaining a block copolymer.
[0591] Next, the above-mentioned hydrogenation catalyst was added to the obtained block copolymer in an amount of 100 ppm in terms of titanium per 100 parts by mass of the block copolymer, and a hydrogenation reaction was carried out under the conditions of a hydrogen pressure of 0.8 MPa and a temperature of 85° C. After the hydrogenation reaction was completed, 0.3 parts by mass of octadecyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate as a stabilizer was added per 100 parts by mass of the polymer to obtain a hydrogenated block copolymer (11).
[0592] The obtained hydrogenated block copolymer (11) had a total styrene content of 43.1% by mass, a styrene content in the polystyrene block A of 99.1% by mass, a vinyl bond content in the polybutadiene block before hydrogenation of 76.8% by mole, a weight average molecular weight of the entire polymer of 103,000, and a molecular weight distribution of 1.14. In addition, the hydrogenation rate of the aliphatic double bonds derived from 1,3-butadiene was 99.6%.
[0593] (Hydrogenated block copolymer (12))
[0594] A tank-type reactor with an internal volume of 100 L and equipped with a stirring device and a jacket was cleaned, dried, and replaced with nitrogen to carry out batch polymerization.
[0595] First, a cyclohexane solution containing 5 parts by mass of 1,3-butadiene monomer was charged, and then 0.125 parts by mass of n-butyl lithium per 100 parts by mass of all monomers and 0.8 mol of TMEDA per 1 mol of n-butyl lithium were added, followed by polymerization at 70° C. for 20 minutes.
[0596] Next, a cyclohexane solution containing 22 parts by mass of a styrene monomer was added, and polymerization was carried out at 70° C. for 25 minutes. Further, a cyclohexane solution containing 52 parts by mass of a 1,3-butadiene monomer was added, and polymerization was carried out at 70° C. for 40 minutes.
[0597] Finally, a cyclohexane solution containing 21 parts by mass of styrene monomer was added and polymerized for 25 minutes at 70° C. After the polymerization reaction was completed, 0.95 mol of methanol was added per 1 mol of n-butyl lithium to deactivate the reaction catalyst, thereby obtaining a block copolymer.
[0598] Next, the above-mentioned hydrogenation catalyst was added to the obtained block copolymer in an amount of 100 ppm in terms of titanium per 100 parts by mass of the block copolymer, and a hydrogenation reaction was carried out under the conditions of a hydrogen pressure of 0.8 MPa and a temperature of 85° C. After the hydrogenation reaction was completed, 0.3 parts by mass of octadecyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate as a stabilizer was added per 100 parts by mass of the polymer to obtain a hydrogenated block copolymer (12).
[0599] The obtained hydrogenated block copolymer (12) had a total styrene content of 43.1% by mass, a styrene content in the polystyrene block A of 99.0% by mass, a vinyl bond content in the polybutadiene block before hydrogenation of 62.5% by mole, a weight average molecular weight of the entire polymer of 102,000, and a molecular weight distribution of 1.13. In addition, the hydrogenation rate of the aliphatic double bonds derived from 1,3-butadiene was 99.4%.
[0600] (Hydrogenated block copolymer (13))
[0601] A tank-type reactor with an internal volume of 100 L and equipped with a stirring device and a jacket was cleaned, dried, and replaced with nitrogen to carry out batch polymerization.
[0602] First, a cyclohexane solution containing 0.5 parts by mass of 1,3-butadiene monomer was added, and then 0.125 parts by mass of n-butyl lithium relative to 100 parts by mass of all monomers, 1.6 mol of TMEDA relative to 1 mol of n-butyl lithium, and 0.04 mol of sodium tert-amyl alcohol relative to 1 mol of n-butyl lithium were added, and polymerization was carried out at 60° C. for 10 minutes.
[0603] Next, a cyclohexane solution containing 22 parts by mass of a styrene monomer was added, and polymerization was carried out at 70° C. for 25 minutes. Further, a cyclohexane solution containing 56.5 parts by mass of a 1,3-butadiene monomer was added, and polymerization was carried out at 60° C. for 1 hour.
[0604] Finally, a cyclohexane solution containing 21 parts by mass of styrene monomer was added and polymerized for 25 minutes at 70° C. After the polymerization reaction was completed, 0.95 mol of methanol was added per 1 mol of n-butyl lithium to deactivate the reaction catalyst, thereby obtaining a block copolymer.
[0605] Next, the above-mentioned hydrogenation catalyst was added to the obtained block copolymer in an amount of 100 ppm in terms of titanium per 100 parts by mass of the block copolymer, and a hydrogenation reaction was carried out under the conditions of a hydrogen pressure of 0.8 MPa and a temperature of 85° C. After the hydrogenation reaction was completed, 0.3 parts by mass of octadecyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate as a stabilizer was added per 100 parts by mass of the polymer to obtain a hydrogenated block copolymer (13).
[0606] The obtained hydrogenated block copolymer (13) had a total styrene content of 43.1% by mass, a styrene content in the polystyrene block A of 99.5% by mass, a vinyl bond content in the polybutadiene block before hydrogenation of 76.8% by mole, a weight average molecular weight of the entire polymer of 103,000, and a molecular weight distribution of 1.13. In addition, the hydrogenation rate of the aliphatic double bonds derived from 1,3-butadiene was 99.1%.
[0607] (Hydrogenated block copolymer (14))
[0608] A tank-type reactor with an internal volume of 100 L and equipped with a stirring device and a jacket was cleaned, dried, and replaced with nitrogen to carry out batch polymerization.
[0609] First, a cyclohexane solution containing 13 parts by mass of 1,3-butadiene monomer was added, and then 0.125 parts by mass of n-butyl lithium relative to 100 parts by mass of all monomers, 1.6 mol of TMEDA relative to 1 mol of n-butyl lithium, and 0.04 mol of sodium tert-amyl alcohol relative to 1 mol of n-butyl lithium were added, and polymerization was carried out at 60° C. for 30 minutes.
