Method for degrading bisphenol A by using lanthanum manganate catalyst rich in oxygen vacancies

By adjusting the oxygen vacancies concentration of the lanthanum manganate catalyst, using heat treatment of lanthanum manganate and sodium borohydride, combined with monosulfate reaction, the problem of high cost of oxygen vacancies catalysts and unclear relationship between oxygen vacancies concentration in the prior art is solved. Rapid degradation of parabens A was achieved.

CN119034721APending Publication Date: 2024-11-29CHINA JILIANG UNIV
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411198305.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

In the prior art, when developing metal oxide catalysts with oxygen vacancies, the raw material cost is high, the preparation method is complex, and the relationship between oxygen vacancies and catalytic activity has not been systematically discussed, making it difficult to effectively remove bisphenol A in water.

Method used

By adjusting the thermal modification temperature, thermal modification time and the ratio of lanthanum manganate to sodium borohydride substances, adjusting the oxygen vacancy concentration, and using the oxygen vacancy-rich lanthanum manganate catalyst to react with permonosulfate to improve the catalyst The redox capacity and charge transfer performance achieve rapid degradation of bisphenol A.

Benefits of technology

Effectively remove bisphenol A from water in a short period of time, avoiding interference from doping other metal elements, maintaining the stability of the crystal structure of the catalyst, and achieving complete degradation of 10mg/L bisphenol A.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119034721A_ABST
    Figure CN119034721A_ABST
Patent Text Reader

Abstract

The invention discloses a method for degrading bisphenol A by activating peroxymonosulfate by using a lanthanum manganate catalyst rich in oxygen vacancies, which comprises the following steps: adding the lanthanum manganate catalyst rich in oxygen vacancies into wastewater containing bisphenol A, adding a peroxymonosulfate oxidant after adsorption and desorption are balanced, and carrying out a degradation reaction of bisphenol A; the preparation method of the oxygen vacancy-rich lanthanum manganate catalyst comprises the following steps: mixing nano lanthanum manganate and sodium borohydride according to a molar ratio of 1: (1-3.5), grinding, carrying out heat treatment in an inert atmosphere at 350-425 DEG C for 40-140 minutes, and cleaning and drying the obtained product to obtain the oxygen vacancy-rich lanthanum manganate catalyst. The method can be used for removing bisphenol A in the water body in a short time.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of environmental remediation, and in particular to a method for degrading bisphenol A by utilizing a lanthanum manganate catalyst rich in oxygen vacancies. Background Art

[0002] Bisphenol A (BPA for short) is 4,4'-dihydroxydiphenylpropane, which is widely used in the manufacture of polycarbonate plastics and personal care products such as shower gel and facial cleanser. BPA is an endocrine disruptor and has potential harm to human health. BPA enters the water, soil, atmosphere and other environments, and accumulates in the human body through the food chain, affecting human health. Among them, BPA is most harmful to infants and young children. A small amount of BPA can lead to endocrine system disorders, cancer, precocious puberty, and metabolic disorder obesity. BPA is highly stable and poorly biodegradable, and can persist in the environment for a long time. Therefore, more effective technologies than traditional treatment methods are needed to remove BPA from sewage.

[0003] At present, the main technologies for degrading BPA include adsorption, photocatalysis and advanced oxidation. The advanced oxidation process based on peroxymonosulfate activation is one of the ideal solutions for eliminating phenolic pollutants in water. In recent years, the role of oxygen vacancies in heterogeneous activation of peroxymonosulfate has attracted more and more attention. For transition metal oxide-based heterogeneous catalytic materials that activate peroxymonosulfate, defect engineering, whether introducing bulk defect structures or surface defect structures, is considered to be an effective strategy for regulating the electronic properties of catalytic materials and generating new active centers. In addition to transition metal cation sites, the defect structure of oxygen atoms (oxygen vacancies) is considered to be another important site for this type of material. Because oxygen vacancies can regulate the local charge distribution of metal atoms and accelerate the redox cycle of high-valent metal sites, the introduction of oxygen vacancies can improve the catalytic performance of metal oxide-activated peroxymonosulfate.

