Thin-wall weak-rigidity structure circumferential weld deformation control and correction method

Through the methods of positioning welding, segmented welding and post-annealing modification welding, combined with three-dimensional scanning technology to adjust welding parameters, the problem of welding deformation control of thin-walled and rigid structures of aerospace products is solved, high-precision contour control is achieved, and welding quality is improved .

CN119016916APending Publication Date: 2024-11-26BEIJING HANGXING MACHINERY MFG CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411184399.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The prior art is difficult to effectively control and correct the welding deformation of the thin-walled and rigid structure of the aerospace product cabin shell, which makes it difficult to ensure the accuracy of the post-welding profile, low adaptability and reliability, and limits production efficiency and product quality.

Method used

Using positioning welding, segmented welding, and post-annealing modification welding, the shape, position and dimension status of the workpiece to be welded is obtained through three-dimensional scanning, and welding parameters are adjusted to realize segmented welding and modification welding, so as to monitor and correct welding deformation in real time to ensure high Precision shape control.

Benefits of technology

It realizes high-precision profile control of thin-walled weak rigid welded structures. The contour accuracy of welding workpieces is less than 0.3mm. It is suitable for titanium alloys, aluminum alloys, stainless steel and other materials, improving welding quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119016916A_ABST
    Figure CN119016916A_ABST
Patent Text Reader

Abstract

The invention provides a thin-wall weak-rigidity structure circumferential weld deformation control and correction method. The method comprises the steps that positioned welding is conducted on an assembled workpiece to be welded; the shape and position size state of the to-be-welded workpiece is obtained; the number of welding segments of the to-be-welded workpiece is determined, welding parameters of a first segment are determined by combining the shape, position and size states of the to-be-welded workpiece, after welding is completed, the shape, position and size states of the to-be-welded workpiece are repeatedly obtained, welding parameters of a next segment are determined, and segment welding is implemented; after segmented welding is completed, a heat treatment tool is used for fastening the workpiece, and stress relief annealing is carried out; and three-dimensional scanning is conducted on the workpiece obtained after stress relief annealing, the shape and position size state of the workpiece is obtained, and if the deformation amount of the maximum deformation position exceeds a set threshold value, modification welding is conducted on the workpiece. Through reasonable process design, welding parameters are continuously adjusted for deformation correction according to the shape and position size state of a workpiece to be welded in the segmented welding and modification welding processes, and high-precision shape and position control over the thin-wall weak-rigidity welding structure is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of weld deformation control and correction, and in particular relates to a method for controlling and correcting the deformation of a thin-wall weak-rigidity structure ring weld. Background Art

[0002] The welding and assembly of thin-walled weak rigidity structural sections is a common technical problem in aerospace products. In the cabin shell structure of aerospace products, thin-walled weak rigidity generally refers to a hollow cylinder with a thickness of no more than 6 mm and an aspect ratio greater than 0.5. During the welding preparation process of thin-walled weak rigidity structures, the products are easily deformed during and after welding due to the influence of welding thermal deformation and the low rigidity of the structure itself.

[0003] In the existing technical solutions, the following methods are usually used to control and correct welding deformation: (1) Rigid fixation of tooling. The product is clamped by process equipment with fastening and positioning functions that fit the product shape, and the welding deformation is limited under the action of external force. This method is less effective under large welding heat input, and will cause the generation of welding residual stress, resulting in a decrease in the mechanical properties of the product; (2) Post-weld heat treatment correction. After welding, the product is heat treated, and deformation external force is applied by process equipment, and the product is corrected by softening at high temperature. This method has extremely high requirements on the structure and materials of heat treatment correction tooling, is costly, and the correction effect is not ideal; (3) Welding simulation and pre-deformation. Welding deformation is predicted by welding simulation, and anti-deformation allowance is added in the deformation zone to ensure the contour accuracy after welding. This method has extremely high requirements on simulation accuracy, and the current level is difficult to guarantee the high requirements of post-weld contour accuracy.

[0004] The above method may be able to meet the welding deformation control needs of some products with simple structures and high rigidity, but there is a certain gap in ensuring the post-welding contour accuracy of the thin-walled, weakly rigid structure of the cabin shell of aerospace products. Summary of the invention

[0005] In the structure of aerospace vehicles, there are often thin-walled weak rigid cabin sections with a wall thickness of no more than 6mm and an aspect ratio greater than 0.5. In order to meet the lightweight requirements of the overall design, the components are spliced ​​into a whole through welding. Due to the thermal deformation during the welding process, the structural accuracy is difficult to ensure, and subsequent supplementary processing is often required, which restricts production efficiency and product quality. The existing methods for controlling welding deformation have low adaptability and reliability, and it is difficult to meet the technical requirements of aerospace products.

