Preparation method of water-repellent textile with self-recovery hydrophobic property after being naturally aired after being washed

Through the joint finishing of nano titanium dioxide gel and water repellent, the problem of degradation of water repellent performance of textiles after washing is solved, and the hydrophobic performance of fabrics is restored when they are naturally dried is achieved, energy consumption and cost are reduced, and fabrics are improved. Water repellent and breathable properties.

CN119020989AActive Publication Date: 2024-11-26LANYUN (QINGDAO) MARINE BIOTECHNOLOGY CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410934884.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-11-26
Estimated Expiration
2044-07-12

AI Technical Summary

Technical Problem

The water-repellent textiles will have a deterioration of water-repellent performance when they are washed and dried naturally after washing, and will need to be dried at high temperature to recover, resulting in large energy consumption and reduced user satisfaction.

Method used

The fabric is sorted with nanotitanium dioxide gel and water repellent agent. The fabric is restored through the photothermal conversion ability of the nanotitanium dioxide gel in the natural drying process and avoids high-temperature drying.

Benefits of technology

The hydrophobic performance of the fabric is restored automatically when it is washed and dried naturally after washing, reducing energy consumption and cost, and improving the water repellent, breathable and hydrophobic properties of the fabric.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004940994550000081
    Figure BDA0004940994550000081
  • Figure BDA0004940994550000101
    Figure BDA0004940994550000101
Patent Text Reader

Abstract

The invention discloses a preparation method of a water-repellent textile capable of naturally airing after washing and self-recovering hydrophobicity, and belongs to the field of textile printing and dyeing auxiliaries and textile dyeing and finishing processing. The method comprises the following steps: firstly, preparing nano titanium dioxide gel from a titanium source, an organic solvent, a reaction catalyst and deionized water, and then finishing the fabric step by step by using an ethanol solution of the nano titanium dioxide gel and an aqueous solution of a water repellent agent. The nano titanium dioxide can absorb ultraviolet rays in sunlight and convert light energy into heat energy, so that the obtained fabric not only has an excellent water-repellent effect (high static water contact angle, high hydrostatic pressure resistance and high spray-resistant grade), but also has the capabilities of not needing to be dried after being washed and effectively recovering the spray-resistant grade in conventional natural airing. The invention aims to solve the problems that the water repellency of a conventional water-repellent finishing fabric is reduced after being washed by water and is recovered after being dried at high temperature (more than or equal to 55 DEG C) in a taking process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing a water-repellent textile with self-recovering hydrophobic properties after washing and naturally drying, and belongs to the field of textile printing and dyeing auxiliaries and textile dyeing and finishing. Background Art

[0002] With the development of science and technology and the continuous improvement of people's living standards, water-repellent textiles have gradually come into the public eye and have been widely used. Although the fabrics treated with conventional water-repellents have good water-repellent effects, there is a problem that the water-repellent performance decreases after natural drying after washing, and the water-repellent performance recovers after high-temperature drying (≥55℃). This has led to a decline in consumer satisfaction with water-repellent textiles in countries where natural drying is the main way to dry clothes. Summary of the invention

[0003] In view of the above problems, in order to improve the water repellent effect of water repellent finished fabrics after washing and natural drying, and to avoid the energy consumption of high temperature drying, the present invention constructs a preparation method of water repellent textiles with self-recovery of hydrophobic properties after washing and natural drying. The present invention uses nano titanium dioxide gel and water repellent to finish fabrics. The prepared fabrics not only have excellent water repellent properties, but also do not need high temperature drying after washing, and the water repellent properties can be restored by natural drying.

[0004] The object of the present invention is to provide a method for preparing a water-repellent textile with self-recovering hydrophobic properties after washing and drying naturally, the method comprising:

[0005] (1) adding a mixed solution B of an organic solvent, a reaction catalyst and deionized water dropwise into a mixed solution A of a titanium source and an organic solvent, and reacting under stirring to obtain a nano-titanium dioxide solution;

[0006] (2) removing the organic solvent from the nano-titanium dioxide solution obtained in step (1) by rotary evaporation and aging at room temperature to obtain a nano-titanium dioxide gel;

[0007] (3) dipping the fabric into the ethanol solution of the nano-titanium dioxide gel obtained in step (2) and then drying;

[0008] (4) The fabric obtained in step (3) is immersed in an aqueous solution of a water repellent and then finished by a pad baking process.

[0009] In one embodiment of the present invention, the mass ratio of the mixed solution A to the mixed solution B in step (1) is 0.8 to 1.5:1.