[0004] Wang et al. from the State Key Laboratory of Petroleum Pollution Control, China University of Petroleum (Beijing) synthesized a series of shape-controllable La 0.5 Ba 0.5 Co x Mn x O 3-δ As a persulfate activator to generate reactive oxygen for water purification, due to the presence of abundant oxygen vacancies and low-valent Co 2+ Ion, cubic La 0.5 Ba 0.5 Co 0.8 Mn 0.2 O 3-δ The catalytic activity is much higher than that of octahedral La 0.5 Ba 0.5 Co 0.2 Mn0.8 O 3-δ , experimentally and theoretically revealed that the increase in the Co / Mn ratio would produce abundant oxygen vacancies as active sites for binding and activation with peroxymonosulfate molecules (Wang, Chi, Chen, Su, Liu and Duan Facet-and defect-dependent activity of perovskites in catalytic evolution of sulfate radicals. Appl. Catal. B 272 (2020) 118972.).

[0005] However, there are still some shortcomings in the development of metal oxide catalysts containing oxygen vacancies: on the one hand, the construction of oxygen vacancies in metal oxide catalytic materials usually adopts the method of doping with other metal elements, which has high raw material costs and complex preparation methods; on the other hand, the work reported so far has mostly focused on the role of oxygen vacancies in the activation of peroxymonosulfate, but rarely systematically discussed the relationship between oxygen vacancy concentration and its promotion of catalytic activity. There are few reports on controlling the oxygen vacancy concentration of perovskite metal oxides and adjusting their catalytic performance for activating peroxymonosulfate through post-treatment methods based on defect engineering. Therefore, it is urgent to develop a controllable oxygen vacancy concentration modification technology for perovskite metal oxides for the development of catalytic materials for efficient activation of peroxymonosulfate for oxidative degradation of bisphenol A. Summary of the invention

[0006] In view of the above technical problems and the shortcomings in the art, the present invention provides a method for degrading bisphenol A by activating peroxymonosulfate using a lanthanum manganate catalyst rich in oxygen vacancies, wherein oxygen vacancies are adjusted by adjusting the thermal modification temperature, the thermal modification time and the molar ratio of nano-lanthanum manganate to sodium borohydride, and oxygen atoms are removed in situ to change the electronic structure of the catalyst surface, so that the catalyst has stronger redox ability and better charge transfer performance, thereby accelerating the peroxymonosulfate activation process, and further removing bisphenol A in water in a short time.

[0007] A method for degrading bisphenol A using a lanthanum manganate catalyst rich in oxygen vacancies comprises: adding the lanthanum manganate catalyst rich in oxygen vacancies into wastewater containing bisphenol A, adding a peroxymonosulfate oxidant after adsorption-desorption equilibrium, and performing a degradation reaction of bisphenol A.

[0008] The preparation method of the lanthanum manganate catalyst rich in oxygen vacancies comprises: mixing and grinding nano-lanthanum manganate and sodium borohydride in a certain molar ratio and then heat treating at high temperature in an inert atmosphere. The molar ratio of nano-lanthanum manganate to sodium borohydride is 1:1-3.5, preferably 1:3. The preferred reason is that too little sodium borohydride will form insufficient oxygen vacancy structure, and too much sodium borohydride will cause deep reduction of lanthanum manganate, lose too many oxygen atoms and collapse the lattice, thereby destroying the original catalytic interface. The heat treatment temperature is 350-425°C, preferably 400°C, and the preferred reason is that the pyrolysis temperature affects the degree of reaction. If the temperature is too low, sodium borohydride decomposes too slowly, and oxygen vacancies are not easy to form. If the temperature is too high, it will cause lattice distortion of lanthanum manganate. The heat treatment time is 40-140min, preferably 120min. The preferred reason is that the heat treatment time affects the degree of surface reduction of lanthanum manganate, that is, the concentration of oxygen vacancies. The inert atmosphere refers to a gas atmosphere that does not participate in the reaction, such as a rare gas atmosphere such as a helium atmosphere or an argon atmosphere. The obtained product is washed and dried to obtain the lanthanum manganate catalyst rich in oxygen vacancies.

[0009] The method for degrading bisphenol A using a lanthanum manganate catalyst rich in oxygen vacancies comprises a dosage ratio of the lanthanum manganate catalyst rich in oxygen vacancies to the bisphenol A in the bisphenol A-containing wastewater of 0.01 to 0.03 g:1 mg, for example, 0.02 g:1 mg.