[0006] In order to overcome the deficiencies in the prior art, the inventors have conducted intensive research and provided a method for controlling and correcting the deformation of a thin-walled weakly rigid structure ring weld. The welding process is designed to include positioning welding, segmented welding, and post-annealing finishing welding. Through reasonable process design and continuous adjustment of welding parameters during segmented welding and finishing welding according to the shape, position and size status of the workpiece to be welded to correct the deformation, high-precision shape and position control of the thin-walled weakly rigid welded structure can be achieved.

[0007] The technical solution provided by the present invention is as follows:

[0008] A method for controlling and correcting deformation of a thin-walled weak rigid structure circumferential weld, comprising:

[0009] Perform positioning welding on the workpiece to be welded after assembly;

[0010] Perform three-dimensional scanning on the workpiece to be welded after positioning welding to obtain the shape, position and size of the workpiece to be welded, including the maximum deformation position and maximum deformation amount;

[0011] Determine the number of welding sections of the workpiece to be welded, determine the welding parameters of the first section in combination with the shape, position, and size of the workpiece to be welded, and after welding is completed, repeatedly obtain the shape, position, and size of the workpiece to be welded and determine the welding parameters of the next section to implement section welding;

[0012] After the segment welding is completed, the workpiece is tightened using heat treatment tooling and stress relief annealing is performed.

[0013] Further, when tack welding is performed on the workpiece to be welded after assembly, the weld length and interval size of the tack welding are confirmed according to the size of the workpiece to be welded, specifically: when the diameter of the workpiece to be welded is 50-200mm, the tack welding length is 10-15mm, and the tack welding interval is 20-30mm; when the diameter of the workpiece to be welded is 200-400mm, the tack welding length is 10-20mm, and the tack welding interval is 20-30mm; when the diameter of the workpiece to be welded is 400-800mm, the tack welding length is 15-25mm, and the tack welding interval is 15-25mm; when the diameter of the workpiece to be welded is 800-1000mm, the tack welding length is 20-30mm, and the tack welding interval is 15-25mm.

[0014] Furthermore, when performing three-dimensional scanning on the workpiece to be welded after positioning welding, support blocks are placed below the workpiece to be welded at intervals of 25-45 mm.

[0015] Further, the determining the number of welding sections of the workpiece to be welded includes determining the number of welding sections of the workpiece to be welded according to the diameter of the workpiece to be welded, specifically: when the diameter of the workpiece to be welded is 50-200 mm, the number of welding sections is 2; when the diameter of the workpiece to be welded is 200-400 mm, the number of welding sections is 2; when the diameter of the workpiece to be welded is 400-600, the number of welding sections is 3; when the diameter of the workpiece to be welded is 600-1000, the number of welding sections is 4.

[0016] Further, the welding parameters of the first segment are determined in combination with the shape, position and size of the workpiece to be welded, and after welding is completed, the shape, position and size of the workpiece to be welded are repeatedly obtained and the welding parameters of the next segment are determined to implement segment welding, including:

[0017] Taking the maximum deformation position as the reference point, determine the center point of the correction weld within the range of 135°-180° between the circumferential direction of the weld of the workpiece to be welded and the correction parameters in the segmented welding process are determined according to the following formula:

[0018] U 1 I 1 ·L 1 ·cos(180-θ) / v 1 =K 1 Δx 1 ·U 0 I 0 ·L 0 / v 0

[0019] Among them, U 1 is the accelerating voltage of the profile segment welding, I 1 For the electron beam current of the segmented welding, v 1 L is the welding speed of the segmented welding, 1 is the length of the segmented weld, U 0 is the accelerating voltage of segmented welding under zero deformation of the workpiece to be welded, I 0 K is the electron beam current of the segmented welding under zero deformation of the workpiece to be welded. 1 is the correction coefficient, the value is between 1.95 and 2.05, v 0 L is the welding speed of segmented welding under zero deformation of the workpiece to be welded, 0 is the length of the segmented weld under zero deformation of the workpiece to be welded, Δx 1 is the deformation amount at the maximum deformation position formed after the previous welding, and θ is the interval angle between the circumferential direction of the weld seam of the workpiece to be welded and the reference point.

[0020] Furthermore, the profile segment welding acceleration voltage U 1 is the accelerating voltage U for segmented welding under zero deformation of the workpiece to be welded 0 60% to 140%;

[0021] Electron beam welding for shape correction I 1 Electron beam flow I for segmented welding with zero deformation of the workpiece to be welded 0 60% to 140%.

[0022] Furthermore, the ring weld deformation control and correction method also includes: performing a three-dimensional scan on the workpiece after stress relief annealing to obtain the shape, position and size status of the workpiece, and if the deformation at the maximum deformation position exceeds a set threshold, performing a touch-up weld on the workpiece.