[0010] In one embodiment of the present invention, the components in the mixed solution A in step (1) include, by mass percentage, 5-20% titanium source and 80-95% organic solvent; the components in the mixed solution B include, by mass percentage, 80-90% organic solvent and 1-10% reaction catalyst, with the remainder being deionized water.

[0011] In one embodiment of the present invention, the titanium source in step (1) is at least one of ethyl titanate, tetrabutyl titanate, tetraisopropyl titanate, titanium tetrachloride or titanium trichloride; the organic solvent is at least one of ethanol, propanol or isopropanol; and the reaction catalyst is at least one of glacial acetic acid, nitric acid or hydrochloric acid.

[0012] In one embodiment of the present invention, the addition rate of the mixed solution B in step (1) is 1-10 g / min, the stirring speed is 100-1000 r / min; and the reaction time is 1-8 h.

[0013] In one embodiment of the present invention, the aging time in step (2) is 12-48 hours.

[0014] In one embodiment of the present invention, the concentration of nano-titanium dioxide in the ethanol solution of nano-titanium dioxide gel in step (3) is 0.5-10 g / L; the rolling rate during the dipping and rolling process is 80-150%, the drying temperature is 80-100° C., and the drying time is 1-5 min.

[0015] In one embodiment of the present invention, the water repellent in step (4) comprises at least one of an acrylate-based fluorine-free water repellent, a silicone-based fluorine-free water repellent, a polyurethane-based fluorine-free water repellent or a fluorine-containing water repellent.

[0016] In one embodiment of the present invention, the concentration of the water repellent in step (4) is 50-100 g / L, and the rolling rate in the rolling baking process is 50-150%.

[0017] In one embodiment of the present invention, in step (4), when finishing the fabric using a pad baking process, the fabric is dipped in an aqueous solution of a water repellent, and then pre-baked and then baked, wherein the pre-baking temperature is 80-110°C, the pre-baking time is 1-5 min, the baking temperature is 130-160°C, and the baking time is 1-5 min.

[0018] In one embodiment of the present invention, the fabric comprises one of cotton, wool, linen, polyester and nylon fabrics.

[0019] The present invention has the following beneficial effects:

[0020] 1. The present invention prepares a water-repellent textile with self-recovering hydrophobic properties after washing and drying naturally by combining nano titanium dioxide gel with a water repellent agent to finish the fabric.

[0021] 2. The self-recovering water-repellent fabric prepared by the present invention can absorb ultraviolet rays in sunlight during natural drying after washing, and the water-repellent effect is restored to the level before washing, which solves the problem that the water-repellent effect of conventional water-repellent finishing fabrics decreases after washing and needs to be dried at high temperature (≥55°C) to recover, which is a cumbersome process and consumes a lot of energy. The self-recovering water-repellent fabric can reduce the temperature conditions required for the recovery of water-repellent performance after washing, save energy, and reduce costs.

[0022] 3. The present invention uses nano titanium dioxide ethanol solution to finish the fabric before water-repellent finishing, thereby improving the surface roughness of the water-repellent fabric, and the fabric can obtain a better water-repellent effect after finishing.

[0023] 4. The combined finishing method of nano titanium dioxide and water repellent provided by the present invention is simple to operate, the product has good uniformity, and can form a water repellent film on the surface of the fabric, greatly improving the water repellency of the fabric. In general, the finished fabric has good water repellency, air permeability, and self-recovery of hydrophobic properties. DETAILED DESCRIPTION

[0024] The present invention is further described below in conjunction with specific examples. The examples are only used to explain the present invention and are not used to limit the scope of the present invention.

[0025] Common water repellents available on the market are divided into two categories: fluorine-free (acrylates, silicones, polyurethanes) and fluorine-containing. The water repellents used in the examples and comparative examples of the present invention are acrylate fluorine-free water repellent (fluorine-free 1), silicone fluorine-free water repellent (fluorine-free 2), polyurethane fluorine-free water repellent (fluorine-free 3), and fluorine-containing water repellent 1 (fluorine 1), and the preparation methods are as follows:

[0026] Preparation of acrylate fluorine-free water repellent 1 (fluorine-free 1):

