Preparation method of super-oleophylic / super-hydrophobic ZnO coated carbon fiber oil-water separation membrane

By preparing super-lipophilic/superhydrophobic ZnO nanoclad layer on carbon fiber, the problems of existing oil-water separation materials are solved, and efficient oil-water separation is achieved and good durability and regeneration capabilities are achieved.

CN119034509AInactive Publication Date: 2024-11-29XIAN UNIV OF TECH
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411296393.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-18
Publication Date
2024-11-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing oil-water separation materials have small oil-water selectivity and separation flux in the oil-water system, and are prone to deterioration in performance due to impurity contamination, so they cannot be used normally.

Method used

The preparation method of super-lipophilic/super-hydrophobic ZnO coated carbon fiber oil-water separation membrane is used to prepare ZnO gel layer by cleaning carbon fiber, low-pressure vacuum plasma technology, sol-gel method, and ZnO nanoparticles are grown and low-surfaced. It can be modified to obtain ZnO nano-coated carbon fibers with super lipophilic/superhydrophobic properties.

Benefits of technology

Improves the oil-water selectivity and separation flux of the oil-water separation membrane, has good wear resistance, friction resistance and cycle stability, and is suitable for oil-water separation in complex acid and alkali environments, and realizes the material through low-pressure vacuum plasma technology. regeneration.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119034509A_ABST
    Figure CN119034509A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a super-oleophylic / super-hydrophobic ZnO coated carbon fiber oil-water separation membrane, which belongs to the technical field of oil-water separation, and is specifically implemented according to the following steps: step 1, cleaning the surface of a carbon fiber, and activating the carbon fiber by adopting a low-pressure vacuum plasma technology; step 2, preparing carbon fibers coated with a ZnO gel layer by using a sol-gel method; 3, processing the carbon fiber coated with the ZnO gel layer prepared in the step 2 by adopting a low-pressure vacuum plasma technology to obtain ZnO coated CF; step 4, continuously growing ZnO nanoparticles on the ZnO (at) CF by adopting a hydrothermal method to obtain ZnONps (at) CF; and step 5, carrying out low surface energy modification on the ZnONps (at) CF to obtain the ZnO nano-coated carbon fiber with the super-oleophylic / super-hydrophobic characteristic. The super-oleophylic / super-hydrophobic ZnO nano-coated carbon fiber prepared by the method disclosed by the invention has excellent oil-water selectivity and separation flux.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of oil-water separation, and in particular relates to a method for preparing a super-oleophilic / super-hydrophobic ZnO-coated carbon fiber oil-water separation membrane. Background Art

[0002] The leakage of oily wastewater and organic solvents poses a huge threat to marine life and human safety. Although traditional oil-water separation materials such as clay and wheat straw are low-cost, they have poor oil-water selectivity and poor recyclability in oil-water systems, which greatly limits their application in the engineering field. Carbon fiber can be used as a potential choice for oil-water separation filter materials due to its excellent properties such as high temperature resistance, friction resistance, and corrosion resistance, but carbon fiber does not have super wetting properties and cannot be directly used in oil-water separation. In addition, after a long period of oil-water separation, the surface of the oil-water filtration membrane material will be contaminated by impurities and the pores will be blocked by impurities, resulting in a deterioration in oil-water selectivity and a decrease in separation flux, making it impossible to continue to use normally. Summary of the invention

[0003] The purpose of the present invention is to provide a method for preparing a super-oleophilic / super-hydrophobic ZnO-coated carbon fiber oil-water separation membrane, so as to solve the problems of low oil-water selectivity and separation flux of existing oil-water separation materials.

[0004] The technical solution adopted by the present invention is a method for preparing a super oleophilic / super hydrophobic ZnO coated carbon fiber oil-water separation membrane, which is specifically implemented according to the following steps:

[0005] Step 1, cleaning the surface of the carbon fiber, and then activating the carbon fiber using low-pressure vacuum plasma technology;

[0006] Step 2, preparing carbon fiber coated with ZnO gel layer by sol-gel method;

[0007] Step 3, using low-pressure vacuum plasma technology to treat the carbon fiber coated with the ZnO gel layer prepared in step 2 to obtain ZnO@CF;

[0008] Step 4, using a hydrothermal method to continue growing ZnO nanoparticles on ZnO@CF to obtain ZnONps@CF;

[0009] Step 5, performing low surface energy modification on the ZnONps@CF obtained in step 4 to obtain super oleophilic / super hydrophobic ZnO nano-coated carbon fibers.

[0010] The present invention is also characterized in that:

[0011] The specific process of step 1 is:

[0012] Step 1.1, soaking the carbon fiber in sodium carbonate solution, rinsing with deionized water, soaking in dilute nitric acid, rinsing with deionized water again and drying;

[0013] Step 1.2, using low-pressure vacuum plasma to treat the surface of the carbon fiber treated in step 1.1 to remove surface organic impurities.

[0014] In step 1.2, the low-pressure vacuum plasma process parameters are: processing time is not less than 3 minutes, vacuum degree is -80Kpa to -95Kpa, and power is 100W to 230W.

[0015] The specific process of step 2 is:

[0016] Step 2.1, adding zinc acetate dihydrate as a zinc source into ethylene glycol methyl ether solvent, stirring, then adding ethanolamine, heating in a water bath, stirring, standing and aging to obtain ZnO sol;

[0017] Step 2.2, immersing the carbon fiber treated in step 1 into ZnO sol, subjecting the entire system to ultrasonic vibration treatment during the immersion process, taking out, spinning and drying, and obtaining carbon fiber coated with a ZnO gel layer.

[0018] In step 2.1, the water bath heating temperature is 50°C to 80°C, the water bath stirring time is 6h to 8h, the static aging time is not less than 24h, the concentration of ZnO sol is 0.1mol / L to 0.3mol / L; the molar ratio of zinc acetate dihydrate to ethanolamine is 1:1;

[0019] In step 2.2, the drying temperature is 80° C. to 140° C., and the drying time is 25 min to 100 min.