[0610] Next, a cyclohexane solution containing 22 parts by mass of a styrene monomer was added, and polymerization was carried out at 70° C. for 25 minutes. Furthermore, a cyclohexane solution containing 44 parts by mass of a 1,3-butadiene monomer was added, and polymerization was carried out at 60° C. for 1 hour.
[0611] Finally, a cyclohexane solution containing 21 parts by mass of styrene monomer was added and polymerized for 25 minutes at 70° C. After the polymerization reaction was completed, 0.95 mol of methanol was added per 1 mol of n-butyl lithium to deactivate the reaction catalyst, thereby obtaining a block copolymer.
[0612] Next, the above-mentioned hydrogenation catalyst was added to the obtained block copolymer in an amount of 100 ppm in terms of titanium per 100 parts by mass of the block copolymer, and a hydrogenation reaction was carried out under the conditions of a hydrogen pressure of 0.8 MPa and a temperature of 85° C. After the hydrogenation reaction was completed, 0.3 parts by mass of octadecyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate as a stabilizer was added per 100 parts by mass of the polymer to obtain a hydrogenated block copolymer (14).
[0613] The obtained hydrogenated block copolymer (14) had a total styrene content of 43.4% by mass, a styrene content in the polystyrene block A of 99.3% by mass, a vinyl bond content in the polybutadiene block before hydrogenation of 78.1% by mole, a weight average molecular weight of the entire polymer of 104,000, and a molecular weight distribution of 1.15. In addition, the hydrogenation rate of the aliphatic double bonds derived from 1,3-butadiene was 99.4%.
[0614] (Hydrogenated block copolymer (15))
[0615] A tank-type reactor with an internal volume of 100 L and equipped with a stirring device and a jacket was cleaned, dried, and replaced with nitrogen to carry out batch polymerization.
[0616] First, a cyclohexane solution containing 5 parts by mass of 1,3-butadiene monomer was added, and then 0.125 parts by mass of n-butyl lithium per 100 parts by mass of all monomers, 1.9 mol of TMEDA per 1 mol of n-butyl lithium, and 0.04 mol of sodium tert-amyl alcohol per 1 mol of n-butyl lithium were added, and polymerization was carried out at 60° C. for 20 minutes.
[0617] Next, a cyclohexane solution containing 22 parts by mass of a styrene monomer was added, and polymerization was carried out at 70° C. for 25 minutes. Further, a cyclohexane solution containing 52 parts by mass of a 1,3-butadiene monomer was added, and polymerization was carried out at 60° C. for 1 hour.
[0618] Finally, a cyclohexane solution containing 21 parts by mass of styrene monomer was added and polymerized for 25 minutes at 70° C. After the polymerization reaction was completed, 0.95 mol of methanol was added per 1 mol of n-butyl lithium to deactivate the reaction catalyst, thereby obtaining a block copolymer.
[0619] Next, the above-mentioned hydrogenation catalyst was added to the obtained block copolymer in an amount of 100 ppm in terms of titanium per 100 parts by mass of the block copolymer, and a hydrogenation reaction was carried out under the conditions of a hydrogen pressure of 0.8 MPa and a temperature of 85° C. After the hydrogenation reaction was completed, 0.3 parts by mass of octadecyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate as a stabilizer was added per 100 parts by mass of the polymer to obtain a hydrogenated block copolymer (15).
[0620] The obtained hydrogenated block copolymer (15) had a total styrene content of 43.2% by mass, a styrene content in the polystyrene block A of 98.9% by mass, a vinyl bond content in the polybutadiene block before hydrogenation of 83.6 mol%, a weight average molecular weight of the entire polymer of 107,000, and a molecular weight distribution of 1.18. In addition, the hydrogenation rate of the aliphatic double bonds derived from 1,3-butadiene was 99.2%.
[0621] (Hydrogenated block copolymer (16))
[0622] A tank-type reactor with an internal volume of 100 L and equipped with a stirring device and a jacket was cleaned, dried, and replaced with nitrogen to carry out batch polymerization.
[0623] First, a cyclohexane solution containing 16 parts by mass of styrene monomer was added, and then 0.140 parts by mass of n-butyl lithium relative to 100 parts by mass of all monomers, 0.7 mol of TMEDA relative to 1 mol of n-butyl lithium, and 0.04 mol of sodium tert-amyl alcohol relative to 1 mol of n-butyl lithium were added, and polymerization was carried out at 70° C. for 25 minutes.
[0624] Next, a cyclohexane solution containing 7 parts by mass of 1,3-butadiene monomer was added and polymerized at 70°C for 15 minutes, and a cyclohexane solution containing 33 parts by mass of styrene monomer and 20 parts by mass of 1,3-butadiene monomer was further added and polymerized at 70°C for 1 hour.
[0625] Then, a cyclohexane solution containing 15 parts by mass of styrene monomer was added, and polymerization was carried out at 70° C. for 25 minutes.
[0626] Finally, a cyclohexane solution containing 9 parts by mass of 1,3-butadiene monomer was added and polymerized at 70° C. for 15 minutes. After the polymerization reaction was completed, 0.95 mol of methanol was added per 1 mol of n-butyl lithium to deactivate the reaction catalyst, thereby obtaining a block copolymer.
[0627] Next, the above-mentioned hydrogenation catalyst was added to the obtained block copolymer in an amount of 100 ppm in terms of titanium per 100 parts by mass of the block copolymer, and a hydrogenation reaction was carried out under the conditions of a hydrogen pressure of 0.8 MPa and a temperature of 85° C. After the hydrogenation reaction was completed, 0.3 parts by mass of octadecyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate as a stabilizer was added per 100 parts by mass of the polymer to obtain a hydrogenated block copolymer (16).