[0023] Further, the modification welding of the workpiece includes: taking the maximum deformation position as a reference point, determining a position 180° apart from the reference point in the circumferential direction of the workpiece weld as the center point of the final correction weld, and determining the correction welding parameters of the modification welding according to the following formula:

[0024] U 2 I 2 / v 2 =K 2 ·Δx 2 / Lδ

[0025] Among them, U 2 is the final correction acceleration voltage, I 2 is the final shaped electron beam current, v 2 is the final shaping welding speed, L is the distance from the maximum deformation position to the weld center, δ is the base material thickness, Δx 2 is the deformation at the maximum deformation position, K 2 is the correction coefficient, and its value is between (0.95~1.05)×10 4 between.

[0026] Furthermore, the final correction acceleration voltage U 2 is the accelerating voltage U for segmented welding under zero deformation of the workpiece to be welded 0 60% to 140%;

[0027] Final calibration electron beam current I 2 Electron beam flow I for segmented welding with zero deformation of the workpiece to be welded 0 60% to 140%;

[0028] Final shaping welding speed v 2 The welding speed v is the segment welding speed under zero deformation of the workpiece to be welded. 0 60% to 140%.

[0029] Further, the modification welding of the workpiece includes: when the diameter of the workpiece to be welded is 50-200mm, the length of the modification welding seam is 20-40mm; when the diameter of the workpiece to be welded is 200-400mm, the length of the modification welding seam is 40-60mm; when the diameter of the workpiece to be welded is 400-800mm, the length of the modification welding seam is 50-80mm; when the diameter of the workpiece to be welded is 800-1000mm, the length of the modification welding seam is 80-100mm.

[0030] Furthermore, the workpiece to be welded is a hollow cylinder with a wall thickness not greater than 6 mm and an aspect ratio greater than 0.5.

[0031] A method for controlling and correcting deformation of a thin-walled weak rigid structure ring weld provided by the present invention has the following beneficial effects:

[0032] The present invention provides a method for controlling and correcting the deformation of a thin-walled weak rigid structure ring weld. The method performs a three-dimensional scan on the workpiece to be welded after positioning welding, obtains the shape and position dimensional state of the workpiece to be welded, and can accurately identify the shape and position dimensional accuracy of the workpiece to be welded. The contour is monitored in real time during the segmented welding process, and the position where the welding deformation occurs is corrected by an effective high-energy beam heat source anti-deformation method; after the segmented welding is completed, the real deformation is obtained by stabilization treatment, and the final shape and position dimensional correction is performed, which can ensure that the contour accuracy of the welded workpiece is less than 0.3mm, and is particularly suitable for thin-walled weak rigid welding structures such as titanium alloys, aluminum alloys, stainless steel, carbon steel and high-temperature alloys. The solution provided by the present invention is efficient and concise, and can achieve extremely high-precision contour control, effectively improving the welding quality. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 A schematic diagram of a structure in which a support block is placed under a workpiece to be welded;

[0034] Figure 2 This is a schematic diagram of segment welding deformation correction;

[0035] Figure 3 This is a schematic diagram of modification welding deformation correction. DETAILED DESCRIPTION

[0036] The following detailed description of the present invention will make the features and advantages of the present invention more clear and explicit.

[0037] The word “exemplary” is used exclusively herein to mean “serving as an example, example, or illustration.” Any embodiment described herein as “exemplary” is not necessarily to be construed as preferred or advantageous over other embodiments.

[0038] The present invention provides a method for controlling and correcting deformation of a thin-walled weak rigid structure ring weld, comprising the following steps:

[0039] The first step is tack welding. After assembling the workpiece to be welded using the tooling, confirm the weld length and interval size of the tack welding according to the size of the workpiece to be welded. The specific values ​​are shown in Table 1 below.

[0040] Table 1 Positioning welding weld length and interval size table

[0041] Diameter of workpiece to be welded (mm) Position welding length (mm) Position welding interval (mm) 50-200 10-15 20-30 200-400 10-20 20-30 400-800 15-25 15-25 800-1000 20-30 15-25

[0042] The second step is to confirm the shape and position dimensions. Use a tracking 3D laser scanner to analyze the shape and position dimensions of the workpiece to be welded and obtain the shape and position dimensional status of the workpiece to be welded. For thin-walled weak rigid structures, in order to prevent the middle section from being deformed due to the influence of its own weight, when confirming the shape and position dimensions, it is necessary to place support blocks every 25-45mm below the workpiece to be welded, see Figure 1 ; Then the obtained scanning results are compared with the theoretical model to obtain the contour accuracy of the workpiece to be welded.