[0020] In step 3, the processing time is 3 min to 10 min, the vacuum degree is -80 Kpa to -95 Kpa, and the power is 100 W to 230 W.

[0021] The specific process of step 4 is:

[0022] Step 4.1, using zinc nitrate hexahydrate as a zinc source and hexamethylenetetramine as an alkali source, the zinc source and the alkali source are fully dissolved in deionized water, stirred and ultrasonically vibrated, and after the solution becomes clear, a hydrothermal reaction solution is obtained;

[0023] Step 4.2, putting the ZnO@CF obtained in step 3 into a reactor, and adding the hydrothermal reaction obtained in step 4.1 into the reactor, sealing the reactor and putting it into an oven for hydrothermal reaction;

[0024] Step 4.3, after the reaction is completed, take out the sample, rinse it with deionized water and anhydrous ethanol to wash off the attachments on the surface of the sample, and then dry it to obtain ZnONps@CF.

[0025] In step 4.1, the ultrasonic vibration time is not less than 2 minutes, the concentration of the hydrothermal reaction solution is 0.02 mol / L to 0.06 mol / L; the molar ratio of zinc nitrate hexahydrate to hexamethylenetetramine is 1:1;

[0026] Step 4.2, the temperature of the hydrothermal reaction is 80°C to 180°C, and the hydrothermal reaction time is 12h to 18h;

[0027] Step 4.3, the drying temperature is 80°C to 200°C, and the drying time is 3min to 15min.

[0028] The specific process of step 5 is: put the ZnONps@CF obtained in step 4 into a reactor, and add a low surface energy modifier solution into the reactor to completely immerse the ZnONps@CF, seal it and put it into an oven for reaction, take out the sample after the reaction is completed, and obtain the super oleophilic / super hydrophobic ZnO nano-coated carbon fiber after drying.

[0029] The concentration of the low surface energy modifier solution is 10 g / L to 50 g / L;

[0030] The low surface energy modifier in the low surface energy modifier solution is one of PDMS, HDMS, VTMS, MTMOS, and OTS, and the solvent is anhydrous ethanol;

[0031] The reaction temperature is 90°C to 120°C, and the reaction time is 4h to 12h;

[0032] The drying temperature is 60°C to 80°C, and the drying time is 12h to 14h.

[0033] The beneficial effects of the present invention are:

[0034] (1) The preparation method of the super-oleophilic / super-hydrophobic ZnO-coated carbon fiber oil-water separation membrane of the present invention has a simple preparation process compared with the preparation method of the traditional oil-water separation membrane; secondly, the carbon fiber is low in cost and has good wear resistance and friction resistance, thereby giving the ZnO-coated carbon fiber oil-water separation membrane good mechanical properties; the ZnO coating layer and the carbon fiber substrate both have good corrosion resistance, durability and cycle stability;

[0035] (2) The super-oleophilic / super-hydrophobic ZnO nano-coated carbon fiber prepared by the method of the present invention has good oil-water selectivity and separation flux, and can be applied to oil-water separation in complex acid-base environments. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 1 is the XRD diagram of ZnO@CF prepared by the method of the present invention before and after the hydrothermal reaction;

[0037] Figure 2is a SEM picture of ZnONps@CF prepared by the method of the present invention;

[0038] Figure 3 This is a water antenna diagram of ZnONps@CF prepared by the method of the present invention;

[0039] Figure 4 It is the oil contact angle diagram of the superoleophilic / superhydrophobic OTS-ZnONps@CF prepared by the method of the present invention;

[0040] Figure 5 This is a separation flux diagram of the superoleophilic / superhydrophobic MTMOS-ZnONps@CF prepared by the method of the present invention after regeneration cycle in a mixed system of cyclohexane and water. DETAILED DESCRIPTION

[0041] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.

[0042] The method for preparing the super oleophilic / super hydrophobic ZnO coated carbon fiber oil-water separation membrane of the present invention is specifically implemented according to the following steps:

[0043] Step 1, cleaning the surface of the carbon fiber, and then activating the carbon fiber using low-pressure vacuum plasma technology;

[0044] The specific process is:

[0045] Step 1.1, soak the carbon fiber in a 1% sodium carbonate solution for 1 hour, rinse with deionized water for 5 times, soak in a 15% dilute nitric acid solution for 5 minutes, rinse with deionized water again and dry;

[0046] Step 1.2, treating the surface of the carbon fiber treated in step 1.1 with low-pressure vacuum plasma to remove organic impurities on the surface;

[0047] Among them, the low-pressure vacuum plasma process parameters are: processing time is not less than 3 minutes, vacuum degree is -80Kpa ~ -95Kpa, power is 100W ~ 230W;

[0048] Step 2, preparing carbon fiber coated with ZnO gel layer by sol-gel method;

[0049] The specific process is:

[0050] Step 2.1, adding zinc acetate dihydrate as a zinc source to ethylene glycol methyl ether solvent, stirring, then adding ethanolamine, heating in a water bath at 50° C. to 80° C. and stirring for 6 h to 8 h, and standing and aging for not less than 24 h to obtain a ZnO sol with a concentration of 0.1 mol / L to 0.3 mol / L;

[0051] The molar ratio of zinc acetate dihydrate to ethanolamine is 1:1, and the volume of ethylene glycol methyl ether is 200 ml;

[0052] Step 2.2, immersing the carbon fiber treated in step 1 into ZnO sol, subjecting the entire system to ultrasonic vibration treatment for 5 minutes during the immersion process, taking out and drying, and drying at 80° C. to 140° C. for 25 minutes to 100 minutes to obtain a carbon fiber coated with a ZnO gel layer;

[0053] Step 3, using low-pressure vacuum plasma technology to treat the carbon fiber coated with the ZnO gel layer prepared in step 2 to obtain ZnO@CF (carbon fiber coated with ZnO ceramic);

