Brazed low-heat-conductivity high-pressure cast aluminum alloy and preparation method thereof

By adding specific proportions of elements to the aluminum alloy and refining and degassing, a low-thermal conductivity and high-pressure cast aluminum alloy is formed, which solves the problem of difficulty in welding of aluminum alloys and the inconsistent welding temperature, and achieves high solid-liquid phase temperature and good welding performance .

CN119020640APending Publication Date: 2024-11-26CHONGQING DAJIANG MILLISON DIE CASTING
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411151351.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing aluminum alloy brazing technology has problems such as high thermal conductivity, low melting point and easy oxidation film, which makes welding difficult, and the conventional brazing temperature is higher than the eutectic temperature of aluminum alloy, making it difficult to meet the welding needs of castings.

Method used

Develop a low-thermal conductivity and high-pressure cast aluminum alloy containing specific proportions of manganese, nickel, iron, titanium, vanadium, molybdenum and other elements. The solid-liquid phase temperature is increased through refining and degassing treatment, and the high-pressure casting process is used to form good fluidity and Aluminum alloy with thermal crack resistance, suitable for brazing processes.

Benefits of technology

The high solid-liquid phase temperature of aluminum alloy is achieved, the feasibility of the welding process is ensured, the casting performance and welding quality are improved, the tensile strength and elongation are achieved, and the thermal conductivity is reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119020640A_ABST
    Figure CN119020640A_ABST
Patent Text Reader

Abstract

The invention discloses a braze-weldable low-thermal-conductivity high-pressure cast aluminum alloy and a preparation method thereof, and the aluminum alloy comprises the following components by weight percent: 0.6-16% of manganese; up to 0.12% by weight of silicon; 1.8 to 6.5 wt% of nickel; 0.2 to 1.3 wt% of iron; 0.02 to 0.1 wt% of chromium; 0.1 to 0.15 wt% of titanium; 0.15 to 0.35 wt% of vanadium; a maximum of 0.03% by weight of boron; up to 0.12% by weight of magnesium; up to 0.02% by weight of copper; 0.15% to 0.45% by weight of calcium; up to 0.02% by weight of zinc; a single impurity element is 0.05 wt% at most, and the sum of the impurity elements is less than 0.15 wt%, with the balance being aluminum. The aluminum alloy has high solid-liquid phase temperature, and the solidus is larger than or equal to 625 DEG C. The high-strength aluminum alloy has the advantages that the high-strength aluminum alloy is low in cost and good in castability, fluidity and hot crack resistance are equivalent to those of a conventional cast A356 alloy, the as-cast yield strength is larger than 100 MPa, and meanwhile the high-strength aluminum alloy has the elongation at break A of 8.0% or above and the tensile strength larger than 230 MPa.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of high-pressure casting materials, and in particular to a brazable low-thermal-conductivity high-pressure casting aluminum alloy and a preparation method thereof. Background Art

[0002] High-pressure casting of liquid metal (die casting for short) refers to a near-net-shape forming technology that fills the mold cavity with liquid or semi-liquid metal at a high speed under the action of the punch movement and solidifies under pressure. During the die casting process, the pressure on the molten metal is generally 30 to 80 MPa, the gate speed during filling reaches 25-50 m / s, and the filling time is only 0.02-0.1 s. It can form parts with complex structures, and has high production efficiency and low manufacturing cost. It is currently the most widely used process in metal liquid forming methods.

[0003] Aluminum alloys are widely used in aviation, automobile manufacturing, rail transportation, electronic equipment and other fields due to their good physical and chemical properties. However, the welding of aluminum and its alloys is relatively difficult, due to reasons such as aluminum's high thermal conductivity, low melting point, easy formation of oxide film, and sensitivity to pollution. Aluminum alloy brazing technology is a welding process used to connect aluminum and its alloys. As an effective connection method, it can achieve the connection of aluminum alloys at a lower temperature, thereby avoiding or reducing problems that may occur during the welding process. However, the current cast aluminum alloys are mainly aluminum-silicon systems, and the eutectic temperature is 577 degrees, which is significantly lower than the conventional brazing temperature. Therefore, it is necessary to develop a new casting alloy system to meet the requirements of casting brazing.