[0628] The obtained hydrogenated block copolymer (16) had a total styrene content of 64.1% by mass, a styrene content in the polystyrene block A of 98.8% by mass, a styrene content in the polystyrene block A' of 60.6% by mass, a vinyl bond content in the polybutadiene block before hydrogenation of 65.3% by mole, a weight average molecular weight of the entire polymer of 94,000, and a molecular weight distribution of 1.21. In addition, the hydrogenation rate of the aliphatic double bonds derived from 1,3-butadiene was 99.4%.
[0629] (Hydrogenated block copolymer (17))
[0630] A tank-type reactor with an internal volume of 100 L and equipped with a stirring device and a jacket was cleaned, dried, and replaced with nitrogen to carry out batch polymerization.
[0631] First, a cyclohexane solution containing 16 parts by mass of styrene monomer was added, and then 0.130 parts by mass of n-butyl lithium relative to 100 parts by mass of all monomers, 0.7 mol of TMEDA relative to 1 mol of n-butyl lithium, and 0.04 mol of sodium tert-amyl alcohol relative to 1 mol of n-butyl lithium were added, and polymerization was carried out at 70° C. for 25 minutes.
[0632] Next, a cyclohexane solution containing 7 parts by mass of 1,3-butadiene monomer was added and polymerized at 70°C for 15 minutes, and a cyclohexane solution containing 29 parts by mass of styrene monomer and 24 parts by mass of 1,3-butadiene monomer was further added and polymerized at 70°C for 1 hour.
[0633] Then, a cyclohexane solution containing 15 parts by mass of styrene monomer was added, and polymerization was carried out at 70° C. for 25 minutes.
[0634] Finally, a cyclohexane solution containing 9 parts by mass of 1,3-butadiene monomer was added and polymerized at 70° C. for 15 minutes. After the polymerization reaction was completed, 0.95 mol of methanol was added per 1 mol of n-butyl lithium to deactivate the reaction catalyst, thereby obtaining a block copolymer.
[0635] Next, the above-mentioned hydrogenation catalyst was added to the obtained block copolymer in an amount of 100 ppm in terms of titanium per 100 parts by mass of the block copolymer, and a hydrogenation reaction was carried out under the conditions of a hydrogen pressure of 0.8 MPa and a temperature of 85° C. After the hydrogenation reaction was completed, 0.3 parts by mass of octadecyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate as a stabilizer was added per 100 parts by mass of the polymer to obtain a hydrogenated block copolymer (17).
[0636] The obtained hydrogenated block copolymer (17) had a total styrene content of 60.2% by mass, a styrene content in the polystyrene block A of 98.6% by mass, a styrene content in the polystyrene block A' of 52.1% by mass, a vinyl bond content in the polybutadiene block before hydrogenation of 64.8 mol%, a weight average molecular weight of the entire polymer of 106,000, and a molecular weight distribution of 1.25. In addition, the hydrogenation rate of the aliphatic double bonds derived from 1,3-butadiene was 98.6%.
[0637] (Hydrogenated block copolymer (18))
[0638] A tank-type reactor with an internal volume of 100 L and equipped with a stirring device and a jacket was cleaned, dried, and replaced with nitrogen to carry out batch polymerization.
[0639] First, a cyclohexane solution containing 5 parts by mass of 1,3-butadiene monomer was added, and then 0.086 parts by mass of n-butyl lithium relative to 100 parts by mass of all monomers, 1.5 mol of TMEDA relative to 1 mol of n-butyl lithium, and 0.04 mol of sodium tert-amyl oxide relative to 1 mol of n-butyl lithium were added, and polymerization was carried out at 60° C. for 20 minutes.
[0640] Next, a cyclohexane solution containing 7 parts by mass of a styrene monomer was added, and polymerization was carried out at 70° C. for 20 minutes. Furthermore, a cyclohexane solution containing 82 parts by mass of a 1,3-butadiene monomer was added, and polymerization was carried out at 60° C. for 1.5 hours.
[0641] Finally, a cyclohexane solution containing 6 parts by mass of styrene monomer was added and polymerized for 20 minutes at 70° C. After the polymerization reaction was completed, 0.95 mol of methanol was added per 1 mol of n-butyl lithium to deactivate the reaction catalyst, thereby obtaining a block copolymer.
[0642] Next, the above-mentioned hydrogenation catalyst was added to the obtained block copolymer in an amount of 100 ppm in terms of titanium per 100 parts by mass of the block copolymer, and a hydrogenation reaction was carried out under the conditions of a hydrogen pressure of 0.8 MPa and a temperature of 85° C. After the hydrogenation reaction was completed, 0.3 parts by mass of octadecyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate as a stabilizer was added per 100 parts by mass of the polymer to obtain a hydrogenated block copolymer (18).
[0643] The obtained hydrogenated block copolymer (18) had a total styrene content of 13.4% by mass, a styrene content in the polystyrene block A of 99.3% by mass, a vinyl bond content in the polybutadiene block before hydrogenation of 76.3% by mole, a weight average molecular weight of the entire polymer of 183,000, and a molecular weight distribution of 1.22. In addition, the hydrogenation rate of the aliphatic double bonds derived from 1,3-butadiene was 99.6%.
[0644] (Hydrogenated block copolymer (19))
[0645] A tank-type reactor with an internal volume of 100 L and equipped with a stirring device and a jacket was cleaned, dried, and replaced with nitrogen to carry out batch polymerization.
[0646] First, a cyclohexane solution containing 5 parts by mass of 1,3-butadiene monomer was charged, and then 0.125 parts by mass of n-butyl lithium per 100 parts by mass of all monomers and 0.4 mol of TMEDA per 1 mol of n-butyl lithium were added, followed by polymerization at 70° C. for 15 minutes.
[0647] Next, a cyclohexane solution containing 22 parts by mass of a styrene monomer was added, and polymerization was carried out at 70° C. for 25 minutes. Further, a cyclohexane solution containing 51 parts by mass of a 1,3-butadiene monomer was added, and polymerization was carried out at 70° C. for 40 minutes.