[0054] Among them, the low-pressure vacuum plasma process parameters are: processing time is 3min~10min, vacuum degree is -80Kpa~-95Kpa, power is 100W~230W;

[0055] Step 4, using a hydrothermal method to continue growing ZnO nanoparticles on ZnO@CF to obtain ZnONps@CF;

[0056] The specific process is:

[0057] Step 4.1, using zinc nitrate hexahydrate as a zinc source and hexamethylenetetramine as an alkali source, the zinc source and the alkali source are fully dissolved in deionized water, stirred and ultrasonically vibrated for not less than 2 minutes, and after the solution becomes clear, a hydrothermal reaction solution with a concentration of 0.02 mol / L to 0.06 mol / L is obtained;

[0058] Wherein, the molar ratio of zinc nitrate hexahydrate to hexamethylenetetramine is 1:1;

[0059] Step 4.2, putting the ZnO@CF obtained in step 3 into a reaction kettle, and adding the hydrothermal reaction solution obtained in step 4.1 into the reaction kettle, sealing it and putting it into an oven at 80° C. to 180° C. for hydrothermal reaction for 12 h to 18 h;

[0060] Step 4.3, after the reaction is completed, take out the sample, rinse it with deionized water and anhydrous ethanol for 3 to 5 times to wash off the surface attachments of the sample, and dry it at 80°C to 200°C for 3min to 15min to obtain ZnONps@CF;

[0061] Step 5, performing low surface energy modification on the ZnONps@CF obtained in step 4 to obtain super oleophilic / super hydrophobic ZnO nano-coated carbon fiber (R-ZnONps@CF, R is the abbreviation of the surface modifier);

[0062] The specific process is as follows: the ZnONps@CF obtained in step 4 is placed in a reactor, and a low surface energy modifier solution with a concentration of 10 g / L to 50 g / L is added to the reactor to completely immerse the ZnONps@CF, and then sealed and placed in an oven at 90°C to 120°C for reaction for 4h to 12h. After the reaction is completed, the sample is taken out and dried at 60°C to 80°C for 12h to 14h to obtain a super oleophilic / super hydrophobic ZnO nano-coated carbon fiber;

[0063] The low surface energy modifier in the low surface energy modifier solution is one of PDMS (polymethylsiloxane), HDMS (hexamethyldisilazane), VTMS (vinyltrimethoxysilane), MTMOS (hexadecyltrimethyloxysilane), and OTS (octadecyltrichlorosilane), and the solvent is anhydrous ethanol;

[0064] Step 6, using a T-shaped bidirectional oil-water separation device, that is, two ports in the same straight line are respectively the oil filter end and the water filter end, specifically, the left side is the oil filter end, which is equipped with R-ZnONps@CF, the right side is the water filter end, which is equipped with ZnONps@CF, and the remaining port is the liquid inlet end, to test the separation flux of the R-ZnONps@CF oil-water separation membrane for the oil phase component; after the separation flux of the oil filter end for the oil phase component in the mixture decreases significantly (note: the standard is a decrease of 5%), the oil-water separation membranes at the oil filter end and the water filter end are taken out and dried, and then the carbon fiber surface is treated with low-pressure vacuum plasma to remove surface pollutants. Repeat step 5 for the regenerated R-ZnONps@CF filter membrane to restore the oil-water separation function.

[0065] Among them, the low-pressure vacuum plasma process parameters are: processing time of at least 3 minutes, vacuum degree of -80Kpa to -95Kpa, power of 100W to 230W;

[0066] The drying temperature is 60°C to 150°C, and the drying time is 40min to 180min.

[0067] The principle of the present invention is: first, a ZnO seed layer is coated on the surface of the carbon fiber by combining a sol-gel technique with a low-pressure vacuum plasma technique, then a hydrothermal method is used to grow ZnO nanoparticles, and finally a molecular self-assembly technique is used to modify the nano ZnO ceramic coating layer with low surface energy, so as to give the carbon fiber super-oleophilic / super-hydrophobic properties and the function of separating the oil phase component from the oil-water mixture. After the oil-water separation operation, the surface of the oil-water separation membrane is easily contaminated and the pore structure is easily blocked, resulting in a decrease in oil-water selectivity and separation flux. The present invention uses a low-pressure vacuum plasma technique to treat the used R-ZnONps@CF oil-water separation membrane, and the pollutants on the surface of the oil-water separation membrane are degraded by the low-pressure vacuum plasma technique, but the ZnO ceramic coating layer is not affected, and then repeated low surface energy modification is repeated to achieve the regeneration of the ZnO-coated carbon fiber oil-water separation membrane material.

[0068] Example 1

[0069] Step 1, cleaning the surface of the carbon fiber, and then activating the carbon fiber using low-pressure vacuum plasma technology;

[0070] The specific process is:

[0071] Step 1.1, soak the carbon fiber in a 1% sodium carbonate solution for 1 hour, rinse with deionized water 5 times, soak in a 15% dilute nitric acid solution for 5 minutes, rinse with deionized water again, and dry for 15 minutes;

[0072] Step 1.2, using low-pressure vacuum plasma (vacuum degree of -80Kpa, power of 100W) to treat the surface of the carbon fiber treated in step 1.1 for no less than 3 minutes to remove surface organic impurities;

[0073] Step 2, preparing carbon fiber coated with ZnO gel layer by sol-gel method;

[0074] The specific process is:

[0075] Step 2.1, adding 4.39 g of zinc acetate dihydrate as a zinc source into 200 ml of ethylene glycol methyl ether solvent, stirring, then adding 1.22 g of ethanolamine, heating in a water bath at 50° C. and stirring for 8 h, and standing and aging for 24 h to obtain a 0.1 mol / L ZnO sol;

[0076] Step 2.2, immersing the carbon fiber treated in step 1 into ZnO sol, subjecting the entire system to ultrasonic vibration treatment for 5 minutes during the immersion process, taking out, drying, and drying at 80° C. for 100 minutes to obtain a carbon fiber coated with a ZnO gel layer;

