Boron-doped diamond and method for treating water pollution

Boron-doped diamond electrode prepared by microwave plasma chemical vapor deposition method solves the problems of metal-based catalyst pollution and complex operation in electrochemical water treatment, and achieves efficient removal of nitrate ions and organic matter in water, and avoids secondary Pollution shows good structural stability and corrosion resistance.

CN119020760AInactive Publication Date: 2024-11-26TIANJIN UNIV

Patent Information

Application Number
CN202411138820.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-26
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

When existing electrochemical water treatment technology treats high concentrations of pollutants, metal-based catalysts are prone to cross-contamination and secondary pollution due to changes in environmental conditions, and are complex in operation, making it difficult to efficiently and stably degrade nitrates and organic matters.

Method used

Boron-doped diamond electrodes were prepared by microwave plasma chemical vapor deposition method to form an efficient dual-electrode system. Boron-doped diamond films were grown on titanium sheets by microwave plasma chemical vapor deposition method, as cathode and anode, using their p The semiconductors have the characteristics of degrading nitrate ions and organic matter in water, reducing competition between hydrogen evolution and oxygen evolution reactions.

Benefits of technology

It realizes efficient removal of nitrate ions and organic matter in water, is easy to operate, avoids secondary contamination of reagents, and boron-doped diamond electrode has good structural stability and corrosion resistance, which is suitable for long-term use.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119020760A_ABST
    Figure CN119020760A_ABST
Patent Text Reader

Abstract

The invention discloses boron-doped diamond and a method for treating water pollution, and belongs to the technical field of water treatment. After matrix metal is ground and polished, the boron-doped diamond film is grown on the surface of the matrix metal by a microwave plasma chemical vapor deposition method. The boron-doped diamond electrode forms a dual-electrode system, an electrolyte is a Na2SO4 solution containing NO3 <-> and phenol, and the current density is set to be 10-20 mA cm <-2 >. By means of the method, NO3 <-> ions and organic matter in water can be removed at the same time, in addition, secondary oxidation of a cathode product on an anode can be accelerated by improving the current density, the selectivity of N2 is improved, and the method is easy and convenient to operate, clean, free of pollution and high in removal rate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of water treatment, and in particular relates to boron-doped diamond and a method for treating water pollution. Background Art

[0002] At present, the strategies for treating nitrate and organic pollution can be divided into two categories: biological methods and physicochemical methods. However, these methods usually have some disadvantages, such as slow remediation speed, secondary contamination of reagents, and complex operation, which limits their application in practice. Among the physicochemical methods, electrochemical processes have received more attention in treating wastewater with high concentrations of pollutants due to their advantages such as versatility, safety, high energy efficiency, and environmental friendliness. Nitrate and phenol are the most common and prevalent inorganic and organic pollutants. Nitrate and phenol can be degraded simultaneously at the cathode and anode of the same electrolysis system without the need for multiple degradation steps or the use of other non-electrochemical treatment methods, which greatly saves treatment time and cost. Traditional metal-based catalysts have been developed in electrochemical wastewater degradation systems. However, under harsh electrochemical water treatment conditions (such as pH changes, high potentials, and long-term use), these materials usually involve the leaching of metal ions, resulting in serious cross-contamination between the two electrodes and secondary pollution of the environment. Therefore, it is necessary to develop efficient and stable bifunctional electrocatalysts for nitrate reduction and organic oxidation. Summary of the invention

[0003] Boron-doped diamond electrodes with high purity and good crystallinity can be prepared by microwave plasma chemical vapor deposition, which can simultaneously degrade nitrates and organic matter while reducing the competition between hydrogen evolution reaction (HER) and oxygen evolution reaction (OER). Boron-doped diamond (BDD) electrodes have p-type semiconductor properties due to boron doping, so they have high conductivity, stable structure, corrosion resistance and high potential for combining with reactant molecules.

[0004] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a method for degrading nitrate ions and organic matter (phenol) in water by using boron-doped diamond. The method is simple to operate, has no pollution to the environment and has good effect.