[0027] A mixture of acrylate monomers (octadecyl acrylate, tetrabutyl acrylate, methyl methacrylate, and glycidyl methacrylate in a molar ratio of 1:1:1:0.4) was added to a deionized aqueous solution of octadecyl trimethyl ammonium chloride and polyoxyethylene stearate (polyoxyethylene number is 20) accounting for 10% of the total mass of the reaction monomers for emulsification (the mass ratio of octadecyl trimethyl ammonium chloride to polyoxyethylene stearate is 1:2.5, and the total mass of the reaction monomers accounts for 20% of the mass of the emulsion). After the emulsion was heated to 80°C, an aqueous solution of azobisisobutylamidine accounting for 1% of the total mass of the reaction monomers (the mass ratio of azobisisobutylamidine to water is 1:20) was added dropwise. After the addition was completed, the reaction was kept warm for 3 hours and naturally cooled to room temperature to obtain an acrylate fluorine-free water repellent (fluorine-free 1).

[0028] Preparation of silicone-based fluorine-free water repellent 2 (fluorine-free 2):

[0029] Methylpropionyl chloride was added to an acetone solution of aminopropyl di-terminated polydimethylsiloxane (molecular weight 1000) in three batches (with an interval of 0.5 h) (the molar ratio of methylpropionyl chloride to aminopropyl di-terminated polydimethylsiloxane was 1:1, and the mass ratio of aminopropyl di-terminated polydimethylsiloxane to acetone was 1:2), and the reaction was carried out at room temperature for 4 h. A deionized water solution of octadecyltrimethylammonium chloride and polyoxyethylene stearate (polyoxyethylene number was 20) accounting for 10% of the total mass of the reaction monomers was added for emulsification (the mass ratio of octadecyltrimethylammonium chloride to polyoxyethylene stearate was 1:2, and the total mass of the reaction monomers accounted for 20% of the mass of the emulsion). After high-speed mechanical stirring to obtain an emulsion, the acetone was removed by rotary evaporation to obtain a silicone-based fluorine-free water repellent (fluorine-free 2).

[0030] Preparation of polyurethane fluorine-free water repellent 3 (fluorine-free 3):

[0031] Add isophorone diisocyanate dropwise to polytetrahydrofuran (the molar ratio of isophorone diisocyanate to polytetrahydrofuran is 3.2:1), stir and react for 2 hours in an anhydrous environment at 85°C, cool to 45°C, add N-methyldiethanolamine dissolved in acetone (the molar ratio of isophorone diisocyanate to N-methyldiethanolamine is 4:1), and continue to react for 1.5 hours. Raise the temperature to 65°C, add trimethylolpropane monoallyl ether (the molar ratio of isophorone diisocyanate to trimethylolpropane monoallyl ether is 4:1) and continue to react for 2 hours. Add methyl ethyl ketone oxime (the molar ratio of isophorone diisocyanate to methyl ethyl ketone oxime is 3:1) to the reactor and react at 70°C for 3 hours for end-capping. After the end-capping, the obtained polyurethane is added with acrylate monomer (methyl methacrylate: butyl acrylate: octadecyl acrylate molar ratio = 1:1:1, the total mass ratio of acrylate monomer to polyurethane monomer is 1:1), the reaction mixture is cooled to 35°C, and acetic acid (neutralization degree is 100%) is added as a neutralizer, and the reaction is carried out for 0.5 hours. Deionized water (the total mass of acrylate monomer and polyurethane monomer is 4 times that of deionized water) is slowly added under vigorous stirring (1200r / min), the temperature is raised to 75°C, and an aqueous solution of azobisisobutylamidine (the mass ratio of azobisisobutylamidine to water is 1:20) accounting for 1% of the total weight of acrylate monomer is added dropwise to the reactor, and the reaction is kept warm for 3 hours to obtain a polyurethane fluorine-free water repellent (fluorine-free 3).

[0032] Preparation of fluorine-containing water repellent 1 (fluorine 1):

[0033] A mixture of 1H,1H,2H,2H-perfluorohexanol acrylate: octadecyl acrylate: methyl methacrylate: glycidyl methacrylate (molar ratio of 2:1:1:0.4) was added to a deionized aqueous solution of octadecyltrimethylammonium chloride and polyoxyethylene stearate (polyoxyethylene number is 20) accounting for 10% of the total mass of the reaction monomers for emulsification (wherein the mass ratio of octadecyltrimethylammonium chloride to polyoxyethylene stearate is 1:3, and the total mass of the reaction monomers accounts for 20% of the mass of the emulsion), and after the emulsion was heated to 80°C, an aqueous solution of azobisisobutylamidine (mass ratio of azobisisobutylamidine to water is 1:20) accounting for 1% of the total mass of the reaction monomers was added dropwise, and after the addition was completed, the reaction was kept warm for 3 hours and naturally cooled to room temperature to obtain a fluorine-containing water repellent 1 (fluorine 1).