[0077] Step 3, using low-pressure vacuum plasma technology (vacuum degree of -80Kpa, power of 100W) to treat the carbon fiber coated with the ZnO gel layer prepared in step 2 for 3 minutes, converting the ZnO gel layer coated on the carbon fiber into a ZnO ceramic layer to obtain ZnO@CF (carbon fiber coated with ZnO ceramic);

[0078] Step 4, using a hydrothermal method to continue growing ZnO nanoparticles on ZnO@CF to obtain ZnONps@CF;

[0079] The specific process is:

[0080] Step 4.1, using 0.298 g of zinc nitrate hexahydrate as a zinc source and 0.140 g of hexamethylenetetramine as an alkali source, the zinc source and the alkali source are fully dissolved in 50 mL of deionized water, stirred and ultrasonically vibrated for 2 min, and after the solution becomes clear, a hydrothermal reaction solution with a concentration of 0.02 mol / L is obtained;

[0081] Step 4.2, putting the ZnO@CF obtained in step 3 into a reaction kettle, and adding the hydrothermal reaction solution obtained in step 4.1 into the reaction kettle, sealing it and putting it into an oven at 80° C. for hydrothermal reaction for 18 hours;

[0082] Step 4.3, after the reaction is completed, take out the sample, rinse it with deionized water and anhydrous ethanol three times to wash off the surface attachments of the sample, and dry it at 80 ° C for 15 min to obtain ZnONps@CF;

[0083] Step 5, performing low surface energy modification on the ZnONps@CF obtained in step 4 to obtain super oleophilic / super hydrophobic PDMS-ZnONps@CF;

[0084] The specific process is as follows: the ZnONps@CF obtained in step 4 is placed in a reactor, and a low surface energy modifier solution with a concentration of 10 g / L is added to the reactor to completely immerse the ZnONps@CF, and then sealed and placed in a 90°C oven for reaction for 6 hours. After the reaction is completed, the sample is taken out and dried at 60°C for 14 hours to obtain a super-oleophilic / super-hydrophobic ZnO nano-coated carbon fiber;

[0085] The low surface energy modifier in the low surface energy modifier solution is PDMS (polymethylsiloxane), and the solvent is anhydrous ethanol;

[0086] Step 6: A T-shaped bidirectional oil-water separation device is used, that is, two ports in the same straight line are respectively the oil filter end and the water filter end. Specifically, the left side is the oil filter end, which is provided with PDMS-ZnONps@CF, and the right side is the water filter end, which is provided with ZnONps@CF. The remaining port is the liquid inlet end. The separation flux of petroleum ether in the petroleum ether-water mixture of PDMS-ZnONps@CF is tested; the initial flux of PDMS-ZnONps@CF for petroleum ether is 86332.59 L / m 2 ·h, after 48h of continuous oil-water separation, the separation flux dropped to 82051.69L / m 2 h, take out the PDMS-ZnONps@CF and ZnONps@CF filter membranes, dry them at 60°C for 180 min, treat the PDMS-ZnONps@CF and ZnONps@CF filter membranes with low-pressure vacuum plasma (vacuum degree of -80 Kpa, power of 100 W) for 7 min to remove surface pollutants, repeat step 5 for the regenerated PDMS-ZnONps@CF filter membrane to restore the oil-water separation function.

[0087] The water contact angle of superoleophilic / superhydrophobic PDMS-ZnONps@CF is 157.2°, and the oil contact angle is 0°. The XRD characterization results of ZnO@CF and ZnONps@CF are shown in Figure 2. Figure 1 As shown, ZnO is hexagonal, and the diffraction peak of ZnO is significantly enhanced after hydrothermal treatment.

[0088] Example 2

[0089] Step 1, cleaning the surface of the carbon fiber, and then activating the carbon fiber using low-pressure vacuum plasma technology;

[0090] The specific process is:

[0091] Step 1.1, soak the carbon fiber in a 1% sodium carbonate solution for 1 hour, rinse with deionized water 5 times, soak in a 15% dilute nitric acid solution for 5 minutes, rinse with deionized water again, and dry for 18 minutes;

[0092] Step 1.2, using low-pressure vacuum plasma (vacuum degree of -85Kpa, power of 150W) to treat the surface of the carbon fiber treated in step 1.1 for 4 minutes to remove surface organic impurities;

[0093] Step 2, preparing carbon fiber coated with ZnO gel layer by sol-gel method;

[0094] The specific process is:

[0095] Step 2.1, adding 6.59 g of zinc acetate dihydrate as a zinc source into 200 ml of ethylene glycol methyl ether solvent, stirring, then adding 1.63 g of ethanolamine, heating in a water bath at 70° C. and stirring for 7 h, and standing and aging for 24 h to obtain a ZnO sol with a concentration of 0.15 mol / L;

[0096] Step 2.2, immersing the carbon fiber treated in step 1 into ZnO sol, subjecting the entire system to ultrasonic vibration treatment for 5 minutes during the immersion process, taking out, drying, and drying at 90° C. for 60 minutes to obtain a carbon fiber coated with a ZnO gel layer;

[0097] Step 3, using low-pressure vacuum plasma technology (vacuum degree of -85Kpa, power of 150W) to treat the carbon fiber coated with the ZnO gel layer prepared in step 2 for 5 minutes, converting the ZnO gel layer coated on the carbon fiber into a ZnO ceramic layer to obtain ZnO@CF (carbon fiber coated with ZnO ceramic);

[0098] Step 4, using a hydrothermal method to continue growing ZnO nanoparticles on ZnO@CF to obtain ZnONps@CF;

[0099] The specific process is:

[0100] Step 4.1, using 0.447 g of zinc nitrate hexahydrate as a zinc source and 0.210 g of hexamethylenetetramine as an alkali source, the zinc source and the alkali source are fully dissolved in 50 mL of deionized water, stirred and ultrasonically vibrated for 2 min, and after the solution becomes clear, a hydrothermal reaction solution with a concentration of 0.03 mol / L is obtained;

