Light low-conductivity high-strength polyurethane encapsulating material
By adopting lightweight, low-conducting and high-strength polyurethane materials, the problems of high density, poor fluidity and high curing strength of epoxy adhesives and silicone rubber adhesives are solved, and polyurethane potting materials with low density, high strength and low thermal conductivity are realized, simplifying the The molding process and reduce production costs are suitable for fixing and sealing of internal cables and components of aircraft.
Patent Information
- Application Number
- CN202411071734.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-11-26
AI Technical Summary
As potting materials, existing epoxy adhesives and silicone rubber adhesives have problems such as high density, poor fluidity, high strength after curing, but difficult to reverse operation, which is difficult to meet the fixing needs of the internal cables and components of the aircraft, especially in complex structures. It is difficult to operate in the cabin and makes the product overweight.
Lightweight low-conductivity and high-strength polyurethane potting materials composed of polyether polyols, silicone oil, amine catalysts and foaming agents are used to form adjustable density, moderate hardness and low thermal conductivity through specific molding ratios and additive preparations. The material adopts a foaming process to simplify the processing process.
It realizes polyurethane potting materials with low density, high strength and low thermal conductivity, simplifies the forming process, reduces production costs, and is easy to operate during reverse operation, meeting the fixing and sealing needs of the internal cables and components of the aircraft.
Smart Images

Figure CN119019632A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polyurethane materials, in particular to a light-weight, low-conductivity and high-strength polyurethane potting material. Background Art
[0002] At present, all kinds of telecommunication transmission inside aircraft are realized through the connection of cables and components, but cables and other parts in the equipment structure are difficult to fix after assembly. For cabins with complex internal structures, traditional clamp fixing or adhesive potting treatment is extremely difficult to operate. Using high-density potting materials such as epoxy glue and silicone glue will not only be difficult to implement due to poor fluidity, but also cause the final product to be overweight.
[0003] At present, epoxy adhesives and silicone rubber adhesives are widely used as potting materials for cables and components. For example, the following patents and patent applications:
[0004] An anhydride-curable silicone-modified epoxy resin potting adhesive and a preparation method thereof (CN105268005B);
[0005] An epoxy potting adhesive and its preparation method and application (CN117247757A);
[0006] An epoxy resin blended modified silicone potting adhesive and its preparation method (CN113337244A);
[0007] An epoxy potting adhesive and a preparation method thereof (CN105368005B);
[0008] A high thermal conductivity, low viscosity epoxy potting adhesive and its preparation method (CN117363287A);
[0009] A silicone rubber for potting that cures quickly at room temperature and a preparation method thereof (CN110506078A).
[0010] The main disadvantages of existing epoxy adhesives and silicone rubber adhesives as potting materials are in the following three aspects:
[0011] (1) High density. The density of the adhesive layer is 1g / cm 3 Above, the density of polyurethane potting material is less than 0.5g / cm 3 Meet the requirements for aircraft product weight reduction;
[0012] (2) Poor fluidity. Most cables and components are installed on the inner wall of a specific structure. The poor fluidity of the glue makes the molding process difficult and implementation is difficult.
[0013] (3) Epoxy adhesives and silicone rubber adhesives have high strength after curing, and reverse operation is difficult. In contrast, although rigid polyurethane potting materials have high strength, they are brittle and easy to reverse operation.
[0014] Therefore, choosing a lightweight, low-conductivity, high-strength material for potting cables and components in aircraft is the current key research direction. Summary of the invention
[0015] In order to solve the above technical problems existing in the prior art, the present invention provides a lightweight, low-conductivity, high-strength polyurethane potting material, which is specifically achieved through the following technical solutions.
[0016] A lightweight, low-conductivity, high-strength polyurethane potting material, which consists of a main material component A and a foaming material component B in parts by weight; the molding ratio of the polyurethane potting material is A:B=100:95-115;
[0017] The component A is a polyurethane polyether composite material, which is mixed and prepared by 90-94 parts of polyether polyol, 1-3 parts of silicone oil, 1-2 parts of amine catalyst, and 4-5 parts of foaming agent; the component B is a foaming material, which is mixed and prepared by 90-98 parts of diphenylmethane diisocyanate, 0-4.5 parts of pentane foaming agent, 0-2 parts of foam stabilizer, 1-2 parts of amine catalyst, 0.5-1.5 parts of toughening agent and 0.5-1.5 parts of other additives.
[0018] Furthermore, the polyether polyol is a mixture of one or more of polyoxypropylene polyol, grafted polyether polyol, flame retardant polyether polyol and polytetramethylene ether glycol in any proportion.
[0019] Furthermore, the silicone oil refers to methyl silicone oil, modified silicone oil, or a mixture of the two in any proportion.
[0020] Furthermore, the amine catalyst is one or more of dimorpholine diethyl ether, dimethylaminopropylamine, and triethylenediamine mixed in any proportion.
[0021] Furthermore, the toughening agent is one or a mixture of two of maleic anhydride grafted phase solvent and polyvinyl alcohol in any proportion.