[0648] Finally, a cyclohexane solution containing 22 parts by mass of styrene monomer was added and polymerized for 25 minutes at 70° C. After the polymerization reaction was completed, 0.95 mol of methanol was added per 1 mol of n-butyl lithium to deactivate the reaction catalyst, thereby obtaining a block copolymer.
[0649] Next, the above-mentioned hydrogenation catalyst was added to the obtained block copolymer in an amount of 100 ppm in terms of titanium per 100 parts by mass of the block copolymer, and a hydrogenation reaction was carried out under the conditions of a hydrogen pressure of 0.8 MPa and a temperature of 85° C. After the hydrogenation reaction was completed, 0.3 parts by mass of octadecyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate as a stabilizer was added per 100 parts by mass of the polymer to obtain a hydrogenated block copolymer (19).
[0650] The obtained hydrogenated block copolymer (19) had a total styrene content of 44.1% by mass, a styrene content in the polystyrene block A of 99.5% by mass, a vinyl bond content in the polybutadiene block before hydrogenation of 39.6 mol%, a weight average molecular weight of the entire polymer of 102,000, and a molecular weight distribution of 1.13. In addition, the hydrogenation rate of the aliphatic double bonds derived from 1,3-butadiene was 99.2%.
[0651] (Hydrogenated block copolymer (20))
[0652] A tank-type reactor with an internal volume of 100 L and equipped with a stirring device and a jacket was cleaned, dried, and replaced with nitrogen to carry out batch polymerization.
[0653] First, a cyclohexane solution containing 5 parts by mass of 1,3-butadiene monomer was added, and then 0.125 parts by mass of n-butyl lithium relative to 100 parts by mass of all monomers, 1.4 mol of TMEDA relative to 1 mol of n-butyl lithium, and 0.04 mol of sodium tert-amyl alcohol relative to 1 mol of n-butyl lithium were added, and polymerization was carried out at 60° C. for 20 minutes.
[0654] Next, a cyclohexane solution containing 38 parts by mass of a styrene monomer was added, and polymerization was carried out at 70° C. for 35 minutes. Furthermore, a cyclohexane solution containing 19 parts by mass of a 1,3-butadiene monomer was added, and polymerization was carried out at 60° C. for 40 minutes.
[0655] Finally, a cyclohexane solution containing 38 parts by mass of styrene monomer was added and polymerized for 35 minutes at 70° C. After the polymerization reaction was completed, 0.95 mol of methanol was added per 1 mol of n-butyl lithium to deactivate the reaction catalyst, thereby obtaining a block copolymer.
[0656] Next, the above-mentioned hydrogenation catalyst was added to the obtained block copolymer in an amount of 100 ppm in terms of titanium per 100 parts by mass of the block copolymer, and a hydrogenation reaction was carried out under the conditions of a hydrogen pressure of 0.8 MPa and a temperature of 85° C. After the hydrogenation reaction was completed, 0.3 parts by mass of octadecyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate as a stabilizer was added per 100 parts by mass of the polymer to obtain a hydrogenated block copolymer (20).
[0657] The obtained hydrogenated block copolymer (20) had a total styrene content of 75.6% by mass, a styrene content in the polystyrene block A of 99.3% by mass, a vinyl bond content in the polybutadiene block before hydrogenation of 75.1% by mole, a weight average molecular weight of the entire polymer of 104,000, and a molecular weight distribution of 1.19. In addition, the hydrogenation rate of the aliphatic double bonds derived from 1,3-butadiene was 99.5%.
[0658] (Hydrogenated block copolymer (21))
[0659] A tank-type reactor with an internal volume of 100 L and equipped with a stirring device and a jacket was cleaned, dried, and replaced with nitrogen to carry out batch polymerization.
[0660] First, a cyclohexane solution containing 33 parts by mass of styrene monomer was charged, and then 0.198 parts by mass of n-butyl lithium per 100 parts by mass of all monomers and 0.4 mol of TMEDA per 1 mol of n-butyl lithium were added, and polymerization was carried out at 70° C. for 30 minutes.
[0661] Next, a cyclohexane solution containing 34 parts by mass of 1,3-butadiene monomer was added, and polymerization was carried out at 70° C. for 30 minutes. Finally, a cyclohexane solution containing 33 parts by mass of styrene monomer was added, and polymerization was carried out at 70° C. for 30 minutes.
[0662] After the polymerization reaction was completed, 0.95 mol of methanol was added to 1 mol of n-butyl lithium to deactivate the reaction catalyst, thereby obtaining a block copolymer.
[0663] Next, the above-mentioned hydrogenation catalyst was added to the obtained block copolymer in an amount of 100 ppm in terms of titanium per 100 parts by mass of the block copolymer, and a hydrogenation reaction was carried out under the conditions of a hydrogen pressure of 0.8 MPa and a temperature of 85° C. After the hydrogenation reaction was completed, 0.3 parts by mass of octadecyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate as a stabilizer was added per 100 parts by mass of the polymer to obtain a hydrogenated block copolymer (21).
[0664] The obtained hydrogenated block copolymer (21) had a total styrene content of 65.7% by mass, a polystyrene block content of 98.9% by mass, a vinyl bond content in the polybutadiene block before hydrogenation of 40.6 mol%, a weight average molecular weight of 57,000 for the entire polymer, and a molecular weight distribution of 1.16. In addition, the hydrogenation rate of the aliphatic double bonds derived from 1,3-butadiene was 99.5%.
[0665] (Hydrogenated block copolymer (22))
[0666] A tank-type reactor with an internal volume of 100 L and equipped with a stirring device and a jacket was cleaned, dried, and replaced with nitrogen to carry out batch polymerization.