[0101] Step 4.2, putting the ZnO@CF obtained in step 3 into a reaction kettle, and adding the hydrothermal reaction solution obtained in step 4.1 into the reaction kettle, sealing the kettle and placing it in an oven at 100° C. for hydrothermal reaction for 17 hours;

[0102] Step 4.3, after the reaction is completed, take out the sample, rinse it with deionized water and anhydrous ethanol three times to wash off the surface attachments of the sample, and dry it at 85 ° C for 9 minutes to obtain ZnONps@CF;

[0103] Step 5, performing low surface energy modification on the ZnONps@CF obtained in step 4 to obtain HMDS-ZnONps@CF with super oleophilic / super hydrophobic properties;

[0104] The specific process is as follows: the ZnONps@CF obtained in step 4 is placed in a reactor, and a low surface energy modifier solution with a concentration of 20 g / L is added to the reactor to completely immerse the ZnONps@CF, and then sealed and placed in an oven at 100°C for reaction for 5 hours. After the reaction is completed, the sample is taken out and dried at 80°C for 12 hours to obtain a super-oleophilic / super-hydrophobic ZnO nano-coated carbon fiber;

[0105] Wherein, the low surface energy modifier in the low surface energy modifier solution is HDMS, and the solvent is anhydrous ethanol;

[0106] Step 6: A T-shaped bidirectional oil-water separation device is used, i.e., two ports in the same straight line are respectively an oil filter end and a water filter end. Specifically, the left side is the oil filter end, which is provided with HMDS-ZnONps@CF, and the right side is the water filter end, which is provided with ZnONps@CF. The separation flux of HMDS-ZnONps@CF for chlorobenzene in a chlorobenzene-water mixture is tested; the initial flux of HMDS-ZnONps@CF for chlorobenzene is 67282.68 L / m 2 ·h, after 50h of continuous oil-water separation, the separation flux dropped to 63502.14L / m 2 h, take out the HMDS-ZnONps@CF and ZnONps@CF filter membranes, dry them at 80°C for 120 min, treat the HMDS-ZnONps@CF and ZnONps@CF filter membranes with low-pressure vacuum plasma (vacuum degree of -85 Kpa, power of 150 W) for 7 min to remove surface pollutants, repeat step 5 for the regenerated HMDS-ZnONps@CF filter membrane to restore the oil-water separation function.

[0107] The water contact angle of the superoleophilic / superhydrophobic modified HMDS-ZnONps@CF was 159.3° and the oil contact angle was 0°. The surface morphology of ZnONps@CF is shown in Figure 2. Figure 2 As shown, the coating layer has a dense structure and the ZnO particles are evenly distributed on the surface of the carbon fibers.

[0108] Example 3

[0109] Step 1, cleaning the surface of the carbon fiber, and then activating the carbon fiber using low-pressure vacuum plasma technology;

[0110] The specific process is:

[0111] Step 1.1, soak the carbon fiber in a 1% sodium carbonate solution for 1 hour, rinse with deionized water 5 times, soak in a 15% dilute nitric acid solution for 5 minutes, rinse with deionized water again, and dry for 15 minutes;

[0112] Step 1.2, using low-pressure vacuum plasma (vacuum degree of -90Kpa, power of 200W) to treat the surface of the carbon fiber treated in step 1.1 for 6 minutes to remove surface organic impurities;

[0113] Step 2, preparing carbon fiber coated with ZnO gel layer by sol-gel method;

[0114] The specific process is:

[0115] Step 2.1, adding 8.78 g of zinc acetate dihydrate as a zinc source into 200 ml of ethylene glycol methyl ether solvent, stirring, then adding 2.44 g of ethanolamine, heating in a water bath at 80° C. and stirring for 6 h, and standing and aging for 24 h to obtain a ZnO sol with a concentration of 0.2 mol / L;

[0116] Step 2.2, immersing the carbon fiber treated in step 1 into ZnO sol, subjecting the entire system to ultrasonic vibration treatment for 5 minutes during the immersion process, taking out, drying, and drying at 100° C. for 40 minutes to obtain a carbon fiber coated with a ZnO gel layer;

[0117] Step 3, using low-pressure vacuum plasma technology (vacuum degree of -90Kpa, power of 200W) to treat the carbon fiber coated with the ZnO gel layer prepared in step 2 for 8 minutes, converting the ZnO gel layer coated on the carbon fiber into a ZnO ceramic layer to obtain ZnO@CF (carbon fiber coated with ZnO ceramic);

[0118] Step 4, using a hydrothermal method to continue growing ZnO nanoparticles on ZnO@CF to obtain ZnONps@CF;

[0119] The specific process is:

[0120] Step 4.1, using 0.596 g of zinc nitrate hexahydrate as a zinc source and 0.280 g of hexamethylenetetramine as an alkali source, the zinc source and the alkali source are fully dissolved in 50 mL of deionized water, stirred and ultrasonically vibrated for 2 min, and after the solution becomes clear, a hydrothermal reaction solution with a concentration of 0.04 mol / L is obtained;

[0121] Step 4.2, putting the ZnO@CF obtained in step 3 into a reaction kettle, and adding the hydrothermal reaction solution obtained in step 4.1 into the reaction kettle, sealing it and putting it into an oven at 120° C. for hydrothermal reaction for 16 hours;

[0122] Step 4.3, after the reaction is completed, take out the sample, rinse it with deionized water and anhydrous ethanol for 4 times to wash off the surface attachment of the sample, and dry it at 90 ° C for 10 min to obtain ZnONps@CF;

[0123] Step 5, performing low surface energy modification on the ZnONps@CF obtained in step 4 to obtain super oleophilic / super hydrophobic VTMS-ZnONps@CF;