[0004] Invention patent application CN113897519A discloses an aluminum-manganese-magnesium-silicon-titanium-tin casting alloy for brazing by vacuum die casting and a preparation method thereof. On the basis of the aluminum-manganese eutectic composition, magnesium and silicon are added to improve the toughness of the alloy, and titanium and tin are added to refine the grains and improve the toughness of the alloy; however, the addition of 0.2 to 0.6 wt.% of silicon will significantly increase the solidification range, aggravate the tendency of hot cracking, and affect the casting performance; invention patent application CN116377288A discloses a high-pressure cast aluminum alloy that can be used for brazing, and the high-pressure cast aluminum alloy that can be used for brazing includes: a maximum of 0.3 wt.% of silicon, 0.6 to 1.5 % manganese by weight, 0.3-1.0% magnesium by weight, and 5.0-12.0% rare earth by weight; wherein the rare earth: 3*Mn weight% ratio is controlled between 2.0 and 3.8; the patented cast aluminum alloy requires the use of a large amount of rare earth, which is costly; invention patent CN115679159B discloses an aluminum-nickel-manganese alloy material for high-temperature brazing and a rheological die-casting method thereof, which improves the casting performance by adding 3-3.5wt.% nickel and 1.0-1.2wt.% manganese, and uses rheological die-casting to alleviate shrinkage and thermal cracking, but the rheological process is difficult to control in actual operation, and defective products are prone to occur, and excessive nickel addition will significantly increase the cost. Summary of the invention

[0005] In view of the deficiencies in the above-mentioned prior art, the present invention provides a brazable low thermal conductivity high pressure cast aluminum alloy, which has a relatively high solid-liquid phase temperature, a solidus line greater than or equal to 625°C, and is suitable for welding processes.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions:

[0007] A brazable low thermal conductivity high pressure cast aluminum alloy, characterized in that: the brazable low thermal conductivity high pressure cast aluminum alloy contains the following components in percentage by mass:

[0008] 0.6-16% by weight of manganese;

[0009] up to 0.12 wt. % silicon;

[0010] 1.8 to 6.5 wt % nickel;

[0011] 0.2-1.3 wt.% iron;

[0012] 0.02-0.1 wt. % chromium;

[0013] 0.1-0.15 wt.% titanium;

[0014] 0.15-0.35 wt. % vanadium;

[0015] Up to 0.03% by weight of boron;

[0016] up to 0.12% by weight of magnesium;

[0017] up to 0.02% by weight of copper;

[0018] 0.15-0.45% by weight of calcium;

[0019] Maximum 0.02% by weight of zinc; maximum 0.05% by weight of individual impurity elements, the sum of impurity elements less than 0.15% by weight, and the remainder is aluminum.

[0020] Furthermore, the total amount of copper+magnesium+silicon is not higher than 0.25 wt %.

[0021] Furthermore, the total amount of manganese + nickel + iron + calcium is not less than 2.6 weight % and not more than 5.8 weight %.

[0022] Further, the brazable low thermal conductivity high pressure cast aluminum alloy contains the following components in percentage by mass:

[0023] 0.6% by weight of manganese;

[0024] up to 0.12 wt. % silicon;

[0025] 1.8 wt% nickel;

[0026] 0.2 wt% iron;

[0027] 0.02% by weight of chromium;

[0028] 0.1 wt.% titanium;

[0029] 0.15 wt.% vanadium;

[0030] Up to 0.03% by weight of boron;

[0031] up to 0.12% by weight of magnesium;

[0032] up to 0.02% by weight of copper;

[0033] 0.15% by weight calcium;

[0034] Maximum 0.02% by weight of zinc; maximum 0.05% by weight of individual impurity elements, the sum of impurity elements less than 0.15% by weight, and the remainder is aluminum.