[0022] Furthermore, the other additives are additives other than silicone oil, amine catalysts, and toughening agents, such as coupling agents (one or more silane coupling agents mixed in any proportion), mildew inhibitors (one or more ammonium persulfate and calcium phosphate mixed in any proportion).
[0023] Furthermore, the component A is a polyurethane polyether composite material, which is mixed and prepared by 92 parts of polyether polyol, 2 parts of silicone oil, 1.5 parts of amine catalyst, and 4.5 parts of foaming agent; the component B is a foaming material, which is mixed and prepared by 98 parts of diphenylmethane diisocyanate, 1 part of toughening agent, and 1 part of other auxiliary agents. The molding ratio of the polyurethane potting material is A:B=100:100 or A:B=100:110 or A:B=100:105.
[0024] Furthermore, the component A is a polyurethane polyether composite material, which is mixed and prepared by 92 parts of polyether polyol, 2 parts of silicone oil, 1.5 parts of amine catalyst, and 4.5 parts of foaming agent; the component B is a foaming material, which is mixed and prepared by 90 parts of diphenylmethane diisocyanate, 4.5 parts of pentane foaming agent, 2 parts of foam stabilizer, 1.5 parts of amine catalyst, 1 part of toughening agent, and 1 part of other additives. The molding ratio of the polyurethane potting material is A:B=100:105.
[0025] The polyurethane potting material of the present application is injected into a product cavity by a filling machine and solidified and formed when in use.
[0026] Compared with the prior art, the technical effects created by the present invention are embodied in:
[0027] (1) The main molding material for the polyurethane potting material of the present application is polyether polyol, and the main curing cross-linking agent is diphenylmethane diisocyanate. The comprehensive performance of the rigid polyurethane potting material is improved by adding various additives. For example, the thermal insulation performance of the rigid polyurethane material can be improved by adding high-temperature resistant thermal insulation vapor phase silica. The thermal insulation, heat protection and other comprehensive properties of the rigid polyurethane material can be significantly improved by mixing and modifying the polyurethane material. Compared with the prior art, the polyurethane potting material provided by the present invention has the performance advantages of adjustable density, moderate hardness, high strength and low thermal conductivity, as well as the process advantage of easy molding and preparation. The application of polyurethane as a potting material has reasonable and effective indicator parameters.
[0028] (2) Polyurethane has the characteristics of light weight, insulation, low thermal conductivity and high strength. This application innovatively uses polyurethane foam material as a potting material, which has the unique advantages of adjustable density and high impact strength, and meets the performance requirements of product fixed sealing, which will give it a broad application field and huge potential value.
[0029] (3) Compared with the traditional sealant molding process such as epoxy glue, the polyurethane potting material foaming one-step molding process of the present application is simpler. When applied in engineering mass production, it can reduce the processing steps and significantly reduce the production cost.
[0030] (4) The polyurethane of the present application is fragile after foaming. The polyurethane foam material is used as a potting material, which is easy to operate during the reverse operation of repairing components such as cables. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 This is the engineering verification result diagram of polyurethane potting materials. DETAILED DESCRIPTION
[0032] The technical solution of the present invention is further defined below in conjunction with specific implementation methods, but the scope of protection required is not limited to the description.
[0033] Example 1: Typical formula of polyurethane potting material is shown in Table 1.
[0034] Table 1 Typical formula of polyurethane potting materials
[0035]
[0036] Example 2: Preparation of polyurethane potting material samples and verification of molding performance with different ratios
[0037] Sample production method:
[0038] Five groups of samples with the same density were molded according to the same ratio. The density was set to the middle limit (calculated as 0.38 g / cm3). The amount of A and B was calculated according to the density and mold cavity size. Samples were produced according to the amount of 5 ratios (A:B=100:95; A:B=100:100; A:B=100:105; A:B=100:110; A:B=100:115). The specific implementation steps are as follows:
[0039] 1. Mold preparation
[0040] (a) Baking the mold: Place the mold in an oven and bake at 40°C to 50°C for 1 hour;
[0041] (b) Apply mold release agent: Use car wax (or high-grade floor wax) to evenly wipe the mold cavity.
[0042] 2. Ingredients
[0043] (a) Weighing: Weigh the components according to the weight ratio of A:B=100:105;
[0044] (b) Mixing: Pour the weighed component B into component A and stir rapidly for no more than 20 seconds;
[0045] (c) Filling: Quickly inject the stirred mixture into the mold cavity;
[0046] (d) Mold closing: close the mold and lock it quickly.
[0047] 3. Curing: Natural curing at room temperature, the curing time is more than 25 minutes.
[0048] 4. Demolding: The molded sample is slowly ejected by the mold ejector to complete the demoulding process.
[0049] 5. Finishing: Grind off the flash of the potting material specimen and place it at room temperature for more than 24 hours.