[0667] First, a cyclohexane solution containing 10 parts by mass of styrene monomer was charged, and then 0.138 parts by mass of n-butyl lithium per 100 parts by mass of all monomers and 0.8 mol of TMEDA per 1 mol of n-butyl lithium were added, followed by polymerization at 70° C. for 20 minutes.
[0668] Next, a cyclohexane solution containing 47 parts by mass of a styrene monomer and 34 parts by mass of a 1,3-butadiene monomer was added, and polymerization was carried out at 70° C. for 50 minutes.
[0669] Finally, a cyclohexane solution containing 9 parts by mass of styrene monomer was added and polymerized for 20 minutes at 70° C. After the polymerization reaction was completed, 0.95 mol of methanol was added per 1 mol of n-butyl lithium to deactivate the reaction catalyst, thereby obtaining a block copolymer.
[0670] Next, the above-mentioned hydrogenation catalyst was added to the obtained block copolymer in an amount of 100 ppm in terms of titanium per 100 parts by mass of the block copolymer, and a hydrogenation reaction was carried out under the conditions of a hydrogen pressure of 0.8 MPa and a temperature of 85° C. After the hydrogenation reaction was completed, 0.3 parts by mass of octadecyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate as a stabilizer was added per 100 parts by mass of the polymer to obtain a hydrogenated block copolymer (22).
[0671] The obtained hydrogenated block copolymer (22) had a total styrene content of 66.2% by mass, a styrene content in the polystyrene block A of 99.1% by mass, a styrene content in the polystyrene block A' of 58.2% by mass, a weight average molecular weight of 95,000 for the entire polymer, and a molecular weight distribution of 1.22. In addition, the hydrogenation rate of the aliphatic double bonds derived from 1,3-butadiene was 99.0%.
[0672] (Hydrogenated block copolymer (23))
[0673] The above hydrogenated block copolymer (8) is desolventized and dried, and pelletized using a single-screw extruder. Then, 2.1 parts by mass of maleic anhydride and 0.12 parts by mass of 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane are added to 100 parts by mass of the hydrogenated block copolymer (8), and an addition reaction is carried out at a set temperature of 200° C. using a twin-screw extruder to obtain a hydrogenated block copolymer (23).
[0674] In the obtained hydrogenated block copolymer (23), the amount of added acid anhydride groups based on maleic anhydride was 1.8% by mass.
[0675] (Hydrogenated block copolymer (24))
[0676] The above hydrogenated block copolymer (18) is desolventized and dried, and pelletized using a single-screw extruder. Then, 2.1 parts by mass of maleic anhydride and 0.12 parts by mass of 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane are added to 100 parts by mass of the hydrogenated block copolymer (18), and an addition reaction is carried out using a twin-screw extruder at a set temperature of 200° C. to obtain a hydrogenated block copolymer (24).
[0677] In the obtained hydrogenated block copolymer (24), the amount of added acid anhydride groups based on maleic anhydride was 1.5% by mass.
[0678] (Hydrogenated block copolymer (25))
[0679] The above hydrogenated block copolymer (22) is desolventized and dried, and pelletized using a single-screw extruder. Then, 2.1 parts by mass of maleic anhydride and 0.12 parts by mass of 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane are added to 100 parts by mass of the hydrogenated block copolymer (22), and an addition reaction is carried out using a twin-screw extruder at a set temperature of 200° C. to obtain a hydrogenated block copolymer (25).
[0680] In the obtained hydrogenated block copolymer (25), the amount of added acid anhydride groups based on maleic anhydride was 1.1% by mass.
[0681] (Hydrogenated block copolymer (26))
[0682] A tank-type reactor with an internal volume of 100 L and equipped with a stirring device and a jacket was cleaned, dried, and replaced with nitrogen to carry out batch polymerization.
[0683] First, a cyclohexane solution containing 11 parts by mass of styrene monomer was added, and then 0.10 parts by mass of n-butyl lithium relative to 100 parts by mass of all monomers, 0.8 mol of TMEDA relative to 1 mol of n-butyl lithium, and 0.04 mol of sodium tert-amyl alcohol relative to 1 mol of n-butyl lithium were added, and polymerization was carried out at 70° C. for 25 minutes.
[0684] Then, a cyclohexane solution containing 10 parts by mass of 1,3-butadiene monomer was added and polymerized at 70°C for 15 minutes, and a cyclohexane solution containing 46 parts by mass of styrene monomer and 19 parts by mass of 1,3-butadiene monomer was further added and polymerized at 70°C for 1 hour.
[0685] Next, a cyclohexane solution containing 9 parts by mass of styrene monomer was added, and polymerization was carried out at 70° C. for 25 minutes.
[0686] Finally, a cyclohexane solution containing 5 parts by mass of 1,3-butadiene monomer was added and polymerized at 70° C. for 15 minutes. After the polymerization reaction was completed, 0.95 mol of methanol was added per 1 mol of n-butyl lithium to deactivate the reaction catalyst, thereby obtaining a block copolymer.
[0687] Next, the above-mentioned hydrogenation catalyst was added to the obtained block copolymer in an amount of 100 ppm in terms of titanium per 100 parts by mass of the block copolymer, and a hydrogenation reaction was carried out under the conditions of a hydrogen pressure of 0.8 MPa and a temperature of 85° C. After the hydrogenation reaction was completed, 0.3 parts by mass of octadecyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate as a stabilizer was added per 100 parts by mass of the polymer to obtain a hydrogenated block copolymer (26).
[0688] The obtained hydrogenated block copolymer (26) had a total styrene content of 66.4% by mass, a styrene content in the polystyrene block A of 99.4% by mass, a styrene content in the polystyrene block A' of 69.2% by mass, a vinyl bond content in the polybutadiene block before hydrogenation of 65.8% by mole, a weight average molecular weight of the entire polymer of 136,000, and a molecular weight distribution of 1.19. In addition, the hydrogenation rate of the aliphatic double bonds derived from 1,3-butadiene was 99.3%.