[0035] Further, the brazable low thermal conductivity high pressure cast aluminum alloy contains the following components in percentage by mass:

[0036] 1.6% by weight of manganese;

[0037] up to 0.12 wt. % silicon;

[0038] 6.5 wt. % nickel;

[0039] 1.3 wt.% iron;

[0040] 0.1 wt.% chromium;

[0041] 0.15 wt.% titanium;

[0042] 0.35 wt.% vanadium;

[0043] Up to 0.03% by weight of boron;

[0044] up to 0.12% by weight of magnesium;

[0045] up to 0.02% by weight of copper;

[0046] 0.45% by weight calcium;

[0047] Maximum 0.02% by weight of zinc; maximum 0.05% by weight of individual impurity elements, the sum of impurity elements less than 0.15% by weight, and the remainder is aluminum.

[0048] It is also intended to provide a method for preparing a brazable low thermal conductivity high pressure cast aluminum alloy, characterized in that it comprises the following steps:

[0049] S1, melting aluminum ingots and controlling the temperature of the aluminum liquid to be 690-745° C.; adjusting the composition of the aluminum liquid to 0.6-1.6 weight % manganese;

[0050] up to 0.12 wt. % silicon;

[0051] 1.8 to 6.5 wt % nickel;

[0052] 0.2-1.3 wt.% iron;

[0053] 0.02-0.1 wt. % chromium;

[0054] 0.1-0.15 wt.% titanium;

[0055] 0.15-0.35 wt. % vanadium;

[0056] Up to 0.03% by weight of boron;

[0057] up to 0.12% by weight of magnesium;

[0058] up to 0.02% by weight of copper;

[0059] 0.15-0.45% by weight of calcium;

[0060] Maximum 0.02% by weight of zinc; maximum 0.05% by weight of individual impurity elements, less than 0.15% by weight of the total impurity elements, and the remainder is aluminum;

[0061] S2. Pressing the aluminum alloy sodium-free refining agent into the degasser for refining and degassing, and setting the refining time to 10-20 minutes to remove hydrogen and inclusions in the aluminum liquid;

[0062] S3, degassing the aluminum alloy by a degasser, and setting a predetermined refining time of 8-15 minutes to remove hydrogen and inclusions in the aluminum liquid;

[0063] S4, the gas content is detected by a hydrogen detector, and when the gas content reaches below 0.15ml / 100g, it is die-casted by a pressure casting device.

[0064] The beneficial effects of the present invention include: the aluminum alloy has a relatively high solid-liquid phase temperature, and the solidus is greater than or equal to 625°C. It also has good castability, fluidity and thermal cracking resistance comparable to conventional cast A356 alloy, a cast yield strength greater than 100 MPa, and a fracture elongation A of more than 8.0%, and a tensile strength greater than 230 MPa. BRIEF DESCRIPTION OF THE DRAWINGS

[0065] Figure 1 It is the metallographic organization diagram of the present invention. DETAILED DESCRIPTION

[0066] The present invention will be further described in detail below with reference to specific embodiments and accompanying drawings.

[0067] Example 1

[0068] Step 1: Add industrial pure aluminum ingots into a crucible resistance furnace and heat to 710-740 degrees Celsius until the pure aluminum ingot is completely melted, and then adjust the aluminum liquid composition. The aluminum alloy liquid includes:

[0069] 0.6 wt% manganese; 0.12 wt% silicon; 1.8 wt% nickel; 0.2 wt% iron; 0.02 wt% chromium; 0.1 wt% titanium; 0.15 wt% vanadium; 0.03 wt% boron; 0.12 wt% magnesium; 0.02 wt% copper; 0.15 wt% calcium; 0.02 wt% zinc; individual impurity elements up to 0.05 wt%, the total impurity elements less than 0.15 wt%, the rest is aluminum.