[0010] In the method for degrading bisphenol A using a lanthanum manganate catalyst rich in oxygen vacancies, the initial pH of the wastewater containing bisphenol A is 5 to 7, such as 6.

[0011] In the method for degrading bisphenol A using a lanthanum manganate catalyst rich in oxygen vacancies, the peroxymonosulfate oxidant may be a potassium hydrogen peroxymonosulfate composite salt.

[0012] In the method for degrading bisphenol A using a lanthanum manganate catalyst rich in oxygen vacancies, the dosage ratio of the lanthanum manganate catalyst rich in oxygen vacancies to the peroxymonosulfate oxidant is 0.01-0.03 g:0.1 mmol, for example, 0.02 g:0.1 mmol.

[0013] In the method for degrading bisphenol A using a lanthanum manganate catalyst rich in oxygen vacancies, the degradation reaction time is 0-60 minutes, such as 20 minutes.

[0014] The method for degrading bisphenol A using a lanthanum manganate catalyst rich in oxygen vacancies of the present invention, when the dosage ratio of the lanthanum manganate catalyst rich in oxygen vacancies to the bisphenol A in the bisphenol A-containing wastewater is 0.02g:1mg, and the dosage ratio of the lanthanum manganate catalyst rich in oxygen vacancies to the peroxymonosulfate oxidant is 0.02g:0.1mmol, the degradation reaction only takes 20min to degrade all the bisphenol A.

[0015] The method for degrading bisphenol A using a lanthanum manganate catalyst rich in oxygen vacancies, and the method for preparing the nano lanthanum manganate may include:

[0016] Citric acid is added to an aqueous solution containing lanthanum nitrate and manganese nitrate, and the mixture is stirred and heated to react to form a sol. The obtained sol is dried and annealed at 700° C. to obtain the nano-lanthanum manganate.

[0017] In the preparation method of the nano-lanthanum manganate, the molar ratio of the citric acid, the lanthanum nitrate and the manganese nitrate can be 2-4:1:1.

[0018] In the method for preparing nano-lanthanum manganate, the temperature of the stirring and heating reaction can be 60-80° C., the time can be 2-4 hours, and the stirring speed can be 250-350 rpm.

[0019] In the method for preparing nano-lanthanum manganate, the annealing atmosphere may be an air atmosphere.

[0020] In the preparation method of the nano-lanthanum manganate, the annealing time can be 2 hours.

[0021] The present invention also provides an application of the oxygen vacancy-rich lanthanum manganate catalyst to activate peroxymonosulfate to form a Fenton-like system in the degradation of bisphenol A.

[0022] Oxygen vacancies are the most common local electron-rich lattice defects. Since oxygen vacancies can adjust the charge distribution of metal atoms and accelerate the redox cycle of high-valent metal species, the introduction of oxygen vacancies in metal oxides may change the activation mode of peroxymonosulfate, or increase the activation pathway of peroxymonosulfate, thereby increasing the rate of metal oxide activation of peroxymonosulfate, and even broadening its practical application capabilities. The high-temperature reduction heat treatment in the preparation process of the oxygen-vacancy-rich lanthanum manganate can cause violent vibrations of oxygen atoms on the surface of the material, and the surface lattice oxygen atoms are more likely to diffuse and escape. By screening the reduction heat treatment temperature, heat treatment time and the amount ratio of nano-lanthanum manganate to sodium borohydride, a controllable concentration of oxygen vacancies is successfully constructed on the surface of lanthanum manganate, and a series of nano-lanthanum manganate with different catalytic activities are obtained. Oxygen vacancies are introduced without doping other metal elements, which can avoid the interference of variables other than oxygen vacancies and better explore the influence mechanism of oxygen vacancy concentration on the performance of nano-lanthanum manganate activation of peroxymonosulfate. In addition, when peroxymonosulfate is activated, oxygen vacancies can capture the active oxygen generated by the heterolysis of peroxymonosulfate and degrade bisphenol A through a non-radical pathway of electron transfer, thereby achieving rapid degradation of bisphenol A in wastewater. Under the mediation of oxygen vacancies, the oxygen-vacancies-rich lanthanum manganate catalyst can achieve complete degradation of 10 mg / L bisphenol A within 20 minutes.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] 1) The present invention uses nano-lanthanum manganate as a carrier, and with the help of a special carrier of a perovskite (ABO3) type catalyst, the number of oxygen atoms is reduced by a certain proportion, and its crystal form can remain unchanged. Sodium borohydride is used as a reducing agent, and sodium borohydride decomposes and generates active hydrogen in situ at a mild reaction temperature. This active hydrogen is more active than hydrogen and other reducing agents previously reported. Its strong reducing ability is conducive to removing oxygen atoms on the surface of nano-lanthanum manganate, thereby forming oxygen vacancies in a shorter time and at a lower temperature, which is conducive to maintaining the original morphology of nano-lanthanum manganate. Compared with metal oxide catalysts containing oxygen vacancies constructed by doping other metal elements, the lanthanum manganate catalyst modified by sodium borohydride will not introduce other metal ions, and the crystal structure is stable, the metal active center is clear, and the oxygen vacancy concentration is easy to adjust. Lanthanum manganate catalysts rich in oxygen vacancies can achieve complete degradation of 10mg / L bisphenol A within 20 minutes. At present, there is no research report on the modification of the oxygen atom defect structure of lanthanum manganate catalysts using sodium borohydride solid.