[0043] The third step is segmented welding. Determine the segmented welding plan according to the diameter of the workpiece to be welded. The number of segments refers to the recommended value shown in Table 2. Use the following method to adjust the welding parameters of each weld to correct the deformation of the workpiece to be welded: Figure 2 As shown, taking the maximum deformation position as the reference point, the center point of the correction weld is determined within the range of 135°-180° between the circumferential direction of the weld of the workpiece to be welded and the reference point, and the welding correction parameters in the segmented welding process are determined according to the following formula:

[0044] U 1 I 1 ·L 1 ·cos(180-θ) / v 1 =K 1 Δx 1 ·U 0 I 0 ·L 0 / v 0

[0045] Among them, U 1 is the accelerating voltage of the profile segment welding, I 1 For the electron beam current of the segmented welding, v 1 L is the welding speed of the segmented welding, 1 is the length of the segmented weld, U 0 is the accelerating voltage of segmented welding under zero deformation of the workpiece to be welded, I 0 K is the electron beam current of the segmented welding under zero deformation of the workpiece to be welded. 1 is the correction factor, the value is between 1.95 and 2.05, such as 2.0, v 0 L is the welding speed of segmented welding under zero deformation of the workpiece to be welded, 0is the length of the segmented weld under zero deformation of the workpiece to be welded, Δx 1 is the deformation amount at the maximum deformation position formed after the previous welding, and θ is the interval angle between the circumferential direction of the weld seam of the workpiece to be welded and the reference point.

[0046] Preferably, the profile segment welding acceleration voltage U 1 is the accelerating voltage U for segmented welding under zero deformation of the workpiece to be welded 0 60% to 140%.

[0047] Electron beam welding for shape correction I 1 Electron beam flow I for segmented welding with zero deformation of the workpiece to be welded 0 60% to 140%.

[0048] Table 2 Segment welding segment quantity table

[0049] Diameter of workpiece to be welded (mm) Number of welding sections 50-200 2 200-400 2 400-600 3 600-1000 4

[0050] Use the welding position and parameters determined by the above method to weld a segmented weld. After welding is completed, repeat the above "shape and position dimension confirmation - welding adjustment" steps until all segmented welding is completed.

[0051] The fourth step is stabilization treatment (stress relief annealing). After completing the welding of all welds, use heat treatment tools to tighten the workpiece and perform stress relief annealing.

[0052] Step 5: Final shape adjustment (modification welding). Refer to step 2 to confirm the shape, position and size of the workpiece after stabilization. After obtaining the deformation situation, refer to the following method to adjust the deformation during welding: Figure 3 As shown, the maximum deformation position is taken as the reference point, and the position 180° away from the reference point in the circumferential direction of the workpiece weld is determined as the center point of the final correction weld, and the welding correction parameters after the overall welding are determined according to the following empirical formula:

[0053] U 2 I 2 / v 2 =K 2 ·Δx 2 / Lδ

[0054] Among them, U 2 is the final correction acceleration voltage, I 2 is the final shaped electron beam current, v 2 is the final shaping welding speed, L is the distance from the maximum deformation position to the weld center, δ is the base material thickness, Δx 2 is the deformation at the maximum deformation position, K 2 is the correction coefficient, and its value is between (0.95~1.05)×10 4 Between, such as 104 .

[0055] Use the welding position and parameters determined by the above method to perform a correction welding. The weld length can refer to Table 3 below to ensure that the final shape and position accuracy of the workpiece is controlled within ±0.3mm.

[0056] Table 3 Reference table of weld length

[0057] Diameter of workpiece to be welded (mm) Correction weld length (mm) 50-200 20-40 200-400 40-60 400-800 50-80 800-1000 80-100

[0058] Example 1

[0059] In this embodiment, the workpiece to be welded is composed of a front barrel section (length 1000 mm, outer diameter 450 mm) + a rear barrel section (length 400 mm, outer diameter 450 mm), the material grade is GH4169 high temperature alloy, and the weld thickness is 5 mm. The initial welding parameters of the workpiece to be welded under zero deformation are: acceleration voltage 120 kV, electron beam current 55 mA, X / Y axis scanning width 0.5 / 0.5 mm, scanning waveform is circular, focusing current is surface focus + (0.01-0.03) A, and welding speed 1000 mm / min.

[0060] (1) Use the tooling to assemble the workpiece to be welded. According to the size of the workpiece, confirm that the weld length of the tack welding is 20 mm, the interval size is 20 mm, and the tack welding parameters are: acceleration voltage 120 kV, X / Y axis scanning width is 0.5 / 0.5 mm, scanning waveform is circular, focusing current is surface focus + (0.01-0.03) A, welding speed is 1000 mm / min, and the tack welding current is 60% of the initial welding current under zero deformation, so the tack welding current is 33 mA.