[0070] Step 2: Press the aluminum alloy sodium-free refining agent into the degasser for refining, and degas for 10 to 20 minutes to remove the gas in the aluminum liquid;

[0071] Step 3: Check whether the composition of the effective aluminum alloy liquid meets the use standard. If so, proceed to step 4. If not, it means that a certain original mass percentage in the aluminum alloy liquid does not reach the above-mentioned preset mass percentage, and an additional mass percentage of elements needs to be added to adjust the mass percentage of the element in the effective aluminum alloy liquid so that the mass percentage of the element meets the use standard, that is, reaches the mass percentage preset in step 1.

[0072] Step 4: Detect the gas content by a hydrogen meter, and when the gas content reaches below 0.15ml / 100g, die-cast it by high-pressure die-casting equipment. If the gas content does not meet the standard, continue with the refining and degassing in step 2.

[0073] Die casting production verification:

[0074] Production equipment and auxiliary accessories: The die-casting machine is equipped with an automatic ladle feeder and a mold temperature controller, a vacuum machine with ultra-low vacuum, a sealing system for the mold structure, a special mold release agent and punch lubrication system for die-casting structural parts, and a 4mm thick test piece mold;

[0075] The process parameters of pressure casting are as follows: mold cavity vacuum is 20Mbar, casting pressure is 65±5MPa, injection speed is 3.5±0.5m / s, mold temperature is 150±10℃, and aluminum alloy liquid temperature is 710±10℃.

[0076] The die-casting test pieces obtained by the above method were cut according to the GBT228 standard test piece line, and then tested using a universal tensile machine equipped with an extensometer, and the mechanical properties and thermal conductivity were tested. The tensile strength of Example 1 was 251.3 MPa; the yield strength was 103.4 MPa; the elongation was 8.5%; and the thermal conductivity was 107.2 W / m·k.

[0077] Example 2

[0078] Step 1: Add industrial pure aluminum ingots into a crucible resistance furnace and heat to 710-740 degrees Celsius until the pure aluminum ingot is completely melted, and then adjust the aluminum liquid composition. The aluminum alloy liquid includes:

[0079] 0.75 wt% manganese; 0.05 wt% silicon; 1.9 wt% nickel; 0.5 wt% iron; 0.08 wt% chromium; 0.13 wt% titanium; 0.25 wt% vanadium; 0.03 wt% boron; 0.03 wt% magnesium; 0.02 wt% copper; 0.15 wt% calcium; 0.02 wt% zinc; individual impurity elements up to 0.05 wt%, the total impurity elements less than 0.15 wt%, the rest is aluminum.

[0080] Step 2: Press the aluminum alloy sodium-free refining agent into the degasser for refining, and degas for 10 to 20 minutes to remove the gas in the aluminum liquid;

[0081] Step 3: Check whether the composition of the effective aluminum alloy liquid meets the use standard. If so, proceed to step 4. If not, it means that a certain original mass percentage in the aluminum alloy liquid does not reach the above-mentioned preset mass percentage, and an additional mass percentage of elements needs to be added to adjust the mass percentage of the element in the effective aluminum alloy liquid so that the mass percentage of the element meets the use standard, that is, reaches the mass percentage preset in step 1.

[0082] Step 4: Detect the gas content by a hydrogen meter, and when the gas content reaches below 0.15ml / 100g, die-cast it by high-pressure die-casting equipment. If the gas content does not meet the standard, continue with the refining and degassing in step 2.

[0083] Die casting production verification:

[0084] Production equipment and auxiliary accessories: The die-casting machine is equipped with an automatic ladle feeder and a mold temperature controller, a vacuum machine with ultra-low vacuum, a sealing system for the mold structure, a special mold release agent and punch lubrication system for die-casting structural parts, and a 4mm thick test piece mold;

[0085] The process parameters of pressure casting are as follows: mold cavity vacuum is 20Mbar, casting pressure is 65±5MPa, injection speed is 3.5±0.5m / s, mold temperature is 150±10℃, and aluminum alloy liquid temperature is 710±10℃.