[0034] Test method:

[0035] The spray resistance of the fabric's water repellency is evaluated by the water level, and the water level of the fabric after drying is tested according to "GB / T 4745-2012 Testing and evaluation of the waterproof performance of textiles by water level test".

[0036] The water repellency and water wetting resistance of the fabric are evaluated by the static water contact angle. The static contact angle of the fabric after water repellent finishing is measured using a contact angle meter: 5 μL of water droplets are added to five different locations on the fabric, and the static contact angle is measured.

[0037] The static water resistance of the fabric water repellency is carried out according to the AATCC-127-2013 "Water Resistance: Hydrostatic Pressure Test" standard.

[0038] Fabric washing and drying parameters: The fabric was washed according to GB / T8629-2017 “Household Washing and Drying Procedure for Textile Experiments” and then exposed to sunlight for 1 hour at 30°C in a sunlight fastness tester.

[0039] The evaluation of fabric softness is carried out in accordance with AATCC TM 202 "Evaluation of Relative Hand Feel of Textiles and Garments: Instrumental Method".

[0040] Embodiment 1:

[0041] Nano-titanium dioxide gel was prepared and combined with water repellent to finish the fabric in the following steps:

[0042] Preparation of nano-titanium dioxide gel:

[0043] At room temperature, tetrabutyl titanate was slowly added to a mixture of ethanol and glacial acetic acid (the mass ratio of tetrabutyl titanate, ethanol and glacial acetic acid was 10:80:10) to obtain a mixture A; ethanol, glacial acetic acid and deionized water were mixed at a mass ratio of 80:10:10 to obtain a mixture B; the mass ratio of the mixture A to the mixture B was 1:1; the B solution was added to the A solution at a speed of 2 g / min, and the stirring speed was maintained at 600 r / min. After the addition was completed, the reaction was carried out for 4 hours. After the ethanol was removed by rotary evaporation, it was allowed to stand for 24 hours to obtain a titanium dioxide gel.

[0044] Fabric Finishing:

[0045] A certain amount of nano titanium dioxide gel was diluted in ethanol to prepare a 1g / L titanium dioxide ethanol solution. The cotton fabric was dipped in the above solution and then rolled, with a rolling rate of 100%, and baked at 100℃ for 2min. Then, the fabric was dipped in an aqueous solution (60g / L) of acrylic ester fluorine-free water repellent 1 (fluorine-free 1) to finish the fabric. The rolling and baking process was adopted, with two dips and two rolls, a rolling rate of 100%, pre-baked at 100℃ for 2min, and baked at 150℃ for 3min. The relevant parameters of the treated fabric are shown in Table 1.

[0046] Embodiment 2-4:

[0047] Preparation of nano-titanium dioxide gel: same as in Example 1.

[0048] Fabric finishing: only the concentration of the nano-titanium dioxide treatment solution was changed (0.5 g / L in Example 2, 5 g / L in Example 3, and 10 g / L in Example 4), and the rest was the same as in Example 1. The relevant parameters of the treated fabric are shown in Table 1.

[0049] Embodiment 5-7:

[0050] Preparation of nano-titanium dioxide gel: same as in Example 1.

[0051] Fabric finishing: only the type of water repellent was changed (Example 5 was silicone-based fluorine-free water repellent 2 (fluorine-free 2), Example 6 was polyurethane-based fluorine-free water repellent 3 (fluorine-free 3), and Example 7 was fluorine-containing water repellent 1 (fluorine 1). Others were the same as Example 1. The relevant parameters of the treated fabrics are shown in Table 2.

[0052] Embodiment 8-9:

[0053] Preparation of nano-titanium dioxide gel: same as in Example 1.

[0054] Fabric finishing: only the type of fabric was changed (polyester in Example 8 and nylon in Example 9), and the rest was the same as in Example 1. The relevant parameters of the treated fabric are shown in Table 1.