[0124] The specific process is as follows: the ZnONps@CF obtained in step 4 is placed in a reactor, and a low surface energy modifier solution with a concentration of 30 g / L is added to the reactor to completely immerse the ZnONps@CF, and then sealed and placed in an oven at 120°C for reaction for 12 hours. After the reaction is completed, the sample is taken out and dried at 80°C for 12 hours to obtain a super-oleophilic / super-hydrophobic ZnO nano-coated carbon fiber;

[0125] The low surface energy modifier in the low surface energy modifier solution is VTMS, and the solvent is anhydrous ethanol;

[0126] Step 6: A T-shaped bidirectional oil-water separation device is used, that is, two ports in the same straight line are respectively the oil filter end and the water filter end. Specifically, the left side is the oil filter end, which is provided with VTMS-ZnONps@CF, and the right side is the water filter end, which is provided with ZnONps@CF. The remaining port is the liquid inlet end. The separation flux of VTMS-ZnONps@CF for 92# gasoline in a 92# gasoline-water mixture is tested; the initial flux of VTMS-ZnONps@CF for 92# gasoline is 61375.63L / m 2 ·h. After 49h of continuous operation, the separation flux dropped to 58354.40L / m 2 h, take out the VTMS-ZnONps@CF and ZnONps@CF filter membranes, dry them at 120°C for 60 min, treat the VTMS-ZnONps@CF and ZnONps@CF filter membranes with low-pressure vacuum plasma (vacuum degree of -90 Kpa, power of 200 W) for 5 min to remove surface pollutants, repeat step 5 for the regenerated VTMS-ZnONps@CF filter membrane to restore the oil-water separation function.

[0127] The water contact angle of the obtained superoleophilic / superhydrophobic VTMS-ZnONps@CF is 161.2°, and the oil contact angle is 0°; the water contact angle of ZnONps@CF is Figure 3 As shown, the water droplet completely wets the carbon fiber surface after contacting it, indicating that the ZnONps@CF prepared at this concentration is hydrophilic.

[0128] Example 4

[0129] Step 1, cleaning the surface of the carbon fiber, and then activating the carbon fiber using low-pressure vacuum plasma technology;

[0130] The specific process is:

[0131] Step 1.1, soak the carbon fiber in a 1% sodium carbonate solution for 1 hour, rinse with deionized water 5 times, soak in a 15% dilute nitric acid solution for 5 minutes, rinse with deionized water again, and dry for 18 minutes;

[0132] Step 1.2, using low-pressure vacuum plasma (vacuum degree of -92Kpa, power of 210W) to treat the surface of the carbon fiber treated in step 1.1 for 7 minutes to remove surface organic impurities;

[0133] Step 2, preparing carbon fiber coated with ZnO gel layer by sol-gel method;

[0134] The specific process is:

[0135] Step 2.1, adding 10.97 g of zinc acetate dihydrate as a zinc source into 200 ml of ethylene glycol methyl ether solvent, stirring, then adding 3.05 g of ethanolamine, heating in a water bath at 50° C. and stirring for 8 h, and standing and aging for 24 h to obtain a ZnO sol with a concentration of 0.25 mol / L;

[0136] Step 2.2, immersing the carbon fiber treated in step 1 into ZnO sol, subjecting the entire system to ultrasonic vibration treatment for 5 minutes during the immersion process, taking out, drying, and drying at 120° C. for 30 minutes to obtain a carbon fiber coated with a ZnO gel layer;

[0137] Step 3, using low-pressure vacuum plasma technology (vacuum degree of -92Kpa, power of 210W) to treat the carbon fiber coated with the ZnO gel layer prepared in step 2 for 10 minutes, converting the ZnO gel layer coated on the carbon fiber into a ZnO ceramic layer to obtain ZnO@CF (carbon fiber coated with ZnO ceramic);

[0138] Step 4, using a hydrothermal method to continue growing ZnO nanoparticles on ZnO@CF to obtain ZnONps@CF;

[0139] The specific process is:

[0140] Step 4.1, using 0.745 g of zinc nitrate hexahydrate as a zinc source and 0.35 g of hexamethylenetetramine as an alkali source, the zinc source and the alkali source are fully dissolved in 50 mL of deionized water, stirred and ultrasonically vibrated for 2 min, and after the solution becomes clear, a hydrothermal reaction solution with a concentration of 0.05 mol / L is obtained;

[0141] Step 4.2, the ZnO@CF obtained in step 3 is placed in a reaction kettle, and the hydrothermal reaction solution obtained in step 4.1 is added to the reaction kettle, and the reaction kettle is sealed and placed in an oven at 150° C. for hydrothermal reaction for 14 hours;

[0142] Step 4.3, after the reaction is completed, take out the sample, rinse it with deionized water and anhydrous ethanol for 5 times to wash off the surface attachments of the sample, and dry it at 100 ° C for 5 min to obtain ZnONps@CF;

[0143] Step 5, performing low surface energy modification on the ZnONps@CF obtained in step 4 to obtain super oleophilic / super hydrophobic OTS-ZnONps@CF;

[0144] The specific process is as follows: the ZnONps@CF obtained in step 4 is placed in a reactor, and a low surface energy modifier solution with a concentration of 40 g / L is added to the reactor to completely immerse the ZnONps@CF, and then sealed and placed in an oven at 120°C for reaction for 4 hours. After the reaction is completed, the sample is taken out and dried at 80°C for 12 hours to obtain a super-oleophilic / super-hydrophobic ZnO nano-coated carbon fiber;

[0145] Wherein, the low surface energy modifier in the low surface energy modifier solution is OTS, and the solvent is anhydrous ethanol;

[0146] Step 6: A T-shaped bidirectional oil-water separation device is used, that is, two ports in the same straight line are respectively the oil filter end and the water filter end. Specifically, the left side is the oil filter end, which is equipped with OTS-ZnONps@CF, and the right side is the water filter end, which is equipped with ZnONps@CF. The remaining port is the liquid inlet end. The separation flux of OTS-ZnONps@CF for edible oil in the edible oil-water mixture is tested; the initial flux of OTS-ZnONps@CF for edible oil is 61243.41 L / m 2 ·h, after 48 hours of continuous work, it dropped to 57843.24L / m 2 h, take out the OTS-ZnONps@CF and ZnONps@CF filter membranes, dry them at 150°C for 40 min, and treat the OTS-ZnONps@CF and ZnONps@CF filter membranes with high-pressure vacuum plasma (vacuum degree of -92Kpa, power of 210W) for 4 min to remove surface pollutants. Repeat step 5 for the regenerated OTS-ZnONps@CF filter membrane to restore the oil-water separation function.