[0086] The die-casting test pieces obtained by the above method were cut according to the GBT228 standard test piece wire, and then tested using a universal tensile machine equipped with an extensometer, and the mechanical properties and thermal conductivity were tested. The tensile strength of Example 2 was 242.1 MPa; the yield strength was 105.3 MPa; the elongation was 4.5%; and the thermal conductivity was 105.3 W / m·k.

[0087] Example 3

[0088] Step 1: Add industrial pure aluminum ingots into a crucible resistance furnace and heat to 710-740 degrees Celsius until the pure aluminum ingot is completely melted, and then adjust the aluminum liquid composition. The aluminum alloy liquid includes:

[0089] 0.85 wt% manganese; 0.04 wt% silicon; 3.3 wt% nickel; 0.5 wt% iron; 0.03 wt% chromium; 0.15 wt% titanium; 0.32 wt% vanadium; 0.02 wt% boron; 0.03 wt% magnesium; 0.02 wt% copper; 0.43 wt% calcium; 0.04 wt% zinc; individual impurity elements up to 0.05 wt%, the total of impurity elements less than 0.15 wt%, the rest is aluminum.

[0090] Step 2: Press the aluminum alloy sodium-free refining agent into the degasser for refining, and degas for 10 to 20 minutes to remove the gas in the aluminum liquid;

[0091] Step 3: Check whether the composition of the effective aluminum alloy liquid meets the use standard. If so, proceed to step 4. If not, it means that a certain original mass percentage in the aluminum alloy liquid does not reach the above-mentioned preset mass percentage, and an additional mass percentage of elements needs to be added to adjust the mass percentage of the element in the effective aluminum alloy liquid so that the mass percentage of the element meets the use standard, that is, reaches the mass percentage preset in step 1.

[0092] Step 4: Detect the gas content by a hydrogen meter, and when the gas content reaches below 0.15ml / 100g, die-cast it by high-pressure die-casting equipment. If the gas content does not meet the standard, continue with the refining and degassing in step 2.

[0093] Die casting production verification:

[0094] Production equipment and auxiliary accessories: The die-casting machine is equipped with an automatic ladle feeder and a mold temperature controller, a vacuum machine with ultra-low vacuum, a sealing system for the mold structure, a special mold release agent and punch lubrication system for die-casting structural parts, and a 4mm thick test piece mold;

[0095] The process parameters of pressure casting are as follows: mold cavity vacuum is 20Mbar, casting pressure is 65±5MPa, injection speed is 3.5±0.5m / s, mold temperature is 150±10℃, and aluminum alloy liquid temperature is 710±10℃.

[0096] The die-casting test pieces obtained by the above method were cut according to the GBT228 standard test piece wire, and then tested using a universal tensile machine equipped with an extensometer, and the mechanical properties and thermal conductivity were tested. The tensile strength of Example 3 was 200.5 MPa; the yield strength was 102.8 MPa; the elongation was 12.6%; and the thermal conductivity was 104.7 W / m·k.

[0097] Example 4

[0098] Step 1: Add industrial pure aluminum ingots into a crucible resistance furnace and heat to 710-740 degrees Celsius until the pure aluminum ingot is completely melted, and then adjust the aluminum liquid composition. The aluminum alloy liquid includes:

[0099] 1.46 wt% manganese; 0.06 wt% silicon; 3.1 wt% nickel; 1.2 wt% iron; 0.05 wt% chromium; 0.13 wt% titanium; 0.24 wt% vanadium; 0.03 wt% boron; 0.04 wt% magnesium; 0.02 wt% copper; 0.33 wt% calcium; 0.02 wt% zinc; individual impurity elements up to 0.05 wt%, the total impurity elements less than 0.15 wt%, the rest is aluminum.

[0100] Step 2: Press the aluminum alloy sodium-free refining agent into the degasser for refining, and degas for 10 to 20 minutes to remove the gas in the aluminum liquid;

[0101] Step 3: Check whether the composition of the effective aluminum alloy liquid meets the use standard. If so, proceed to step 4. If not, it means that a certain original mass percentage in the aluminum alloy liquid does not reach the above-mentioned preset mass percentage, and an additional mass percentage of elements needs to be added to adjust the mass percentage of the element in the effective aluminum alloy liquid so that the mass percentage of the element meets the use standard, that is, reaches the mass percentage preset in step 1.