[0055] Embodiment 10:

[0056] The nano titanium dioxide solution was prepared and the fabric was treated with a water repellent agent in the following steps:

[0057] Preparation of nano-titanium dioxide gel:

[0058] At room temperature, ethyl titanate was slowly added to a mixture of propanol and nitric acid (1 g / L) (the mass ratio of ethyl titanate, propanol and nitric acid was 20:75:5) to obtain a mixture A; propanol, nitric acid (1 g / L) and deionized water were mixed at a mass ratio of 80:5:15 to obtain a mixture B; the mass ratio of the mixture A to the mixture B was 0.8:1; the B solution was added to the A solution at a speed of 1 g / min, and the stirring speed was maintained at 100 r / min. After the addition was completed, the reaction was carried out for 1 hour. After the ethanol was removed by rotary evaporation, it was allowed to stand for 48 hours to obtain titanium dioxide gel.

[0059] Fabric Finishing:

[0060] A certain amount of nano titanium dioxide gel was diluted in ethanol to prepare a 1g / L titanium dioxide ethanol solution. The cotton fabric was dipped in the above solution and then rolled, with a rolling rate of 80%, and baked at 80℃ for 5min. Then, the fabric was dipped in an aqueous solution (50g / L) of acrylic ester fluorine-free water repellent 1 (fluorine-free 1) to finish the fabric. The rolling and baking process was adopted, with two dips and two rolls, a rolling rate of 150%, pre-baked at 80℃ for 5min, and baked at 160℃ for 1min. The relevant parameters of the treated fabric are shown in Table 1.

[0061] Embodiment 11:

[0062] The nano titanium dioxide solution was prepared and the fabric was treated with a water repellent agent in the following steps:

[0063] Preparation of nano-titanium dioxide gel:

[0064] At room temperature, tetraisopropyl titanate was slowly added to a mixture of isopropanol and hydrochloric acid (0.5 g / L) (the mass ratio of ethyl titanate, isopropanol and hydrochloric acid was 20:60:20) to obtain a mixture A; isopropanol, hydrochloric acid (0.5 g / L) and deionized water were mixed at a mass ratio of 70:10:20 to obtain a mixture B; the mass ratio of the mixture A to the mixture B was 1.5:1; the B solution was added to the A solution at a speed of 1 g / min, and the stirring speed was maintained at 1000 r / min. After the addition was completed, the reaction was carried out for 8 hours. After the ethanol was removed by rotary evaporation, it was allowed to stand for 12 hours to obtain titanium dioxide gel.

[0065] Fabric Finishing:

[0066] A certain amount of nano titanium dioxide gel was diluted in ethanol to prepare a 1g / L titanium dioxide ethanol solution. The cotton fabric was dipped in the above solution and then rolled, with a rolling rate of 150%, and baked at 90℃ for 3min. Then, the fabric was dipped in an aqueous solution (100g / L) of acrylic ester fluorine-free water repellent 1 (fluorine-free 1) to finish the fabric. The rolling and baking process was adopted, with two dips and two rolls, a rolling rate of 50%, pre-baked at 90℃ for 3min, and baked at 130℃ for 5min. The relevant parameters of the treated fabric are shown in Table 1.

[0067] Comparative Example 1-2:

[0068] Preparation of nano-titanium dioxide gel: same as in Example 1.

[0069] Fabric finishing: only the concentration of the nano-titanium dioxide treatment solution was changed (0.1 g / L for control example 1 and 20 g / L for control example 2), and the rest was the same as in Example 1. The relevant parameters of the treated fabric are shown in Table 1.

[0070] Comparative Example 3:

[0071] The nano titanium dioxide solution was prepared and the fabric was treated with a water repellent agent in the following steps:

[0072] Preparation of nano-titanium dioxide gel:

[0073] At room temperature, tetrabutyl titanate was slowly added to a mixture of ethanol and glacial acetic acid (the mass ratio of tetrabutyl titanate, ethanol and glacial acetic acid was 1:90:9) to obtain a mixture A; ethanol, glacial acetic acid and deionized water were mixed at a mass ratio of 40:3:57 to obtain a mixture B; A:B = (2:1, mass ratio); liquid B was added to liquid A at a speed of 2g / min, and stirred at a speed of 600r / min. After the addition was completed, the reaction was carried out for 4h. After the ethanol was removed by rotary evaporation, it was allowed to stand for 24h to obtain titanium dioxide gel.

[0074] Fabric finishing: Same as Example 1. The relevant parameters of the treated fabric are shown in Table 1.

[0075] Comparative Example 4:

[0076] Nano-titanium dioxide finishing: Take commercial nano-titanium dioxide powder and dilute it in ethanol to prepare a 1g / L titanium dioxide ethanol solution.

[0077] Fabric finishing: Same as Example 1. The relevant parameters of the treated fabric are shown in Table 1.