[0147] like Figure 4 As shown, the water contact angle of the obtained superoleophilic / superhydrophobic OTS-ZnONps@CF is 172°, and the oil contact angle is 0°, which exhibits superhydrophobicity / superoleophilicity.

[0148] Example 5

[0149] Step 1, cleaning the surface of the carbon fiber, and then activating the carbon fiber using low-pressure vacuum plasma technology;

[0150] The specific process is:

[0151] Step 1.1, soak the carbon fiber in a 1% sodium carbonate solution for 1 hour, rinse with deionized water 5 times, soak in a 15% dilute nitric acid solution for 5 minutes, rinse with deionized water again, and dry for 20 minutes;

[0152] Step 1.2, using low-pressure vacuum plasma (vacuum degree of -95Kpa, power of 230W) to treat the surface of the carbon fiber treated in step 1.1 for 9 minutes to remove surface organic impurities;

[0153] Step 2, preparing carbon fiber coated with ZnO gel layer by sol-gel method;

[0154] The specific process is:

[0155] Step 2.1, adding 13.17 g of zinc acetate dihydrate as a zinc source into 200 ml of ethylene glycol methyl ether solvent, stirring, then adding 3.66 g of ethanolamine, heating in a water bath at 50° C. and stirring for 8 h, and standing and aging for 24 h to obtain a ZnO sol with a concentration of 0.3 mol / L;

[0156] Step 2.2, immersing the carbon fiber treated in step 1 into ZnO sol, subjecting the entire system to ultrasonic vibration treatment for 5 minutes during the immersion process, taking out, drying, and drying at 140° C. for 25 minutes to obtain a carbon fiber coated with a ZnO gel layer;

[0157] Step 3, using low-pressure vacuum plasma technology (vacuum degree of -95Kpa, power of 230W) to treat the carbon fiber coated with the ZnO gel layer prepared in step 2 for 4 minutes, converting the ZnO gel layer coated on the carbon fiber into a ZnO ceramic layer to obtain ZnO@CF (carbon fiber coated with ZnO ceramic);

[0158] Step 4, using a hydrothermal method to continue growing ZnO nanoparticles on ZnO@CF to obtain ZnONps@CF;

[0159] The specific process is:

[0160] Step 4.1, using 0.894 g of zinc nitrate hexahydrate as a zinc source and 0.42 g of hexamethylenetetramine as an alkali source, the zinc source and the alkali source are fully dissolved in 50 mL of deionized water, stirred and ultrasonically vibrated for 2 min, and after the solution becomes clear, a hydrothermal reaction solution with a concentration of 0.06 mol / L is obtained;

[0161] Step 4.2, putting the ZnO@CF obtained in step 3 into a reaction kettle, and adding the hydrothermal reaction solution obtained in step 4.1 into the reaction kettle, sealing it and putting it into an oven at 180° C. for hydrothermal reaction for 12 hours;

[0162] Step 4.3, after the reaction is completed, take out the sample, rinse it with deionized water and anhydrous ethanol for 5 times to wash off the surface attachments of the sample, and dry it at 200 ° C for 3 min to obtain ZnONps@CF;

[0163] Step 5, performing low surface energy modification on the ZnONps@CF obtained in step 4 to obtain MTMOS-ZnONps@CF with super oleophilic / super hydrophobic properties;

[0164] The specific process is as follows: the ZnONps@CF obtained in step 4 is placed in a reactor, and a low surface energy modifier solution with a concentration of 50 g / L is added to the reactor to completely immerse the ZnONps@CF, and then sealed and placed in an oven at 120°C for reaction for 4 hours. After the reaction is completed, the sample is taken out and dried at 80°C for 12 hours to obtain a super-oleophilic / super-hydrophobic ZnO nano-coated carbon fiber;

[0165] The low surface energy modifier in the low surface energy modifier solution is MTMOS, and the solvent is anhydrous ethanol;

[0166] Step 6: A T-shaped bidirectional oil-water separation device is used, that is, two ports in the same straight line are respectively the oil filter end and the water filter end. Specifically, the left side is the oil filter end, which is provided with MTMOS-ZnONps@CF, and the right side is the water filter end, which is provided with ZnONps@CF. The remaining port is the liquid inlet end. The separation flux of MTMOS-ZnONps@CF for cyclohexane in a cyclohexane-water mixture is tested; the initial flux of MTMOS-ZnONps@CF for cyclohexane is 54080.04 L / m 2 ·h, after 48h of continuous oil-water separation, it dropped to 51374.94L / m 2 h, take out the MTMOS-ZnONps@CF and ZnONps@CF filter membranes, dry them at 120°C for 60 min, and treat the MTMOS-ZnONps@CF and ZnONps@CF filter membranes with low-pressure vacuum plasma (vacuum degree of -95Kpa, power of 230W) for 5 min to remove surface pollutants. Repeat step 5 for the regenerated MTMOS-ZnONps@CF filter membrane to restore the oil-water separation function. Figure 5 As shown in Figure 2, after 5 regeneration cycles, the initial separation flux of MTMOS-ZnONps@CF filtration membrane for cyclohexane is still 53000 L / m 2 ·h or more, showing excellent regeneration and recycling performance.

[0167] The obtained superoleophilic / superhydrophobic MTMOS~ZnONps@CF has a water contact angle of 170.45° and an oil contact angle of 0°, showing superhydrophobic / superoleophilic properties.