[0102] Step 4: Detect the gas content by a hydrogen meter, and when the gas content reaches below 0.15ml / 100g, die-cast it by high-pressure die-casting equipment. If the gas content does not meet the standard, continue with the refining and degassing in step 2.

[0103] Die casting production verification:

[0104] Production equipment and auxiliary accessories: The die-casting machine is equipped with an automatic ladle feeder and a mold temperature controller, a vacuum machine with ultra-low vacuum, a sealing system for the mold structure, a special mold release agent and punch lubrication system for die-casting structural parts, and a 4mm thick test piece mold;

[0105] The process parameters of pressure casting are as follows: mold cavity vacuum is 20Mbar, casting pressure is 65±5MPa, injection speed is 3.5±0.5m / s, mold temperature is 150±10℃, and aluminum alloy liquid temperature is 710±10℃.

[0106] The die-casting test pieces obtained by the above method were cut according to the GBT228 standard test piece wire, and then tested using a universal tensile machine equipped with an extensometer, and the mechanical properties and thermal conductivity were tested. The tensile strength of Example 4 was 195.8 MPa; the yield strength was 107.4 MPa; the elongation was 11.8%; and the thermal conductivity was 99.4 W / m·k.

[0107] Example 5

[0108] Step 1: Add industrial pure aluminum ingots into a crucible resistance furnace and heat to 710-740 degrees Celsius until the pure aluminum ingot is completely melted, and then adjust the aluminum liquid composition. The aluminum alloy liquid includes:

[0109] 1.6 wt% manganese; 0.12 wt% silicon; 6.5 wt% nickel; 1.3 wt% iron; 0.1 wt% chromium; 0.15 wt% titanium; 0.35 wt% vanadium; 0.03 wt% boron; 0.12 wt% magnesium; 0.02 wt% copper; 0.45 wt% calcium; 0.02 wt% zinc; individual impurity elements up to 0.05 wt%, the total of impurity elements less than 0.15 wt%, the rest is aluminum.

[0110] Step 2: Press the aluminum alloy sodium-free refining agent into the degasser for refining, and degas for 10 to 20 minutes to remove the gas in the aluminum liquid;

[0111] Step 3: Check whether the composition of the effective aluminum alloy liquid meets the use standard. If so, proceed to step 4. If not, it means that a certain original mass percentage in the aluminum alloy liquid does not reach the above-mentioned preset mass percentage, and an additional mass percentage of elements needs to be added to adjust the mass percentage of the element in the effective aluminum alloy liquid so that the mass percentage of the element meets the use standard, that is, reaches the mass percentage preset in step 1.

[0112] Step 4: Detect the gas content by a hydrogen meter, and when the gas content reaches below 0.15ml / 100g, die-cast it by high-pressure die-casting equipment. If the gas content does not meet the standard, continue with the refining and degassing in step 2.

[0113] Die casting production verification:

[0114] Production equipment and auxiliary accessories: The die-casting machine is equipped with an automatic ladle feeder and a mold temperature controller, a vacuum machine with ultra-low vacuum, a sealing system for the mold structure, a special mold release agent and punch lubrication system for die-casting structural parts, and a 4mm thick test piece mold;

[0115] The process parameters of pressure casting are as follows: mold cavity vacuum is 20Mbar, casting pressure is 65±5MPa, injection speed is 3.5±0.5m / s, mold temperature is 150±10℃, and aluminum alloy liquid temperature is 710±10℃.

[0116] The die-casting test pieces obtained by the above method were cut according to the GBT228 standard test piece wire, and then tested using a universal tensile machine equipped with an extensometer, and the mechanical properties and thermal conductivity were tested. The tensile strength of Example 5 was 192.1 MPa; the yield strength was 112.5 MPa; the elongation was 8.9%; and the thermal conductivity was 89.2 W / m·k.