[0078] Comparative Example 5:

[0079] Preparation of Nano-TiO2 Hydrosol:

[0080] After tetrabutyl titanate and glacial acetic acid are uniformly mixed at room temperature (the mass ratio of tetrabutyl titanate to glacial acetic acid is 10:1), they are added into a 0.3% hydrochloric acid solution (the mass of the hydrochloric acid solution is 4 times that of tetrabutyl titanate), and the temperature is raised to 50°C and reacted for 30 minutes to obtain nano titanium dioxide hydrosol.

[0081] Fabric finishing: cotton fabric was dipped in the above solution and then rolled, with a rolling rate of 100%, baked at 100°C for 2 min, and then dipped in an aqueous solution (60 g / L) of acrylic ester non-fluorine water repellent 1 (non-fluorine 1) to finish the fabric, using a rolling and baking process, two dips and two rolls, with a rolling rate of 100%, pre-baked at 100°C for 2 min, and baked at 150°C for 3 min. The relevant parameters of the treated fabric are shown in Table 1.

[0082] Comparative Examples 6-9:

[0083] The fabric was not treated with nano titanium dioxide, but only treated with a water repellent. The water repellents were fluorine-free 1 (control example 6), fluorine-free 2 (control example 7), fluorine-free 3 (control example 8), and fluorine 1 (control example 9). Other parameters of the water repellent treatment were the same as those in Example 1, specifically: the fabric was treated with an aqueous solution (60 g / L) of a water repellent, and a padding and baking process was adopted, with two dips and two pads, a padding rate of 100%, pre-baking at 100°C for 2 minutes, and baking at 150°C for 3 minutes. The relevant parameters of the treated fabric are shown in Table 1.

[0084] Comparative Examples 10-11:

[0085] The fabric was not treated with nano-titanium dioxide, but only treated with a water repellent. The amount of the water repellent was 30 g / L (Comparative Example 10) and 150 g / L (Comparative Example 11), and the other parameters of the water repellent treatment were the same as those in Example 1. The relevant parameters of the treated fabric are shown in Table 1.

[0086] Comparative Example 12:

[0087] The fabric was only treated with titanium dioxide gel finishing without water repellent finishing. The titanium dioxide finishing parameters were the same as those in Example 1, specifically: a certain amount of nano titanium dioxide gel was diluted in ethanol to prepare a 1 g / L titanium dioxide ethanol solution. The cotton fabric was immersed in the above solution and then rolled, with a rolling rate of 100%, and dried at 100°C for 2 minutes.

[0088] Table 1 Relevant parameters of treated fabrics

[0089]

[0090] Note: The untreated cotton fabric was completely wetted by water before and after washing, and its hydrostatic pressure resistance was 170 mm and its softness was 53.8.

[0091] - indicates complete wetting.

[0092] Self-recovery effect of product hydrophobic performance: The spray resistance level after washing is the main evaluation index of the water-repellent self-recovery performance of water-repellent fabrics after washing and drying naturally. It can be seen from Examples 1-4 in Table 1 that the cotton fabrics obtained by the combined finishing of titanium dioxide and water repellent according to the method provided by the present invention have good spray resistance after washing and drying naturally (according to the detection characterization method, the highest water repellency level of the fabric is 5), mainly because titanium dioxide can increase the surface roughness of the fabric and has photothermal conversion ability. It can effectively convert light into heat under the same sunlight irradiation, promoting the recovery of the water repellent performance of the fabric; at the same time, Examples 1-4 also have good static water contact angle, hydrostatic pressure resistance, softness, and spray resistance before washing.

[0093] It can be seen from Examples 1-4 and Control Example 1 in Comparative Table 1 that when the amount of titanium dioxide used in the finishing process is too low, its static water contact angle, hydrostatic pressure resistance, and spray resistance level before and after washing are all reduced, especially the spray resistance level after washing is level 2, that is, the water repellent performance of the fabric cannot be restored after washing and drying. The reason is that the light-heat conversion ability of the fabric decreases, and the main reason for the decrease in the static water contact angle is that the surface roughness of the fabric decreases due to insufficient titanium dioxide. It can be seen from Examples 1-4 and Control Example 2 in Comparative Table 1 that when the amount of titanium dioxide used in the finishing process is too high, although the water repellent performance and the spray resistance level before and after washing of the fabric are good, the softness of the fabric is greatly reduced.