[0025] 2) In the present invention, nano-lanthanum manganate is reduced by high-temperature thermal modification with sodium borohydride under an inert atmosphere to generate oxygen vacancies. The method is simple and controllable. Modern characterization methods such as X-ray diffraction analysis and electron paramagnetic resonance have proved that the crystalline structure of the lanthanum manganate catalyst rich in oxygen vacancies is stable and the surface oxygen vacancy concentration is controllable.

[0026] 3) Oxygen vacancy-mediated peroxymonosulfate activation pathways can produce a variety of reactive oxygen species. The use of lanthanum manganate catalysts with controllable morphology and oxygen vacancy concentration to activate peroxymonosulfate to form a Fenton-like system for the degradation of bisphenol A is a reaction mechanism of electron transfer, not a single free radical oxidation (such as SO4 - ·,·OH oxidation) or singlet oxygen alone, the corresponding reaction pathway is conducive to the selective degradation of organic pollutants. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 X-ray diffraction patterns of nano-lanthanum manganate (LaMnO3) prepared in Example 1 and lanthanum manganate catalysts rich in oxygen vacancies prepared by using nano-lanthanum manganate and sodium borohydride in equal molar ratios at different thermal modification temperatures in Example 2.

[0028] Figure 2 This is a graph showing the change in bisphenol A removal rate during the degradation of bisphenol A using nano lanthanum manganate (LaMnO3) prepared in Example 1 and lanthanum manganate catalysts rich in oxygen vacancies prepared using nano lanthanum manganate and sodium borohydride in equal molar ratios at different thermal modification temperatures in Example 2.

[0029] Figure 3X-ray diffraction patterns of nano lanthanum manganate (LaMnO3) prepared in Example 1 and lanthanum manganate catalysts rich in oxygen vacancies prepared by using nano lanthanum manganate and sodium borohydride in equal molar ratios at different thermal modification times in Example 3.

[0030] Figure 4 The graph of the change in bisphenol A removal rate during the degradation of bisphenol A by the nano lanthanum manganate (LaMnO3) prepared in Example 1 and the lanthanum manganate catalyst rich in oxygen vacancies prepared by using nano lanthanum manganate and sodium borohydride in equal molar ratios at different thermal modification times in Example 3.

[0031] Figure 5 X-ray diffraction patterns of nano lanthanum manganate (LaMnO3) prepared in Example 1 and lanthanum manganate catalysts rich in oxygen vacancies prepared in Example 4 using different sodium borohydride dosage ratios.

[0032] Figure 6 The graph of the change in bisphenol A removal rate during the degradation of bisphenol A by the nano lanthanum manganate (LaMnO3) prepared in Example 1 and the lanthanum manganate catalyst rich in oxygen vacancies prepared in Example 4 with different sodium borohydride dosage ratios.