[0050] The main tests for the potting materials of cables and electrical components are their density, hardness, thermal conductivity and compressive strength. The performance indicators of different ratios are shown in Table 2.
[0051] Table 2 Performance indicators of various ratios of potting materials
[0052]
[0053] Note: Preparation and test results of specimens with the same formula, same density, but different A and B ratios.
[0054] Example 3: Engineering verification of polyurethane potting materials
[0055] The engineering test of polyurethane potting material is carried out according to the formula of the present invention. The engineering verification simulates the technical status of a certain product for verification. The product is a 20# steel cylinder closed body, with a design size of outer diameter φ83mm (inner diameter φ73), length 200mm, two φ12 threaded holes are opened on the cylinder (one for filling the potting material, the other for molding exhaust), and the cavity volume is 773mm 3 , the cavity simulates the actual product to arrange cables of different thicknesses. After theoretical calculation, the polyurethane A:B ratio is 1:1.05. Among them, 160g of material A and 168g of material B are weighed. After high-speed stirring and mixing, they are immediately injected into the mold cavity with a filler, and then the injection hole and exhaust hole are blocked with screws. After complete curing, the cylinder is cut open by cutting. For details of the polyurethane potting molding material inside the product, see Figure 1 .
[0056] like Figure 1 As shown in the figure, after the polyurethane foaming, the micropores are uniform and dense, without defects such as large bubbles and cracks. The foaming process does not damage the cables in the cavity, and the cables are tightly wrapped after foaming, which plays a good role in fastening and supporting protection. After weighing and calculation, the weight of the foaming material in the cavity is 330g, and the density of the foaming material is 0.382g / cm 3 , meeting the requirements of product design technical indicators. Engineering tests show that the feasibility of the patented polyurethane potting material formula and molding process technology has been verified.
[0057] Finally, it should be pointed out that the above embodiments are only representative examples of the present invention. Obviously, the technical solution of the present invention is not limited to the above embodiments, and there are many variations. All variations that can be directly derived or associated with the content disclosed by ordinary technicians in this field should be considered as the protection scope of the present invention.
Claims
1. A lightweight, low-conductivity, high-strength polyurethane potting material, characterized in that: According to weight parts, it is composed of component A main material and component B foaming material; the molding ratio of the polyurethane potting material is A:B=100:95-115; The component A is a polyurethane polyether composite material, which is mixed and prepared by 90-94 parts of polyether polyol, 1-3 parts of silicone oil, 1-2 parts of amine catalyst, and 4-5 parts of foaming agent; the component B is a foaming material, which is mixed and prepared by 90-98 parts of diphenylmethane diisocyanate, 0-4.5 parts of pentane foaming agent, 0-2 parts of foam stabilizer, 1-2 parts of amine catalyst, 0.5-1.5 parts of toughening agent and 0.5-1.5 parts of other additives.
2. The lightweight, low-conductivity, high-strength polyurethane potting material according to claim 1, characterized in that: The polyether polyol is a mixture of one or more of polyoxypropylene polyol, grafted polyether polyol, flame retardant polyether polyol and polytetramethylene ether glycol in any proportion.
3. The lightweight, low-conductivity, high-strength polyurethane potting material according to claim 1, characterized in that: The other additives are additives other than silicone oil, amine catalysts and toughening agents.
4. The method for preparing the lightweight, low-conductivity, high-strength polyurethane potting material according to claim 1, characterized in that: The component A is a polyurethane polyether composite material, which is mixed and prepared by 92 parts of polyether polyol, 2 parts of silicone oil, 1.5 parts of amine catalyst, and 4.5 parts of foaming agent; the component B is a foaming material, which is mixed and prepared by 98 parts of diphenylmethane diisocyanate, 1 part of toughening agent, and 1 part of other auxiliary agents.
5. The lightweight, low-conductivity, high-strength polyurethane potting material according to claim 4, characterized in that: The molding ratio of the polyurethane potting material is A:B=100:
100.
6. The lightweight, low-conductivity, high-strength polyurethane potting material according to claim 4, characterized in that: The molding ratio of the polyurethane potting material is A:B=100:
110.
7. The lightweight, low-conductivity, high-strength polyurethane potting material according to claim 4, characterized in that: The molding ratio of the polyurethane potting material is A:B=100:
105.
8. The method for preparing a lightweight, low-conductivity, high-strength polyurethane potting material according to claim 1, characterized in that: The component A is a polyurethane polyether composite material, which is mixed and prepared by 92 parts of polyether polyol, 2 parts of silicone oil, 1.5 parts of amine catalyst, and 4.5 parts of foaming agent; the component B is a foaming material, which is mixed and prepared by 90 parts of diphenylmethane diisocyanate, 4.5 parts of pentane foaming agent, 2 parts of foam stabilizer, 1.5 parts of amine catalyst, 1 part of toughening agent, and 1 part of other additives.
9. The lightweight, low-conductivity, high-strength polyurethane potting material according to claim 8, characterized in that: The molding ratio of the polyurethane potting material is A:B=100:105.