[0094] By comparing Examples 1-4 and Control Example 3 in Table 1, it can be seen that the titanium dioxide preparation parameters are beyond the range provided by the present invention, the obtained titanium dioxide is insufficient, and the spray resistance level of the fabric after washing and drying naturally is Level 2, that is, the water repellent performance of the fabric cannot be restored after washing and drying naturally.

[0095] By comparing Examples 1-4 and Control Example 4 in Table 1, it can be seen that the fabric treated with commercial titanium dioxide and a water repellent has a spray resistance level of 2 after being washed and dried naturally, that is, the water repellent properties of the fabric cannot be restored after being washed and dried naturally. The reason is that commercial titanium dioxide has been calcined at high temperature, and its surface lacks chemical groups that can react with the fabric and the water repellent. It is easy to detach from the fabric during the washing process and cannot play its photothermal conversion role.

[0096] By comparing Examples 1-4 and Control Example 5 in Table 1, it can be seen that although the fabric obtained in Control Example 5 has a good static contact angle, hydrostatic pressure resistance and spray resistance before washing, the spray resistance after natural drying after washing is lower than that of the fabrics obtained in Examples 1-4. The main reason is that Control Example 5 directly uses the prepared nano-titanium dioxide hydrosol to impregnate the fabric. During the baking process, the water evaporation rate in the fabric surface treatment liquid is different. Nano-titanium dioxide migrates on the fabric surface with water, resulting in its enrichment in local areas of the fabric and existing in a relatively large volume, which reduces the contact area between titanium dioxide and light and seriously reduces the photothermal conversion capacity of the fabric.

[0097] By comparing Examples 1-4 and Control Example 6 in Table 1, it can be seen that the static contact angle, hydrostatic pressure resistance, and spray resistance level before and after washing and drying naturally after washing of the fabric obtained without using titanium dioxide for finishing are all reduced, especially the spray resistance level after washing and drying naturally is level 2, that is, the water repellent performance of the fabric cannot be restored after washing and drying naturally.

[0098] By comparing Example 1 and Control Examples 6-9 in Table 1, it can be seen that the fabric obtained by finishing without titanium dioxide and changing the type of water repellent only has a slight effect on the static water contact angle and the hydrostatic pressure resistance, which is mainly due to the difference in the types of water repellents, which is reflected in the fact that the fluorine-containing water repellent is more effective than the fluorine-free water repellent, but its spray resistance level is level 5 before washing and level 3 after washing and natural drying, that is, the water repellent performance of the fabric cannot be restored after washing and natural drying.

[0099] By comparing Example 1, Comparative Example 6 and Comparative Examples 10-11 in Table 1, it can be seen that when the fabric is not finished with titanium dioxide and the amount of water repellent is reduced (Comparative Example 10), the water repellent cannot effectively cover the fabric fibers, and the water repellent properties of the fabric are reduced; when the amount of water repellent is increased (Comparative Example 11), although the static water contact angle and hydrostatic pressure resistance of Comparative Example 11 are higher than those of Comparative Example 5, the spray resistance of the fabric before and after washing is not improved, but the softness is greatly reduced, indicating that the combined finishing of titanium dioxide and water repellent is not suitable. Only by increasing the amount of water repellent, the water repellent property of the fabric cannot be restored by drying it naturally after washing.

[0100] By comparing Example 1 and Comparative Example 12 in Table 1, it can be seen that the fabric does not have water-repellent properties when only the prepared titanium dioxide gel is used for treatment without a water-repellent agent. This is mainly because the surface of titanium dioxide is rich in hydroxyl groups and is hydrophilic, and the surface of the fabric lacks effective coverage of groups that can reduce its surface energy, which are provided by the water-repellent agent.

[0101] Table 2 Relevant parameters of treated fabrics

[0102]

[0103] Note: Untreated cotton fabrics were completely wetted by water before washing and after washing, with a hydrostatic pressure resistance of 170 mm and a softness of 53.8. Untreated polyester fabrics were completely wetted by water before washing and after washing, with a hydrostatic pressure resistance of 210 mm and a softness of 48.8. Untreated nylon fabrics were completely wetted by water before washing and after washing, with a hydrostatic pressure resistance of 190 mm and a softness of 66.8.