[0033] Figure 7 Transmission electron microscope photos of the nano lanthanum manganate (LaMnO3) prepared in Example 1 and the lanthanum manganate catalyst rich in oxygen vacancies prepared in Example 4 with different sodium borohydride dosage ratios.

[0034] Figure 8 The electron paramagnetic resonance images are of the nano lanthanum manganate (LaMnO3) prepared in Example 1 and the lanthanum manganate catalyst rich in oxygen vacancies prepared in Example 4 with different sodium borohydride dosage ratios. DETAILED DESCRIPTION

[0035] The present invention will be further described below in conjunction with the accompanying drawings and specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention.

[0036] Example 1

[0037] Step 1: Take 10 mmol of lanthanum nitrate hexahydrate (La(NO3)3·6H2O) and 10 mmol of manganese nitrate solution (Mn(NO3)2) (50 wt% aqueous solution), add them to 50 mL of deionized water, stir for 5 min, and obtain solution A;

[0038] Step 2: Take 24 mmol of citric acid (C6H8O7), add it to solution A, stir for 1 hour, and obtain solution B;

[0039] Step 3: Place liquid B in a water bath heating pot, the heating temperature of the water bath pot is 80°C, the stirring speed is 350r / min, the stirring reaction time is 4h, and a sol is obtained;

[0040] Step 4: drying the sol in a vacuum oven at 80° C. for 8 h to obtain an unmodified lanthanum manganate precursor;

[0041] Step 5: Grind the unmodified lanthanum manganate precursor into powder (about 30 minutes), transfer it to a crucible, and then place it in a muffle furnace for annealing. The annealing treatment is: raise the temperature in the furnace to 700°C at a heating rate of 2°C / min and maintain it for 2 hours. Then cool it naturally to obtain nano-lanthanum manganate, marked as LaMnO3.

[0042] Degradation experiment: 100 mL of wastewater to be treated was added to a conical flask, the concentration of bisphenol A in the wastewater to be treated was 10 mg / L, the initial pH of the wastewater to be treated was 6, and the initial temperature was 25°C; then, 0.02 g of nano-lanthanum manganate was added, ultrasonicated for 5 minutes, oscillated for 25 minutes, and then 1 mL of 100 mM permonosulfate (potassium permonosulfate complex salt) solution was added to initiate a reaction to degrade and remove bisphenol A, and the nano-lanthanum manganate in the solution was recovered after the reaction was completed.

[0043] The nano-lanthanum manganate obtained in this example can completely degrade 10 mg / L of bisphenol A within 60 minutes.

[0044] Example 2

[0045] Step 1: Take 1 mmol of nano-lanthanum manganate LaMnO3 prepared in Example 1 and 1 mmol of sodium borohydride, mix and grind into powder (about 15 minutes);

[0046] Step 2: Transfer the mixed and ground solids into a quartz boat, and then place it in a tube furnace for annealing. The annealing treatment is as follows: in an argon atmosphere, the temperature in the furnace is raised to 350°C, 375°C, 400°C, and 425°C at a heating rate of 5°C / min and kept warm for 1 hour. The annealed sample is washed with deionized water and dried to obtain a lanthanum manganate catalyst rich in oxygen vacancies, which are marked as LaMnO3-350, LaMnO3-375, LaMnO3-400, and LaMnO3-425, respectively. The characterization and application results of the samples prepared in this example are shown as follows. Figure 1 and Figure 2 shown.

[0047] The specific operation of the degradation experiment is shown in Example 1.

[0048] Example 3

[0049] Step 1: Take 1 mmol of nano-lanthanum manganate LaMnO3 prepared in Example 1 and 1 mmol of sodium borohydride, mix and grind into powder (about 15 minutes);

[0050] Step 2: Transfer the mixed and ground solids into a quartz boat, and then place it in a tubular furnace for annealing. The annealing treatment is as follows: in an argon atmosphere, raise the temperature in the furnace to 400°C at a heating rate of 5°C / min and keep warm for 40min, 60min, 80min, 120min, and 140min, respectively. Wash the annealed sample with deionized water and dry it to obtain a lanthanum manganate catalyst rich in oxygen vacancies, which are labeled LaMnO3-40, LaMnO3-60, LaMnO3-80, LaMnO3-120, and LaMnO3-140, respectively. The characterization and application results of the samples prepared in this example are shown as follows. Figure 3 and Figure 4 shown.