[0061] (2) Confirm the shape and size. Use a tracking 3D laser scanner to analyze the shape and size of the workpiece after positioning welding. To prevent deformation caused by its own weight, support blocks are placed under the workpiece at intervals of 30 mm according to the size of the workpiece. The scan results are compared with the theoretical model to obtain the contour accuracy of the workpiece at this time. The deformation at the maximum deformation position is +1.2 mm (where the horizontal line on which the workpiece is placed during scanning is used as the reference, the direction above the horizontal line is positive, and the direction below the horizontal line is negative).

[0062] (3) Perform segmented welding. According to the diameter of the workpiece to be welded, the number of welding segments is determined to be 3, and the length of the segmented weld under zero deformation of the workpiece to be welded is 500 mm. When welding the first segment, the position of 180° at the maximum deformation is selected as the center of the first weld, and the welding correction parameters during the segmented welding process are determined according to the deformation size and initial welding parameters: acceleration voltage 120 kV, electron beam current 66 mA, X / Y axis scanning width 0.5 / 0.5 mm, scanning waveform is circular, focusing current is surface focus + (0.01-0.03) A, welding speed 800 mm / min, and weld length is 800 mm. After the first section of segmented welding is completed, the shape and position dimensions are confirmed to obtain the contour accuracy of the workpiece at this time. The deformation at the maximum deformation position is +0.8mm. According to the formula mentioned above, while ensuring the continuity of the weld, the welding correction parameters of the second section are determined as follows: the position of 135° at the maximum deformation is selected as the center of the second weld, the acceleration voltage is 120kV, the electron beam current is 66mA, the X / Y axis scanning width is 0.5 / 0.5mm, the scanning waveform is circular, the focusing current is surface focus + (0.01-0.03)A, the welding speed is 750mm / min, and the weld length is 714mm. After the second section of segment welding is completed, the shape and position dimensions are confirmed to obtain the contour accuracy of the workpiece at this time. The deformation at the maximum deformation position is +0.5mm. Therefore, the welding correction parameters of the third section are determined as follows: the position of 160° at the maximum deformation is selected as the center of the third weld, the acceleration voltage is 120kV, the electron beam current is 55mA, the X / Y axis scanning width is 0.5 / 0.5mm, the scanning waveform is circular, the focusing current is surface focus + (0.01-0.03)A, the welding speed is 1000mm / min, and the weld length is 538mm.

[0063] (4) After completing the welding of all the segmented welds, use the heat treatment tooling to tighten the workpiece and perform stress relief annealing.

[0064] (5) Use a tracking 3D laser scanner to analyze the shape and position dimensions of the stabilized workpiece to obtain the contour accuracy of the workpiece at this time. The deformation at the maximum deformation position is +0.5mm. Therefore, the final welding correction parameters are determined as follows: the position of 180° at the maximum deformation is selected as the center of the correction weld, the distance from the maximum deformation position to the weld center is 400mm, the final correction acceleration voltage is 120kV, the final correction electron beam current is 21mA, the X / Y axis scanning width is 0.5 / 0.5mm, the scanning waveform is circular, the focusing current is surface focus +(0.01-0.03)A, the final correction welding speed is 1000mm / min, and the weld length is 60mm. Finally, the contour accuracy is confirmed to be less than 0.3mm through shape and position dimensions.

[0065] Example 2

[0066] In this embodiment, the workpiece to be welded is composed of a front barrel section (length 800 mm, outer diameter 600 mm) + an end frame (length 200 mm, outer diameter 600 mm), the material grade is 5A06 aluminum alloy, and the weld thickness is 3 mm. The initial welding parameters under zero deformation of the workpiece to be welded are: acceleration voltage 100 kV, electron beam current 30 mA, X / Y axis scanning width 0.5 / 0.5 mm, scanning waveform is circular, focusing current is surface focus + (0.01-0.03) A, and welding speed 800 mm / min.

[0067] (1) Use the tooling to assemble the workpiece to be welded. According to the size of the workpiece, confirm that the weld length of the tack welding is 25 mm, the interval size is 15 mm, and the tack welding parameters are: acceleration voltage 100 kV, X / Y axis scanning width is 0.5 / 0.5 mm, scanning waveform is circular, focusing current is surface focus + (0.01-0.03) A, welding speed is 800 mm / min, and the tack welding current is 60% of the initial welding current under zero deformation, so the tack welding current is 18 mA.