[0005] In order to solve the above technical problems, the present invention relates to a method for degrading nitrate ions and organic matter (phenol) in water by using boron-doped diamond, comprising the following steps:

[0006] Step 1: Grind the titanium sheet with 400#, 600#, 800#, 1000# and 2000# sandpaper until the surface is bright, polish the surface with W0.5 diamond powder, perform ultrasonic treatment on the polished titanium sheet for 2 minutes to remove residual diamond powder on the surface, and then blow dry with nitrogen.

[0007] Step 2: Place the titanium sheet obtained in step 1 into a microwave plasma chemical vapor deposition system (MPCVD) chamber and introduce 300 sccm of H 2 , 6 sccm CH 4 and 8 sccm of H through trimethyl borate solution 2 The microwave power was set to 1900W, the pressure was controlled to 50Torr, and the growth time was 10h. After the growth was completed, the microwave power and pressure were reduced to 400W and 6Torr, all gases were turned off, and the sample was cooled to room temperature and then taken out to obtain a boron-doped diamond film grown on a titanium substrate.

[0008] Step 3: The non-diamond surface of the boron-doped diamond grown on the titanium substrate obtained in step 2 is sealed with silicone. Two pieces of boron-doped diamond prepared by the same process are used as the cathode and the anode to form a double-electrode system. The electrolyte contains 1000 mg L -1 NO 3 - and 100mgL -1 Na of organic matter (phenol) 2 SO 4 Solution, current density set to 10-20 mA cm -2 .

[0009] Compared with the prior art, the present invention has the following beneficial effects:

[0010] Boron-doped diamond double-electrode system can realize NO in water 3 - ions and organic matter (phenol) are removed simultaneously with high removal rate. In addition, increasing the current density can accelerate the secondary oxidation of cathode products at the anode and increase N 2 This method is easy to operate and avoids secondary contamination of reagents. In addition, boron-doped diamond has good structural stability and corrosion resistance and can be used for a long time. BRIEF DESCRIPTION OF THE DRAWINGS

[0011] Figure 1 This is the XRD pattern of boron-doped diamond film on titanium substrate.

[0012] Figure 2 This is the Raman image of boron-doped diamond film on titanium substrate.

[0013] Figure 3 This is the SEM image of boron-doped diamond film on titanium substrate.

[0014] Figure 4 Boron-doped diamond film on titanium substrate simultaneously degrades NO in water 3 - Physical picture of ions and organic matter (phenol).

[0015] Figure 5 The results show that boron-doped diamond on titanium matrix can simultaneously treat NO in water at three current densities. 3 - The removal rate and generation rate of ions and organic matter (phenol) after 24 hours, where R: removal rate; S: generation rate.

[0016] Figure 6 These are the XRD, Raman and SEM images of boron-doped diamond before and after degradation. DETAILED DESCRIPTION

[0017] In order to further illustrate the present invention, the technical solutions provided by the present invention are described in detail below in conjunction with embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0018] Example 1

[0019] Boron-doped diamond on titanium matrix for NO degradation in water 3 - Ions and organic matter, the steps are as follows:

[0020] Step 1: Grind the 15*10*1mm titanium sheet with 400#, 600#, 800#, 1000# and 2000# sandpaper until the surface is bright, polish the surface with W0.5 diamond powder, perform ultrasonic treatment on the polished titanium sheet for 2 minutes to remove the residual diamond powder on the surface, and then blow dry with nitrogen.

[0021] Step 2: Place the titanium sheet obtained in step 1 into a microwave plasma chemical vapor deposition (MPCVD) chamber and introduce 300 sccm of H 2 , 6 sccm CH 4 and 8 sccm of H through trimethyl borate solution 2 The microwave power was set to 1900W, the pressure was controlled to 50Torr, and the growth time was 10h. After the growth was completed, the microwave power and pressure were reduced to 400W and 6Torr, all gases were turned off, and the sample was cooled to room temperature and then taken out to obtain a boron-doped diamond film grown on a titanium substrate.