[0689] (Hydrogenated block copolymer (27))
[0690] A tank-type reactor with an internal volume of 100 L and equipped with a stirring device and a jacket was cleaned, dried, and replaced with nitrogen to carry out batch polymerization.
[0691] First, a cyclohexane solution containing 5 parts by mass of 1,3-butadiene monomer was added, and then 0.215 parts by mass of n-butyl lithium relative to 100 parts by mass of all monomers, 1.6 mol of TMEDA relative to 1 mol of n-butyl lithium, and 0.04 mol of sodium tert-amyl alcohol relative to 1 mol of n-butyl lithium were added, and polymerization was carried out at 60° C. for 20 minutes.
[0692] Next, a cyclohexane solution containing 19 parts by mass of a styrene monomer was added, and polymerization was carried out at 70° C. for 25 minutes. Further, a cyclohexane solution containing 57 parts by mass of a 1,3-butadiene monomer was added, and polymerization was carried out at 60° C. for 1 hour.
[0693] Finally, a cyclohexane solution containing 19 parts by mass of styrene monomer was added and polymerized for 25 minutes at 70° C. After the polymerization reaction was completed, 0.95 mol of methanol was added per 1 mol of n-butyl lithium to deactivate the reaction catalyst, thereby obtaining a block copolymer.
[0694] Next, the above-mentioned hydrogenation catalyst was added to the obtained block copolymer in an amount of 100 ppm in terms of titanium per 100 parts by mass of the block copolymer, and a hydrogenation reaction was carried out under the conditions of a hydrogen pressure of 0.8 MPa and a temperature of 85° C. After the hydrogenation reaction was completed, 0.3 parts by mass of octadecyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate as a stabilizer was added per 100 parts by mass of the polymer to obtain a hydrogenated block copolymer (27).
[0695] The obtained hydrogenated block copolymer (27) had a total styrene content of 37.6% by mass, a styrene content in the polystyrene block A of 99.1% by mass, a vinyl bond content in the polybutadiene block before hydrogenation of 77.5% by mole, a weight average molecular weight of the entire polymer of 54,000, and a molecular weight distribution of 1.16. In addition, the hydrogenation rate of the aliphatic double bonds derived from 1,3-butadiene was 99.5%.
[0696] (Hydrogenated block copolymer (28))
[0697] A tank-type reactor with an internal volume of 100 L and equipped with a stirring device and a jacket was cleaned, dried, and replaced with nitrogen to carry out batch polymerization.
[0698] First, a cyclohexane solution containing 5 parts by mass of 1,3-butadiene monomer was charged, and then 0.078 parts by mass of n-butyl lithium per 100 parts by mass of all monomers and 0.4 mol of TMEDA per 1 mol of n-butyl lithium were added, followed by polymerization at 70° C. for 15 minutes.
[0699] Next, a cyclohexane solution containing 34 parts by mass of styrene monomer was added, and polymerization was carried out at 70° C. for 30 minutes.
[0700] Next, a cyclohexane solution containing 28 parts by mass of 1,3-butadiene monomer was added, and polymerization was carried out at 70° C. for 30 minutes. Finally, a cyclohexane solution containing 33 parts by mass of styrene monomer was added, and polymerization was carried out at 70° C. for 30 minutes.
[0701] After the polymerization reaction was completed, 0.95 mol of methanol was added to 1 mol of n-butyl lithium to deactivate the reaction catalyst, thereby obtaining a block copolymer.
[0702] Next, the above-mentioned hydrogenation catalyst was added to the obtained block copolymer in an amount of 100 ppm in terms of titanium per 100 parts by mass of the block copolymer, and a hydrogenation reaction was carried out under the conditions of a hydrogen pressure of 0.8 MPa and a temperature of 85° C. After the hydrogenation reaction was completed, 0.3 parts by mass of octadecyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate as a stabilizer was added per 100 parts by mass of the polymer to obtain a hydrogenated block copolymer (28).
[0703] The obtained hydrogenated block copolymer (28) had a total styrene content of 66.7% by mass, a polystyrene block content of 99.3% by mass, a vinyl bond content in the polybutadiene block before hydrogenation of 40.3% by mole, a weight average molecular weight of the entire polymer of 195,000, and a molecular weight distribution of 1.14. In addition, the hydrogenation rate of the aliphatic double bonds derived from 1,3-butadiene was 99.2%.
[0704] (Hydrogenated block copolymer (29))
[0705] A tank-type reactor with an internal volume of 100 L and equipped with a stirring device and a jacket was cleaned, dried, and replaced with nitrogen to carry out batch polymerization.
[0706] First, a cyclohexane solution containing 5 parts by mass of 1,3-butadiene monomer was charged, and then 0.125 parts by mass of n-butyl lithium per 100 parts by mass of all monomers and 0.4 mol of TMEDA per 1 mol of n-butyl lithium were added, followed by polymerization at 70° C. for 15 minutes.
[0707] Next, a cyclohexane solution containing 15 parts by mass of a styrene monomer was added, and polymerization was carried out at 70° C. for 25 minutes. Furthermore, a cyclohexane solution containing 65 parts by mass of a 1,3-butadiene monomer was added, and polymerization was carried out at 70° C. for 40 minutes.
[0708] Finally, a cyclohexane solution containing 15 parts by mass of styrene monomer was added and polymerized for 25 minutes at 70° C. After the polymerization reaction was completed, 0.95 mol of methanol was added per 1 mol of n-butyl lithium to deactivate the reaction catalyst, thereby obtaining a block copolymer.
[0709] Next, the above-mentioned hydrogenation catalyst was added to the obtained block copolymer in an amount of 100 ppm in terms of titanium per 100 parts by mass of the block copolymer, and a hydrogenation reaction was carried out under the conditions of a hydrogen pressure of 0.8 MPa and a temperature of 85° C. After the hydrogenation reaction was completed, 0.3 parts by mass of octadecyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate as a stabilizer was added per 100 parts by mass of the polymer to obtain a hydrogenated block copolymer (29).