[0068] (2) Confirm the shape and size. Use a tracking 3D laser scanner to analyze the shape and size of the workpiece after positioning welding. To prevent deformation caused by its own weight, support blocks are placed at intervals of 40 mm under the workpiece according to the size of the workpiece. The scan results are compared with the theoretical model to obtain the contour accuracy of the workpiece at this time. The deformation at the maximum deformation position is +2 mm.

[0069] (3) Perform segmented welding. According to the diameter of the workpiece to be welded, the number of welding segments is determined to be 4, and the length of the segmented weld under zero deformation of the workpiece to be welded is 550 mm. When welding the first segment, the position of 180° at the maximum deformation is selected as the center of the first weld, and the welding correction parameters during the segmented welding process are determined according to the deformation size and initial welding parameters: acceleration voltage 100 kV, electron beam current 30 mA, X / Y axis scanning width 0.5 / 0.5 mm, scanning waveform is circular, focusing current is surface focus + (0.01-0.03) A, welding speed 400 mm / min, and weld length is 1100 mm. After the first section of segmented welding is completed, the shape and position dimensions are confirmed to obtain the contour accuracy of the workpiece at this time. The deformation at the maximum deformation position is +1mm. According to the formula mentioned above, while ensuring the continuity of the weld, the welding correction parameters of the second section are determined as follows: the position of 135° at the maximum deformation is selected as the center of the second weld, the acceleration voltage is 100kV, the electron beam current is 40mA, the X / Y axis scanning width is 0.5 / 0.5mm, the scanning waveform is circular, the focusing current is surface focus + (0.01-0.03)A, the welding speed is 600mm / min, and the weld length is 904mm. After the second section of segment welding is completed, the shape and position dimensions are confirmed to obtain the contour accuracy of the workpiece at this time. The deformation at the maximum deformation position is +0.5mm. Therefore, the welding correction parameters of the third section are determined as follows: the position of 160° at the maximum deformation is selected as the center of the third weld, the acceleration voltage is 100kV, the electron beam current is 33mA, the X / Y axis scanning width is 0.5 / 0.5mm, the scanning waveform is circular, the focusing current is surface focus + (0.01-0.03)A, the welding speed is 800mm / min, and the weld length is 550mm. After the third section welding is completed, the shape and position dimensions are confirmed to obtain the contour accuracy of the workpiece at this time. The deformation at the maximum deformation position is +0.5mm. Therefore, the welding correction parameters of the fourth section are determined as follows: the position 180° from the maximum deformation is selected as the center of the third weld, the acceleration voltage is 100kV, the electron beam current is 30mA, the X / Y axis scanning width is 0.5 / 0.5mm, the scanning waveform is circular, the focusing current is surface focus + (0.01-0.03)A, the welding speed is 800mm / min, and the weld length is 550mm.

[0070] (4) After completing the welding of all the segmented welds, use the heat treatment tooling to tighten the workpiece and perform stress relief annealing.

[0071] (5) Use a tracking 3D laser scanner to analyze the shape and position of the stabilized workpiece to obtain the contour accuracy of the workpiece at this time. The deformation at the maximum deformation position is +0.5mm. Therefore, the final welding correction parameters are determined as follows: the position of 180° at the maximum deformation is selected as the center of the correction weld, the distance from the maximum deformation position to the weld center is 800mm, the acceleration voltage is 100kV, the electron beam current is 17mA, the X / Y axis scanning width is 0.5 / 0.5mm, the scanning waveform is circular, the focusing current is surface focus + (0.01-0.03)A, the welding speed is 800mm / min, and the weld length is 80mm. Finally, the contour accuracy is confirmed to be less than 0.3mm through shape and position dimensions.

[0072] Example 3

[0073] In this embodiment, the workpiece to be welded is composed of a front barrel section (length 500 mm, outer diameter 200 mm) + an end frame (length 100 mm, outer diameter 200 mm), the material grade is TC4 titanium alloy, and the weld thickness is 1 mm. The initial welding parameters are: acceleration voltage 50 kV, electron beam current 15 mA, X / Y axis scanning width 0.5 / 0.5 mm, scanning waveform is circular, focusing current is surface focus + (0.01-0.03) A, and welding speed 1000 mm / min.

[0074] (1) Use the tooling to assemble the workpiece to be welded. According to the size of the workpiece, confirm that the weld length of the tack welding is 15 mm, the interval size is 20 mm, and the tack welding parameters are: acceleration voltage 50 kV, X / Y axis scanning width is 0.5 / 0.5 mm, scanning waveform is circular, focusing current is surface focus + (0.01-0.03) A, welding speed is 1000 mm / min, and the tack welding current is 60% of the initial welding current under zero deformation, so the tack welding current is 9 mA.