[0022] Step 3: Use silica gel to seal the back of the diamond film grown on the titanium substrate obtained in step 2 to form a double-electrode system with a contact area of ​​1 cm between the electrode and the solution. 2 , electrolytes contain 1000mgL -1 NO 3 - and 100mgL -1 0.5MNa of phenol 2 SO 4solution, the current density was set to 10 mA cm -2 , the reaction time is 24h.

[0023] Step 4: Use an ultraviolet-visible spectrophotometer and a total organic carbon analyzer to detect the product content of the solution treated in step 3.

[0024] Example 2

[0025] Boron-doped diamond on titanium matrix for NO degradation in water 3 - Ions and organic matter, the steps are as follows:

[0026] Step 1: Grind the 15*10*1mm titanium sheet with 400#, 600#, 800#, 1000# and 2000# sandpaper until the surface is bright, polish the surface with W0.5 diamond powder, perform ultrasonic treatment on the polished titanium sheet for 2 minutes to remove the residual diamond powder on the surface, and then blow dry with nitrogen.

[0027] Step 2: Place the titanium sheet obtained in step 1 into a microwave plasma chemical vapor deposition (MPCVD) chamber and introduce 300 sccm of H 2 , 6 sccm CH 4 and 8 sccm of H through trimethyl borate solution 2 The microwave power was set to 1900W, the pressure was controlled to 50Torr, and the growth time was 10h. After the growth was completed, the microwave power and pressure were reduced to 400W and 6Torr, all gases were turned off, and the sample was cooled to room temperature and then taken out to obtain a boron-doped diamond film grown on a titanium substrate.

[0028] Step 3: Use silica gel to seal the back of the diamond film grown on the titanium substrate obtained in step 2 to form a double-electrode system with a contact area of ​​1 cm between the electrode and the solution. 2 , electrolytes contain 1000mgL -1 NO 3 - and 100mgL -1 0.5MNa of phenol 2 SO 4 solution, the current density was set to 15 mA cm -2 , the reaction time is 24h.

[0029] Step 4: Use an ultraviolet-visible spectrophotometer and a total organic carbon analyzer to detect the product content of the solution treated in step 3.

[0030] Example 3

[0031] Boron-doped diamond on titanium matrix for NO degradation in water3 - Ions and organic matter, the steps are as follows:

[0032] Step 1: Grind the 15*10*1mm titanium sheet with 400#, 600#, 800#, 1000# and 2000# sandpaper until the surface is bright, polish the surface with W0.5 diamond powder, perform ultrasonic treatment on the polished titanium sheet for 2 minutes to remove the residual diamond powder on the surface, and then blow dry with nitrogen.

[0033] Step 2: Place the titanium sheet obtained in step 1 into a microwave plasma chemical vapor deposition (MPCVD) chamber and introduce 300 sccm of H 2 , 6 sccm CH 4 and 8 sccm of H through trimethyl borate solution 2 The microwave power was set to 1900W, the pressure was controlled to 50Torr, and the growth time was 10h. After the growth was completed, the microwave power and pressure were reduced to 400W and 6Torr, all gases were turned off, and the sample was cooled to room temperature and then taken out to obtain a boron-doped diamond film grown on a titanium substrate.

[0034] Step 3: Use silica gel to seal the back of the diamond film grown on the titanium substrate obtained in step 2 to form a double-electrode system with a contact area of ​​1 cm between the electrode and the solution. 2 , electrolytes contain 1000mgL -1 NO 3 - and 100mgL -1 0.5MNa of phenol 2 SO 4 solution, the current density was set to 20 mA cm -2 , the reaction time is 24h.

[0035] Step 4: Use an ultraviolet-visible spectrophotometer and a total organic carbon analyzer to detect the product content of the solution treated in step 3.