[0710] The obtained hydrogenated block copolymer (29) had a total styrene content of 30.3% by mass, a styrene content in the polystyrene block A of 99.5% by mass, a vinyl bond content in the polybutadiene block before hydrogenation of 41.2 mol%, a weight average molecular weight of the entire polymer of 103,000, and a molecular weight distribution of 1.16. In addition, the hydrogenation rate of the aliphatic double bonds derived from 1,3-butadiene was 99.5%.
[0711] (Polypropylene resin (b))
[0712] As the polypropylene-based resin (b), the following commercially available products were used.
[0713] Polypropylene resin (b): PM801A manufactured by SunAllomer Co., Ltd., propylene homopolymer nonamer, MFR (230°C, 2.16 kg) 13 g / 10 min
[0714] (Non-aromatic softener (c))
[0715] As the non-aromatic softener (c), the following commercially available products were used.
[0716] Non-aromatic softener (c): Diana process oil PW90 manufactured by Idemitsu Kosan Co., Ltd., paraffin oil, weight average molecular weight 530, kinematic viscosity (40° C.) = 90.5 mm 2 / Second
[0717] [Components used in the multilayer molded article]
[0718] (Thermoplastic resin containing polar groups)
[0719] PC molded board: PC1600 from CITAKIRON Co., Ltd., 95mm×145mm×2mm thick flat board
[0720] ABS molded plate: SUMITOMO BAKELITE Co., Ltd. EAR003, 95mm × 145mm × thickness 2mm flat plate
[0721] PC / ABS molded board: SUMITOMO BAKELITE Co., Ltd. ROA EFN800-04, 95mm×145mm×thickness 2mm flat plate
[0722] PMMA molding plate: Mitsubishi Chemical Corporation Acrylite L-100, 95 mm × 145 mm × 2 mm thick flat plate
[0723] PET molding plate: PET-6010 produced by CITAKIRON Co., Ltd., 95 mm × 145 mm × 2 mm thick flat plate
[0724] Tables 1 to 3 below show the types, formulations, and physical properties of the hydrogenated block copolymers (1) to (29).
[0725] In the table, A and A' are polymer blocks mainly composed of vinyl aromatic monomer units, B is a polymer block mainly composed of conjugated diene monomer units, and X is a residue of a coupling agent.
[0726]
[0727]
[0728]
[0729] The following Tables 4 to 7 show the compounding ratios and properties of the thermoplastic elastomer compositions of Examples 1 to 25 and Comparative Examples 1 to 15.
[0730] In addition, in the following tables, the numbers and description order of Examples and Comparative Examples may not necessarily be the same.
[0731]
[0732]
[0733]
[0734]
[0735] This application is based on the Japanese patent application (Japanese Patent Application No. 2022-081255) filed with the Japan Patent Office on May 18, 2022, and its contents are incorporated into this specification as a reference.
[0736] Industrial Applicability
[0737] The thermoplastic elastomer composition and the multilayer molded article of the present invention have no problems such as odor and color tone and are excellent in moldability and thermal bonding strength, and therefore have industrial applicability as a skin material of a polar resin or various sealing materials.
Claims
1. A thermoplastic elastomer composition for multilayer molding, which is a thermoplastic elastomer composition for multilayer molding that is heat-welded by injection molding, comprising: 100 parts by mass of a hydrogenated block copolymer (a-1); 10 to 100 parts by mass of a polypropylene-based resin (b); and 50 to 300 parts by mass of a non-aromatic softener (c), further comprising a hydrogenated block copolymer (a-2), wherein the hydrogenated block copolymer (a-1) and the hydrogenated block copolymer (a-2) are both unmodified hydrogenated block copolymers, in, The content of the hydrogenated block copolymer (a-2) is 5 to 70% by mass relative to the total amount of the components (a-1), (a-2), (b), and (c). The hydrogenated block copolymer (a-1) satisfies the following conditions (1-1) to (1-4), The hydrogenated block copolymer (a-2) satisfies the following conditions (2-1) to (2-6), (1-1): Contains one or more polymer blocks A1 mainly composed of vinyl aromatic monomer units, and one or more polymer blocks B1 mainly composed of conjugated diene monomer units; (1-2): The content of all vinyl aromatic monomer units is 15% by mass or more and less than 35% by mass; (1-3): weight average molecular weight of 150,000 to 550,000; (1-4): More than 50 mol% of the double bonds of the conjugated diene monomer units are hydrogenated; (2-1): Containing one or more polymer blocks A2 mainly composed of vinyl aromatic monomer units, and one or more polymer blocks B2 mainly composed of conjugated diene monomer units; (2-2): The content of the vinyl aromatic monomer unit in the polymer block A2 is 50% by mass or more; (2-3): The content of all vinyl aromatic monomer units is 35% to 70% by mass; (2-4): The weight average molecular weight is 30,000 or more and less than 150,000; (2-5): The amount of vinyl bonds in the conjugated diene monomer units in the polymer block B2 before hydrogenation is 60 mol% to 95 mol%; (2-6): 50 mol% or more of the double bonds of the conjugated diene monomer units are hydrogenated.
2. The thermoplastic elastomer composition for multilayer molding according to claim 1, in, The hydrogenated block copolymer (a-2): It has at least two polymer blocks A2 mainly composed of vinyl aromatic monomer units, and at least two polymer blocks B2 mainly composed of conjugated diene monomer units, At least one of the polymer blocks B2 is located at the end of the hydrogenated block copolymer (a-2), and the content of the polymer block B2 located at the end is 1% to 10% by mass in the hydrogenated block copolymer (a-2). There is no peak having a weight average molecular weight of 250,000 or more.
3. The thermoplastic elastomer composition for multilayer molding according to claim 2, in, The content of the vinyl aromatic monomer unit in the polymer block A2 of the hydrogenated block copolymer (a-2) is 90% by mass or more.