Claims

1. A method for preparing a super oleophilic / super hydrophobic ZnO coated carbon fiber oil-water separation membrane, characterized in that: Follow the steps below to implement it: Step 1, cleaning the surface of the carbon fiber, and then activating the carbon fiber using low-pressure vacuum plasma technology; Step 2, preparing carbon fiber coated with ZnO gel layer by sol-gel method; Step 3, using low-pressure vacuum plasma technology to treat the carbon fiber coated with the ZnO gel layer prepared in step 2 to obtain ZnO@CF; Step 4, using a hydrothermal method to continue growing ZnO nanoparticles on ZnO@CF to obtain ZnONps@CF; Step 5, performing low surface energy modification on the ZnONps@CF obtained in step 4 to obtain super oleophilic / super hydrophobic ZnO nano-coated carbon fibers.

2. The method for preparing the super oleophilic / super hydrophobic ZnO coated carbon fiber oil-water separation membrane according to claim 1, characterized in that: The specific process of step 1 is: Step 1.1, soaking the carbon fiber in sodium carbonate solution, rinsing with deionized water, soaking in dilute nitric acid, rinsing with deionized water again and drying; Step 1.2, using low-pressure vacuum plasma to treat the surface of the carbon fiber treated in step 1.1 to remove surface organic impurities.

3. The method for preparing the super oleophilic / super hydrophobic ZnO coated carbon fiber oil-water separation membrane according to claim 1, characterized in that: In step 1.2, the low-pressure vacuum plasma process parameters are: processing time is not less than 3 minutes, vacuum degree is -80Kpa to -95Kpa, and power is 100W to 230W.

4. The method for preparing the super oleophilic / super hydrophobic ZnO coated carbon fiber oil-water separation membrane according to claim 1, characterized in that: The specific process of step 2 is: Step 2.1, adding zinc acetate dihydrate as a zinc source into ethylene glycol methyl ether solvent, stirring, then adding ethanolamine, heating in a water bath, stirring, standing and aging to obtain ZnO sol; Step 2.2, immersing the carbon fiber treated in step 1 into ZnO sol, subjecting the entire system to ultrasonic vibration treatment during the immersion process, taking out, spinning and drying, and obtaining carbon fiber coated with a ZnO gel layer.

5. The method for preparing the super oleophilic / super hydrophobic ZnO coated carbon fiber oil-water separation membrane according to claim 4, characterized in that: In step 2.1, the water bath heating temperature is 50°C to 80°C, the water bath stirring time is 6h to 8h, the static aging time is not less than 24h, the concentration of ZnO sol is 0.1mol / L to 0.3mol / L; the molar ratio of zinc acetate dihydrate to ethanolamine is 1:1; In step 2.2, the drying temperature is 80° C. to 140° C., and the drying time is 25 min to 100 min.

6. The method for preparing the super oleophilic / super hydrophobic ZnO coated carbon fiber oil-water separation membrane according to claim 1, characterized in that: In step 3, the processing time of the low-pressure plasma is 3 minutes to 10 minutes, the vacuum degree is -80Kpa to -95Kpa, and the power is 100W to 230W.

7. The method for preparing the super oleophilic / super hydrophobic ZnO coated carbon fiber oil-water separation membrane according to claim 1, characterized in that: The specific process of step 4 is: Step 4.1, using zinc nitrate hexahydrate as a zinc source and hexamethylenetetramine as an alkali source, the zinc source and the alkali source are fully dissolved in deionized water, stirred and ultrasonically vibrated, and after the solution becomes clear, a hydrothermal reaction solution is obtained; Step 4.2, putting the ZnO@CF obtained in step 3 into a reactor, and adding the hydrothermal reaction obtained in step 4.1 into the reactor, sealing the reactor and putting it into an oven for hydrothermal reaction; Step 4.3, after the reaction is completed, take out the sample, rinse it with deionized water and anhydrous ethanol to wash off the attachments on the surface of the sample, and then dry it to obtain ZnONps@CF.

8. The method for preparing the super oleophilic / super hydrophobic ZnO coated carbon fiber oil-water separation membrane according to claim 7, characterized in that: In step 4.1, the ultrasonic vibration time is not less than 2 minutes, the concentration of the hydrothermal reaction solution is 0.02 mol / L to 0.06 mol / L; the molar ratio of zinc nitrate hexahydrate to hexamethylenetetramine is 1:1; Step 4.2, the temperature of the hydrothermal reaction is 80°C to 180°C, and the hydrothermal reaction time is 12h to 18h; Step 4.3, the drying temperature is 80°C to 200°C, and the drying time is 3min to 15min.

9. The method for preparing the super oleophilic / super hydrophobic ZnO coated carbon fiber oil-water separation membrane according to claim 1, characterized in that: The specific process of step 5 is: put the ZnONps@CF obtained in step 4 into a reactor, and add a low surface energy modifier solution into the reactor to completely immerse the ZnONps@CF, seal it and put it into an oven for reaction, take out the sample after the reaction is completed, and obtain the super oleophilic / super hydrophobic ZnO nano-coated carbon fiber after drying.

10. The method for preparing the super oleophilic / super hydrophobic ZnO coated carbon fiber oil-water separation membrane according to claim 9, characterized in that: The concentration of the low surface energy modifier solution is 10 g / L to 50 g / L; The low surface energy modifier in the low surface energy modifier solution is one of PDMS, HDMS, VTMS, MTMOS, and OTS, and the solvent is anhydrous ethanol; The reaction temperature is 90°C to 120°C, and the reaction time is 4h to 12h; the drying temperature is 60°C to 80°C, and the drying time is 12h to 14h.

Citation Information

Cited By

  • Super-hydrophobic super-oleophylic renewable oil-water separation material as well as preparation method and application thereof

    CN121513650A

  • Superhydrophobic superoleophilic renewable oil-water separation material, and preparation method and application thereof

    CN121513650B