[0036] Figure 1 The XRD pattern of boron-doped diamond film on titanium substrate is shown, which has obvious diamond characteristic peaks, proving that the diamond film is successfully prepared. Figure 2 The Raman image of boron-doped diamond film on titanium substrate is shown, which has obvious diamond characteristic peaks and boron doping characteristic peaks, proving that boron is successfully introduced. Figure 3 The SEM image of the boron-doped diamond film on titanium substrate is shown, in which fine diamond grains can be seen, proving that it has good crystallinity. Figure 4 Demonstrated simultaneous degradation of NO in water by boron-doped diamond films on titanium substrate 3- Actual picture of ions and organic matter (phenol). As the degradation process proceeds, the solution gradually turns dark yellow. This is due to the conversion of phenol into intermediate products such as aldehydes during the degradation process. After the degradation is completed, the solution becomes clear. Figure 5 10mAcm -2 、15mAcm -2 and 20mAcm -2 Simultaneous treatment of NO in water using boron-doped diamond on titanium matrix at three current densities 3 - The removal rate and generation rate of ions and organic matter (phenol) after 24 hours. The figure shows that high total organic carbon (TOC) removal rate can be achieved under three current densities. When the current density is 10mAcm -2 When NO 3 -The removal rate was the lowest (66.9%); when the current density was 15 mA cm -2 When NO 3 - The removal rate was the highest (92.6%). 2 The generation rate of N also increases. This is because increasing the current density can accelerate the secondary oxidation of cathode products at the anode, increasing the N 2 selectivity. Figure 6 The XRD, Raman and SEM images of boron-doped diamond before and after degradation show that the structure of the material does not change before and after degradation, indicating that the boron-doped diamond electrode has good stability. The above proves that the boron-doped diamond film on titanium substrate grown by microwave plasma chemical vapor deposition can achieve NO in water. 3 - Effective removal of ions and organic matter.

[0037] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. People can also obtain other embodiments based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.

Claims

1. A method for preparing a boron-doped diamond film, characterized in that: The following steps are involved: After the surface of the base metal is ground and polished, a boron-doped diamond film is grown on the surface by microwave plasma chemical vapor deposition.

2. The preparation method according to claim 1, characterized in that: The base metal includes titanium.

3. The preparation method according to claim 2, characterized in that: The process includes grinding the titanium with sandpaper until the surface is bright, polishing it with diamond micropowder, ultrasonically treating the polished titanium, and then drying it with nitrogen.

4. The preparation method according to claim 1, characterized in that: The flow rates of H2, CH4, and H2 after trimethyl borate for the boron-doped diamond film grown by microwave plasma chemical vapor deposition were 300 sccm, 6 sccm, and 8 sccm, respectively, the microwave power was set to 1900 W, the pressure was controlled to 50 Torr, and the growth time was 10 h.

5. The preparation method according to claim 4, characterized in that: After the growth is completed, the microwave power and pressure are reduced to 400W and 6Torr, all gases are turned off, and the sample is cooled to room temperature and then taken out to obtain a boron-doped diamond film grown on a titanium substrate.

6. A boron-doped diamond film prepared by the preparation method according to any one of claims 1 to 5.

7. Use of the boron-doped diamond film according to claim 6 in the simultaneous degradation of nitrate ions and organic matter in water.

8. A method for simultaneously degrading nitrate ions and organic matter in water, characterized in that: The method comprises forming a double-electrode system with a boron-doped diamond film grown on a titanium substrate, and simultaneously degrading nitrate ions and organic matter in water by an electrochemical method.

9. The method according to claim 8, characterized in that: During the electrochemical method, the current density is set to 10-20 mA cm -2 .

10. The method according to claim 8, characterized in that: The organic matter includes phenol.

Citation Information

Patent Citations

  • Method for preparing organic pollutant-degrading electrode material

    CN101905912A

  • Electrocatalytic oxidation electrode for sewage treatment and preparation method thereof

    CN108117137A

  • Preparation method of electrochemical alanine biosensor based on boron-doped diamond microelectrode and application thereof

    CN108362751A

  • Diamond nanoneedle array light absorption layer and preparation method thereof

    CN115928051A

  • Production process of diamond semiconductor heat sink material

    CN116904958A

Cited By

  • Method for regulating and controlling surface hydrophilicity and hydrophobicity of boron-doped diamond film and improving degradation performance of organic wastewater

    CN119793434A