4. The thermoplastic elastomer composition for multilayer molding according to claim 2 or 3, in, The content of all vinyl aromatic monomer units in the hydrogenated block copolymer (a-2) is greater than 40% by mass and less than 70% by mass.
5. The thermoplastic elastomer composition for multilayer molding according to claim 2 or 3, in, In the hydrogenated block copolymer (a-1), the amount of vinyl bonds in the conjugated diene monomer units before hydrogenation is 30 mol% to 50 mol%.
6. A multilayer molded body comprising: A layer of the thermoplastic elastomer composition for multi-layer molding according to claim 1 or 2; and A thermoplastic resin layer containing polar groups.
7. A multilayer molded body comprising: a thermoplastic resin layer containing polar groups; and A thermoplastic elastomer composition layer comprising a hydrogenated block copolymer (a), a polypropylene resin (b) and a non-aromatic softener (c), in, The thermoplastic elastomer composition layer is provided in contact with the polar group-containing thermoplastic resin layer. The hydrogenated block copolymer (a) does not contain a modifying group, The hydrogenated block copolymer (a): A hydrogenated block copolymer which is a hydrogenated product of a block copolymer having a vinyl aromatic monomer unit and a conjugated diene monomer unit, The molecular weight peaks based on GPC are 30,000 to less than 150,000 and 150,000 to 550,000, respectively, and there are at least one peak. The hydrogenated block copolymer having a molecular weight peak of 30,000 to less than 150,000 based on GPC has a total vinyl aromatic monomer unit content of 35% to 70% by mass, and a vinyl bond content before hydrogenation in the conjugated diene monomer unit of 60% to 95% by mole. The hydrogenated block copolymer having a molecular weight peak of 150,000 to 550,000 based on GPC has a content of all vinyl aromatic monomer units of 15% to less than 35% by mass. The hydrogenation rate of double bonds in the conjugated diene monomer units is 50 mol% or more.
8. The multilayer molded body according to claim 7, in, The hydrogenated block copolymer (a) is composed of a hydrogenated block copolymer (a-1) and a hydrogenated block copolymer (a-2), The above (a-1) satisfies the following conditions (1-1) to (1-4), The above (a-2) satisfies the following conditions (2-1) to (2-6), The thermoplastic elastomer composition layer contains 100 parts by mass of the (a-1), 10 to 100 parts by mass of the (b), and 50 to 300 parts by mass of the (c), The content of the (a-2) in the thermoplastic elastomer composition layer is 5 to 70% by mass relative to the total amount of the components (a-1), (a-2), (b), and (c). (1-1): Contains one or more polymer blocks A1 mainly composed of vinyl aromatic monomer units, and one or more polymer blocks B1 mainly composed of conjugated diene monomer units; (1-2): The content of all vinyl aromatic monomer units is 15% by mass or more and less than 35% by mass; (1-3): weight average molecular weight of 150,000 to 550,000; (1-4): More than 50 mol% of the double bonds of the conjugated diene monomer units are hydrogenated; (2-1): Containing one or more polymer blocks A2 mainly composed of vinyl aromatic monomer units, and one or more polymer blocks B2 mainly composed of conjugated diene monomer units; (2-2): The content of the vinyl aromatic monomer unit in the polymer block A2 is 50% by mass or more; (2-3): The content of all vinyl aromatic monomer units is 35% to 70% by mass; (2-4): The weight average molecular weight is 30,000 or more and less than 150,000; (2-5): The amount of vinyl bonds in the conjugated diene monomer units in the polymer block B2 before hydrogenation is 60 mol% to 95 mol%; (2-6): 50 mol% or more of the double bonds of the conjugated diene monomer units are hydrogenated.
9. The multilayer molded body according to claim 8, in, The hydrogenated block copolymer (a-2): It has at least two polymer blocks A2 mainly composed of vinyl aromatic monomer units, and at least two polymer blocks B2 mainly composed of conjugated diene monomer units, at least one of the polymer blocks B2 is located at the end of the hydrogenated block copolymer (a-2), and the content of the polymer block B2 located at the end is 1% to 10% by mass in the hydrogenated block copolymer (a-2). The content of all vinyl aromatic monomer units is greater than 40% by mass and less than 70% by mass, There is no peak having a weight average molecular weight of 250,000 or more.
10. The multilayer molded body according to claim 8 or 9, in, The content of the vinyl aromatic monomer unit in the polymer block A2 of the hydrogenated block copolymer (a-2) is 90% by mass or more.
11. The multilayer molded body according to claim 7, in, The polar group-containing thermoplastic resin is at least one selected from the group consisting of polycarbonate resin, ABS resin, polyester resin, acrylic resin, and a mixture thereof.
12. The multilayer molded body according to claim 8, in, In the hydrogenated block copolymer (a-1), the amount of vinyl bonds in the conjugated diene monomer units before hydrogenation is 30 mol% to 50 mol%.
13. A thermoplastic elastomer composition used in the multilayer molded product according to claim 8 or 9, in, In the multilayer molded body, the polar group-containing thermoplastic resin layer and the thermoplastic elastomer composition layer are heat-fused by injection molding.
14. A method for producing a multilayer molded body, which is the method for producing a multilayer molded body according to claim 8 or 9, comprising the following steps: A step of molding the thermoplastic resin containing polar groups to obtain a molded body; and A step of injecting the thermoplastic elastomer composition according to claim 13 into a gap between the mold and the molded body with the molded body placed in the mold to perform heat fusion bonding.
Citation Information
Patent Citations
Olefinic polymerisation using silylether initiators
GB2241239A
Thermoplastic elastomer composition
JP2009209273A
Method for manufacturing a bonded body
JP2014168940A
Functionalized amine initiators for anionic polymerization
US5527753A
Functionalized chain extended initiators for anionic polymerization
US5708092A