[0117] Example 6

[0118] Step 1: Add industrial pure aluminum ingots into a crucible resistance furnace and heat to 710-740 degrees Celsius until the pure aluminum ingot is completely melted, and then adjust the aluminum liquid composition. The aluminum alloy liquid includes:

[0119] 0.32 wt% manganese; 0.10 wt% silicon; 1.65 wt% nickel; 1.22 wt% iron; 0.03 wt% chromium; 0.05 wt% titanium; 0.07 wt% vanadium; 0.02 wt% boron; 0.08 wt% magnesium; 0.02 wt% copper; 0.02 wt% calcium; 0.03 wt% zinc; individual impurity elements up to 0.05 wt%, the total impurity elements less than 0.15 wt%, the rest is aluminum.

[0120] Step 2: Press the aluminum alloy sodium-free refining agent into the degasser for refining, and degas for 10 to 20 minutes to remove the gas in the aluminum liquid;

[0121] Step 3: Check whether the composition of the effective aluminum alloy liquid meets the use standard. If so, proceed to step 4. If not, it means that a certain original mass percentage in the aluminum alloy liquid does not reach the above-mentioned preset mass percentage, and an additional mass percentage of elements needs to be added to adjust the mass percentage of the element in the effective aluminum alloy liquid so that the mass percentage of the element meets the use standard, that is, reaches the mass percentage preset in step 1.

[0122] Step 4: Detect the gas content by a hydrogen meter, and when the gas content reaches below 0.15ml / 100g, die-cast it by high-pressure die-casting equipment. If the gas content does not meet the standard, continue with the refining and degassing in step 2.

[0123] Die casting production verification:

[0124] Production equipment and auxiliary accessories: The die-casting machine is equipped with an automatic ladle feeder and a mold temperature controller, a vacuum machine with ultra-low vacuum, a sealing system for the mold structure, a special mold release agent and punch lubrication system for die-casting structural parts, and a 4mm thick test piece mold;

[0125] The process parameters of pressure casting are as follows: mold cavity vacuum is 20Mbar, casting pressure is 65±5MPa, injection speed is 3.5±0.5m / s, mold temperature is 150±10℃, and aluminum alloy liquid temperature is 710±10℃.

[0126] The die-casting test pieces obtained by the above method were cut according to the GBT228 standard test piece wire, and then tested using a universal tensile machine equipped with an extensometer, and the mechanical properties and thermal conductivity were tested. The tensile strength of Example 6 was 214.7 MPa; the yield strength was 123.5 MPa; the elongation was 9.7%; and the thermal conductivity was 153.30 W / m·k.

[0127] Example 6 is a comparative example. Compared with Examples 1-5, it can be seen that the thermal conductivity of the comparative example is high. The feasibility of brazing the high-pressure cast aluminum-based composite material was tested by gas shielded brazing process. The results showed that after high-temperature brazing, there was no obvious pore bulging and local melting phenomenon in the casting. Its metallographic structure is as follows: Figure 1 This indicates that the casting material has an extremely low gas content and a high solid-liquid phase temperature, and has no obvious defects during high-temperature brazing. This indicates that the alloy material of the present invention has good weldability.

[0128] The technical solutions provided by the embodiments of the present invention are introduced in detail above. Specific examples are used herein to illustrate the principles and implementation methods of the embodiments of the present invention. The description of the above embodiments is only applicable to help understand the principles of the embodiments of the present invention. At the same time, for those skilled in the art, according to the embodiments of the present invention, there will be changes in the specific implementation methods and application scopes. In summary, the content of this specification should not be understood as limiting the present invention.