[0051] The specific operation of the degradation experiment is shown in Example 1.

[0052] Example 4

[0053] Step 1: Mix the nano-lanthanum manganate LaMnO3 prepared in Example 1 with sodium borohydride in different molar ratios (1:1.5, 1:2, 1:2.5, 1:3, 1:3.5) and grind into powder (about 15 minutes);

[0054] Step 2: Transfer the mixed and ground solid into a quartz boat, and then place it in a tube furnace for annealing. The annealing treatment is as follows: in an argon atmosphere, raise the temperature in the furnace to 400°C at a heating rate of 5°C / min and keep it warm for 120 minutes. Wash the annealed sample with deionized water and dry it to obtain a lanthanum manganate catalyst rich in oxygen vacancies, which are marked as LaMnO3-1.5n, LaMnO3-2n, LaMnO3-2.5n, LaMnO3-3n, and LaMnO3-3.5n respectively. The characterization and application results of the samples prepared in this example are shown as follows. Figure 5 and Figure 6 shown.

[0055] In this embodiment, the degradation experiment method is the same as the degradation experiment scheme in Example 1. During the reaction process, the concentration of bisphenol A in the reaction solution is tested. Specifically, 1 mL of the reaction solution is taken at a set time and filtered through a 220 nm filter membrane into a chromatographic bottle containing 0.5 mL of methanol solution. High performance liquid chromatography (HPLC) is used to test the concentration of bisphenol A in the reaction solution. The adsorption-degradation curve of bisphenol A in water obtained by the test is as follows: Figure 4As shown, during the first 20 minutes of adsorption-desorption process, bisphenol A was adsorbed by about 1.16%. After the degradation process began, when the molar ratio of LaMnO3 to sodium borohydride was 1:3, bisphenol A in the water was 100% completely degraded within 20 minutes, while the unmodified nano lanthanum manganate required 60 minutes to 100% degrade bisphenol A under the same conditions. Therefore, the lanthanum manganate catalysts with different oxygen vacancy concentrations prepared in this embodiment far exceeded the unmodified nano lanthanum manganate.

[0056] Attached Figure 1 X-ray diffraction patterns of the nano-lanthanum manganate (LaMnO3) prepared in Example 1 and the lanthanum manganate catalyst rich in oxygen vacancies prepared by using the same molar ratio of nano-lanthanum manganate and sodium borohydride at different thermal modification temperatures in Example 2. It can be seen from the figure that the crystal form of nano-lanthanum manganate (LaMnO3) remains stable at different thermal modification temperatures.

[0057] Attached Figure 2 The figure shows the change of the removal rate of bisphenol A by the activated persulfate of the nano lanthanum manganate (LaMnO3) prepared in Example 1 and Example 2 prepared by using the lanthanum manganate catalyst rich in oxygen vacancies and the equimolar ratio of nano lanthanum manganate and sodium borohydride at different thermal modification temperatures. It can be seen from the figure that at 350-400°C, the efficiency of LaMnO3 activating persulfate to degrade bisphenol A is proportional to the thermal modification temperature. However, when the thermal modification temperature is 425°C, the efficiency of LaMnO3 activating persulfate to degrade bisphenol A decreases. Therefore, the optimal thermal modification temperature is 400°C.

[0058] Attached Figure 3 X-ray diffraction patterns of the nano-lanthanum manganate (LaMnO3) prepared in Example 1 and the lanthanum manganate catalyst rich in oxygen vacancies prepared by using the same molar ratio of nano-lanthanum manganate and sodium borohydride at different thermal modification times in Example 3. It can be seen from the figure that the crystal form of nano-lanthanum manganate (LaMnO3) remains stable under different thermal modification times.

[0059] Attached Figure 4 The figure shows the change of the removal rate of bisphenol A by the activated persulfate of the nano lanthanum manganate (LaMnO3) prepared in Example 1 and Example 3, which is rich in oxygen vacancies and prepared by using the lanthanum manganate catalyst with equal molar ratio of nano lanthanum manganate and sodium borohydride at different thermal modification times. It can be seen from the figure that the efficiency of LaMnO3 in activating persulfate to degrade bisphenol A is proportional to the thermal modification time within 40 to 120 minutes. However, when the thermal modification time is increased to 140 minutes, the efficiency of LaMnO3 in activating persulfate to degrade bisphenol A decreases slightly. It is concluded that the optimal thermal modification time is 120 minutes.