[0075] (2) Confirm the shape and position dimensions. Use a tracking 3D laser scanner to analyze the shape and position dimensions of the workpiece after positioning welding. To prevent deformation caused by its own weight, support blocks are placed at intervals of 45 mm under the workpiece according to the size of the workpiece. The scan results are compared with the theoretical model to obtain the contour accuracy of the workpiece at this time. The deformation at the maximum deformation position is +1 mm.

[0076] (3) Perform segmented welding. According to the diameter of the workpiece to be welded, the number of welding segments is determined to be 2, and the length of the segmented weld under zero deformation of the workpiece to be welded is 350 mm. When welding the first segment, the position of 180° at the maximum deformation is selected as the center of the first weld, and the welding correction parameters during the segmented welding process are determined according to the deformation size and initial welding parameters: acceleration voltage 50 kV, electron beam current 15 mA, X / Y axis scanning width 0.5 / 0.5 mm, scanning waveform is circular, focusing current is surface focus + (0.01-0.03) A, welding speed 600 mm / min, and weld length is 420 mm. After the first section of segmented welding is completed, the shape and position dimensions are confirmed to obtain the contour accuracy of the workpiece at this time. The deformation at the maximum deformation position is +0.8mm. According to the formula mentioned above, the welding correction parameters of the second section are determined as follows: the position 180° from the maximum deformation is selected as the center of the second weld, the acceleration voltage is 50kV, the electron beam current is 16mA, the X / Y axis scanning width is 0.5 / 0.5mm, the scanning waveform is circular, the focusing current is surface focus + (0.01-0.03)A, the welding speed is 800mm / min, and the weld length is 420mm.

[0077] (4) After completing the welding of all the segmented welds, use the heat treatment tooling to tighten the workpiece and perform stress relief annealing.

[0078] (5) Use a tracking 3D laser scanner to analyze the shape and position of the stabilized workpiece to obtain the contour accuracy of the workpiece at this time. The deformation at the maximum deformation position is +0.5mm. Therefore, the final welding correction parameters are determined as follows: the position of 180° at the maximum deformation is selected as the center of the correction weld, the distance from the maximum deformation position to the weld center is 500mm, the acceleration voltage is 100kV, the electron beam current is 10mA, the X / Y axis scanning width is 0.5 / 0.5mm, the scanning waveform is circular, the focusing current is surface focus +(0.01-0.03)A, the welding speed is 100mm / min, and the weld length is 40mm. Finally, the contour accuracy is confirmed to be less than 0.3mm through shape and position dimensions.

[0079] The present invention has been described in detail above in conjunction with specific implementations and exemplary examples, but these descriptions cannot be understood as limiting the present invention. Those skilled in the art understand that, without departing from the spirit and scope of the present invention, a variety of equivalent substitutions, modifications or improvements may be made to the technical solution of the present invention and its implementation methods, all of which fall within the scope of the present invention. The scope of protection of the present invention shall be subject to the attached claims.

[0080] The contents not described in detail in the specification of the present invention belong to the common knowledge of those skilled in the art.

Claims

1. A method for controlling and correcting deformation of a thin-walled weak rigid structure ring weld, characterized in that: include: Perform positioning welding on the workpiece to be welded after assembly; Perform three-dimensional scanning on the workpiece to be welded after positioning welding to obtain the shape, position and size of the workpiece to be welded, including the maximum deformation position and maximum deformation amount; Determine the number of welding sections of the workpiece to be welded, determine the welding parameters of the first section in combination with the shape, position, and size of the workpiece to be welded, and after welding is completed, repeatedly obtain the shape, position, and size of the workpiece to be welded and determine the welding parameters of the next section to implement section welding; After the segment welding is completed, the workpiece is tightened using heat treatment tooling and stress relief annealing is performed.

2. The method for controlling and correcting deformation of a thin-walled weak rigid structure ring weld according to claim 1 is characterized in that: When tack welding is performed on the workpiece to be welded after assembly, the weld length and interval size of the tack welding are confirmed according to the size of the workpiece to be welded. Specifically: when the diameter of the workpiece to be welded is 50-200mm, the tack welding length is 10-15mm, and the tack welding interval is 20-30mm; when the diameter of the workpiece to be welded is 200-400mm, the tack welding length is 10-20mm, and the tack welding interval is 20-30mm; when the diameter of the workpiece to be welded is 400-800mm, the tack welding length is 15-25mm, and the tack welding interval is 15-25mm; when the diameter of the workpiece to be welded is 800-1000mm, the tack welding length is 20-30mm, and the tack welding interval is 15-25mm.

3. The method for controlling and correcting deformation of a thin-walled weak rigid structure ring weld according to claim 1 is characterized in that: When performing a three-dimensional scan of the workpiece to be welded after positioning welding, support blocks are placed under the workpiece to be welded at intervals of 25-45 mm.