Claims

1. A brazable low thermal conductivity high pressure cast aluminum alloy, characterized in that: The brazable low thermal conductivity high pressure cast aluminum alloy contains the following components in percentage by mass: 0.6-16% by weight of manganese; up to 0.12 wt. % silicon; 1.8 to 6.5 wt % nickel; 0.2-1.3 wt.% iron; 0.02-0.1 wt. % chromium; 0.1-0.15 wt.% titanium; 0.15-0.35 wt. % vanadium; Up to 0.03% by weight of boron; up to 0.12% by weight of magnesium; up to 0.02% by weight of copper; 0.15-0.45% by weight of calcium; Maximum 0.02% by weight of zinc; maximum 0.05% by weight of individual impurity elements, the sum of impurity elements less than 0.15% by weight, and the remainder is aluminum.

2. A brazable low thermal conductivity high pressure cast aluminum alloy according to claim 1, characterized in that: The total of copper+magnesium+silicon is not higher than 0.25 wt %.

3. A brazable low thermal conductivity high pressure cast aluminum alloy according to claim 1, characterized in that: The total amount of manganese+nickel+iron+calcium is not less than 2.6% by weight and not more than 5.8% by weight.

4. The brazable low thermal conductivity high pressure cast aluminum alloy according to claim 1, characterized in that: The brazable low thermal conductivity high pressure cast aluminum alloy contains the following components in percentage by mass: 0.6% by weight of manganese; up to 0.12 wt. % silicon; 1.8 wt. % nickel; 0.2 wt% iron; 0.02% by weight of chromium; 0.1 wt.% titanium; 0.15 wt.% vanadium; Up to 0.03% by weight of boron; up to 0.12% by weight of magnesium; up to 0.02% by weight of copper; 0.15% by weight calcium; Maximum 0.02% by weight of zinc; maximum 0.05% by weight of individual impurity elements, the sum of impurity elements less than 0.15% by weight, and the remainder is aluminum.

5. The brazable low thermal conductivity high pressure cast aluminum alloy according to claim 1, characterized in that: The brazable low thermal conductivity high pressure cast aluminum alloy contains the following components in percentage by mass: 1.6% by weight of manganese; up to 0.12 wt. % silicon; 6.5 wt. % nickel; 1.3 wt.% iron; 0.1 wt.% chromium; 0.15 wt.% titanium; 0.35 wt.% vanadium; Up to 0.03% by weight of boron; up to 0.12% by weight of magnesium; up to 0.02% by weight of copper; 0.45% by weight calcium; Maximum 0.02% by weight of zinc; maximum 0.05% by weight of individual impurity elements, the sum of impurity elements less than 0.15% by weight, and the remainder is aluminum.

6. A method for preparing a brazable low thermal conductivity high pressure cast aluminum alloy, characterized in that: The following steps are included: S1, melting aluminum ingots and controlling the temperature of the aluminum liquid to be 690-745° C.; adjusting the composition of the aluminum liquid to 0.6-1.6 weight % manganese; up to 0.12 wt. % silicon; 1.8 to 6.5 wt % nickel; 0.2-1.3 wt.% iron; 0.02-0.1 wt. % chromium; 0.1-0.15 wt.% titanium; 0.15-0.35 wt. % vanadium; Up to 0.03% by weight of boron; up to 0.12% by weight of magnesium; up to 0.02% by weight of copper; 0.15-0.45% by weight of calcium; Maximum 0.02% by weight of zinc; maximum 0.05% by weight of individual impurity elements, less than 0.15% by weight of the total impurity elements, and the remainder is aluminum; S2. Pressing the aluminum alloy sodium-free refining agent into the degasser for refining and degassing, and setting the refining time to 10-20 minutes to remove hydrogen and inclusions in the aluminum liquid; S3, degassing the aluminum alloy by a degasser, and setting a predetermined refining time of 8-15 minutes to remove hydrogen and inclusions in the aluminum liquid; S4, the gas content is detected by a hydrogen detector, and when the gas content reaches below 0.15ml / 100g, it is die-casted by a pressure casting device.

Citation Information

Cited By

  • Aluminum alloy for extrusion casting and preparation method and application thereof

    CN121109820A

  • High solidus die-casting aluminum alloy capable of being brazed and preparation method of high solidus die-casting aluminum alloy

    CN121137416A