[0060] Attached Figure 5X-ray diffraction patterns of the nano-lanthanum manganate (LaMnO3) prepared in Example 1 and the lanthanum manganate catalyst rich in oxygen vacancies prepared in different sodium borohydride dosage ratios in Example 4. It can be seen from the figure that under the same thermal modification temperature and thermal modification time conditions, the XRD patterns of the samples with the LaMnO3 and sodium borohydride molar ratios changed have diffraction peaks very similar to those of the nano-lanthanum manganate, indicating that the crystal forms of the samples are stable.

[0061] Attached Figure 6 The figure shows the change of bisphenol A removal rate during the degradation of bisphenol A by persulfate activated by the nano lanthanum manganate (LaMnO3) prepared in Example 1 and the lanthanum manganate catalyst rich in oxygen vacancies prepared in Example 4 with different sodium borohydride dosage ratios. 30 minutes before the addition of persulfate, LaMnO3 and the reaction solution have reached adsorption equilibrium, and the bisphenol A removal rate is less than 2%, which shows that bisphenol A cannot be effectively removed by the adsorption of LaMnO3. As shown in the figure, when the ratio of the amount of LaMnO3 to the amount of sodium borohydride increases from 1:1.5 to 1:3, the performance of LaMnO3 in activating persulfate to degrade bisphenol A gradually increases, and reaches the highest at 1:3, indicating that the introduction of oxygen vacancies greatly optimizes the catalytic performance of the catalyst, while the unmodified LaMnO3 needs to degrade bisphenol A 100% within 60 minutes under the same conditions. However, when the ratio of LaMnO3 to sodium borohydride is 1:3.5, the efficiency of the catalyst sample in activating persulfate to degrade bisphenol A is reduced. It is concluded that the optimal ratio of LaMnO3 to sodium borohydride is 1:3. This result shows that when the ratio of LaMnO3 to sodium borohydride is 1:3, the oxygen vacancy concentration of the prepared lanthanum manganate catalytic material rich in oxygen vacancies is optimal, which has a good promoting effect on enhancing the performance of the original LaMnO3 in activating persulfate to degrade bisphenol A.

[0062] Attached Figure 7 Transmission electron micrographs of the nano-lanthanum manganate (LaMnO3) prepared in Example 1 and the lanthanum manganate catalyst rich in oxygen vacancies prepared in different sodium borohydride dosage ratios in Example 4. (a.LaMnO3, b.LaMnO3-2.5n, c.LaMnO3-3n, d.LaMnO3-3.5n) It can be seen from the figure that the four samples of LaMnO3, LaMnO3-2.5n, LaMnO3-3n, and LaMnO3-3.5n are all disordered particles, and there is no obvious difference in the morphology surface, indicating that the introduction of oxygen vacancies in LaMnO3 by the method described in this patent will not destroy the microscopic morphology structure of LaMnO3.

[0063] Attached Figure 8The electron paramagnetic resonance images are of the nano lanthanum manganate (LaMnO3) prepared in Example 1 and the lanthanum manganate catalyst rich in oxygen vacancies prepared in Example 4 with different sodium borohydride dosage ratios. The stronger the oxygen vacancy signal peak in the figure, the higher the oxygen vacancy concentration of the sample, that is, the order of oxygen vacancy concentration of each sample is LaMnO3-3.5n>LaMnO3-3n>LaMnO3-2.5n>LaMnO3. The present invention has found that in the application of using a lanthanum manganate catalyst rich in oxygen vacancies to activate persulfate to form a Fenton-like system for degrading bisphenol A, the oxygen vacancy concentration of the lanthanum manganate catalyst rich in oxygen vacancies is not always the higher the better. Specifically, Figure 6 The bisphenol A removal rate change diagram of the nano lanthanum manganate (LaMnO3) prepared in Example 1 and the lanthanum manganate catalyst rich in oxygen vacancies prepared in Example 4 with different sodium borohydride dosage ratios during the degradation of bisphenol A. It can be seen from the figure that when the ratio of the amount of LaMnO3 to the amount of sodium borohydride is 1:3, the catalyst activity is the best and the bisphenol A removal effect is the best; while the catalyst LaMnO3-3.5n prepared when the ratio of the amount of LaMnO3 to the amount of sodium borohydride is 1:3.5, its performance of activating persulfate to degrade bisphenol A is not as good as LaMnO3-3n. This result shows that when the ratio of the amount of LaMnO3 to the amount of sodium borohydride is 1:3, the oxygen vacancy concentration on the surface of the prepared lanthanum manganate catalyst rich in oxygen vacancies is moderate, and it has very good catalytic performance for activating persulfate to degrade bisphenol A.