[0104] It can be seen from the comparison between Example 1 and Example 5-11 in Table 2 that the fabrics obtained by the combined finishing of titanium dioxide and water repellent according to the method provided by the present invention all have good spray resistance after washing and natural drying, mainly because titanium dioxide can increase the surface roughness of the fabric and has light-heat conversion ability, and can effectively convert light into heat under the same sunlight irradiation, thereby promoting the recovery of the water repellency of the fabric; at the same time, the examples all have good static water contact angle, hydrostatic pressure resistance, softness, and water-staining level before washing and after washing and drying; the water repellency difference between Example 5-7 and Example 1 is mainly The reason for this is the difference in the types of water repellents. The reason why Example 7 is higher than other examples is that the water repellent used is a fluorine-containing water repellent, which can more effectively reduce the surface energy of the fabric. The reason for the difference in water repellency between Examples 8-9 and Example 1 is that the types of fabrics used are different, where Example 8 is polyester, Example 9 is nylon, and Example 1 is cotton. Different fabrics have slightly different adsorption capacities for water repellents and titanium dioxide. The reason for the difference in water repellency between Examples 10-11 and Example 1 is that the titanium dioxide size and content are slightly different due to different parameters in the preparation of titanium dioxide.

Claims

1. A method for preparing a water-repellent textile with self-recovering hydrophobic properties that can be naturally dried after washing, characterized in that: The method comprises: (1) adding a mixed solution B of an organic solvent, a reaction catalyst and deionized water dropwise into a mixed solution A of a titanium source and an organic solvent, and reacting under stirring to obtain a nano-titanium dioxide solution; (2) removing the organic solvent from the nano-titanium dioxide solution obtained in step (1) by rotary evaporation and aging at room temperature for 12 to 48 hours to obtain a nano-titanium dioxide gel; (3) dipping the fabric into the ethanol solution of the nano-titanium dioxide gel obtained in step (2) and then drying; (4) The fabric obtained in step (3) is immersed in an aqueous solution of a water repellent and then finished by a pad baking process.

2. The method according to claim 1, characterized in that In the step (1), the mass ratio of the mixed solution A to the mixed solution B is 0.8 to 1.5:

1.

3. The method according to claim 1, characterized in that In step (1), the components of the mixed solution A include 5-20% titanium source and 80-95% organic solvent by mass percentage; the components of the mixed solution B include 80-90% organic solvent and 1-10% reaction catalyst, and the balance is deionized water by mass percentage.

4. The method according to claim 1, characterized in that: In step (1), the titanium source is at least one of ethyl titanate, tetrabutyl titanate, tetraisopropyl titanate, titanium tetrachloride or titanium trichloride; the organic solvent is at least one of ethanol, propanol or isopropanol; and the reaction catalyst is at least one of glacial acetic acid, nitric acid or hydrochloric acid.

5. The method according to claim 1, characterized in that In step (1), the addition rate of the mixed solution B is 1-10 g / min, the stirring speed is 100-1000 r / min; and the reaction time is 1-8 h.

6. The method according to claim 1, characterized in that The concentration of nano-titanium dioxide in the ethanol solution of nano-titanium dioxide gel in step (3) is 0.5-10 g / L; the rolling rate in the dipping and rolling process is 80-150%, the drying temperature is 80-100° C., and the drying time is 1-5 min.

7. The method according to claim 1, characterized in that The water repellent in step (4) includes at least one of an acrylate-based fluorine-free water repellent, a silicone-based fluorine-free water repellent, a polyurethane-based fluorine-free water repellent or a fluorine-containing water repellent.

8. The method according to claim 1, characterized in that The concentration of the water repellent in step (4) is 50-100 g / L, and the rolling rate in the rolling baking process is 50-150%.

9. The method according to claim 1, characterized in that: In step (4), when finishing the fabric using the pad baking process, the fabric is dipped in the aqueous solution of the water repellent, and then pre-baked and then baked. The pre-baking temperature is 80-110°C, the pre-baking time is 1-5 minutes, and the baking temperature is 130-160°C, and the baking time is 1-5 minutes.

10. The method according to any one of claims 1 to 9, characterized in that: The fabric comprises one of cotton, wool, linen, polyester and nylon fabric.

Citation Information

Patent Citations

  • Freon-free super hydrophobic UV resistant cotton fabric and method for preparing same

    CN101768854A

  • Fluorine-free superhydrophobic finishing agent containing modified nano silicon dioxide hydrosol and application thereof

    CN102021819A

  • Method for clearing up nanometer uvioresistant antibacterial self-cleaning fabric

    CN102277724A

  • Preparation method for fluoride-free super-hydrophobic cotton fabric

    CN105350282A

  • Titanium dioxide / baffeta with super-hydrophobic and self-cleaning functions

    CN107653673A