4. The method for controlling and correcting deformation of a thin-walled weak rigid structure ring weld according to claim 1, characterized in that: The determining the number of welding sections of the workpiece to be welded includes determining the number of welding sections of the workpiece to be welded according to the diameter of the workpiece to be welded. Specifically: when the diameter of the workpiece to be welded is 50-200 mm, the number of welding sections is 2; when the diameter of the workpiece to be welded is 200-400 mm, the number of welding sections is 2; when the diameter of the workpiece to be welded is 400-600, the number of welding sections is 3; when the diameter of the workpiece to be welded is 600-1000, the number of welding sections is 4.

5. The method for controlling and correcting deformation of a thin-walled weak rigid structure ring weld according to claim 1, characterized in that: The method comprises: determining the welding parameters of the first segment in combination with the shape, position and size of the workpiece to be welded, and after welding is completed, repeatedly obtaining the shape, position and size of the workpiece to be welded and determining the welding parameters of the next segment, and performing segment welding, including: Taking the maximum deformation position as the reference point, determine the center point of the correction weld within the range of 135°-180° between the circumferential direction of the weld of the workpiece to be welded and the correction parameters in the segmented welding process are determined according to the following formula: U1·I1·L1·cos(180-θ) / v1=K1·Δx1·U0·I0·L0 / v0 Among them, U1 is the acceleration voltage of the shaping segmented welding, I1 is the electron beam current of the shaping segmented welding, v1 is the welding speed of the shaping segmented welding, L1 is the length of the shaping segmented welding weld, U0 is the acceleration voltage of the segmented welding under zero deformation of the workpiece to be welded, I0 is the electron beam current of the segmented welding under zero deformation of the workpiece to be welded, K1 is the correction coefficient, the value is between 1.95 and 2.05, v0 is the welding speed of the segmented welding under zero deformation of the workpiece to be welded, L0 is the length of the segmented weld under zero deformation of the workpiece to be welded, Δx1 is the deformation of the maximum deformation position formed after the previous welding, and θ is the interval angle between the circumferential direction of the weld of the workpiece to be welded and the reference point.

6. The method for controlling and correcting deformation of a thin-walled weak rigid structure ring weld according to claim 5, characterized in that: The acceleration voltage U1 of the shape correction segment welding is 60% to 140% of the acceleration voltage U0 of the segment welding under zero deformation of the workpiece to be welded; The electron beam current I1 of the shape correction segment welding is 60% to 140% of the electron beam current I0 of the segment welding under zero deformation of the workpiece to be welded.

7. The method for controlling and correcting deformation of a thin-walled weak rigid structure ring weld according to claim 1, characterized in that: The ring weld deformation control and correction method also includes: performing three-dimensional scanning on the workpiece after stress relief annealing to obtain the shape, position and size status of the workpiece, and if the deformation at the maximum deformation position exceeds a set threshold, performing touch-up welding on the workpiece.

8. The method for controlling and correcting deformation of a thin-walled weak rigid structure ring weld according to claim 7, characterized in that: The modification welding of the workpiece includes: taking the maximum deformation position as a reference point, determining a position 180° apart from the reference point in the circumferential direction of the workpiece weld as the center point of the final correction weld, and determining the correction welding parameters of the modification welding according to the following formula: U2·I2 / v2=K2·Δx2 / Lδ Among them, U2 is the final correction acceleration voltage, I2 is the final correction electron beam current, v2 is the final correction welding speed, L is the distance between the maximum deformation position and the weld center, δ is the parent material thickness, Δx2 is the deformation at the maximum deformation position, and K2 is the correction coefficient, which ranges from (0.95 to 1.05)×10 4 between.

9. The method for controlling and correcting deformation of a thin-walled weak rigid structure ring weld according to claim 7, characterized in that: The modification welding of the workpiece includes: when the diameter of the workpiece to be welded is 50-200mm, the length of the modification welding seam is 20-40mm; when the diameter of the workpiece to be welded is 200-400mm, the length of the modification welding seam is 40-60mm; when the diameter of the workpiece to be welded is 400-800mm, the length of the modification welding seam is 50-80mm; when the diameter of the workpiece to be welded is 800-1000mm, the length of the modification welding seam is 80-100mm.

10. The method for controlling and correcting deformation of a thin-walled weak rigid structure ring weld according to claim 1, characterized in that: The workpiece to be welded is a hollow cylinder with a wall thickness not greater than 6 mm and an aspect ratio greater than 0.5.

Citation Information

Cited By

  • Method for welding lower half part of low-pressure rear cylinder of steam turbine

    CN121402886A

  • Welding method for lower half of low-pressure rear cylinder of steam turbine