[0064] In addition, it should be understood that after reading the above description of the present invention, those skilled in the art may make various changes or modifications to the present invention, and these equivalent forms also fall within the scope defined by the claims attached to this application.

Claims

1. A method for degrading bisphenol A using a lanthanum manganate catalyst rich in oxygen vacancies, characterized in that: include: Lanthanum manganate catalyst rich in oxygen vacancies is added to wastewater containing bisphenol A, and peroxymonosulfate oxidant is added after adsorption-desorption equilibrium is reached to carry out degradation reaction of bisphenol A; The preparation method of the lanthanum manganate catalyst rich in oxygen vacancies comprises: mixing and grinding nano-lanthanum manganate and sodium borohydride, heat treating at 350-425° C., preferably 400° C., in an inert atmosphere, for 40-140 min, preferably 120 min, mixing the nano-lanthanum manganate and sodium borohydride in a molar ratio of 1:1-3.5, preferably 1:3, washing and drying the obtained product, and obtaining the lanthanum manganate catalyst rich in oxygen vacancies.

2. The method for degrading bisphenol A using a lanthanum manganate catalyst rich in oxygen vacancies according to claim 1, characterized in that: The dosage ratio of the lanthanum manganate catalyst rich in oxygen vacancies to the bisphenol A in the bisphenol A-containing wastewater is 0.01-0.03 g:1 mg.

3. The method for degrading bisphenol A using a lanthanum manganate catalyst rich in oxygen vacancies according to claim 1, characterized in that: The initial pH of the wastewater containing bisphenol A is 5-7.

4. The method for degrading bisphenol A using a lanthanum manganate catalyst rich in oxygen vacancies according to claim 1, characterized in that: The peroxymonosulfate oxidant is a potassium peroxymonosulfate composite salt.

5. The method for degrading bisphenol A using a lanthanum manganate catalyst rich in oxygen vacancies according to claim 1, 2 or 4, characterized in that: The dosage ratio of the lanthanum manganate catalyst rich in oxygen vacancies to the peroxymonosulfate oxidant is 0.01-0.03 g:0.1 mmol.

6. The method for degrading bisphenol A using a lanthanum manganate catalyst rich in oxygen vacancies according to claim 5, characterized in that: The degradation reaction time is 0-60min.

7. The method for degrading bisphenol A using a lanthanum manganate catalyst rich in oxygen vacancies according to claim 1, characterized in that: The preparation method of the nano lanthanum manganate comprises: Citric acid is added to an aqueous solution containing lanthanum nitrate and manganese nitrate, and the mixture is stirred and heated to react to form a sol. The obtained sol is dried and annealed at 700° C. to obtain the nano-lanthanum manganate.

8. The method for degrading bisphenol A using a lanthanum manganate catalyst rich in oxygen vacancies according to claim 7, characterized in that: In the preparation method of the nano lanthanum manganate: The molar ratio of the citric acid, the lanthanum nitrate and the manganese nitrate is 2-4:1:1; The stirring and heating reaction temperature is 80-100°C, the time is 2-4h, and the stirring speed is 250-350rpm; The annealing atmosphere is an air atmosphere; The annealing time is 2h.

9. Application of a lanthanum manganate catalyst rich in oxygen vacancies to activate peroxymonosulfate to form a Fenton-like system in the degradation of bisphenol A, characterized in that: The preparation method of the lanthanum manganate catalyst rich in oxygen vacancies comprises: mixing and grinding nano-lanthanum manganate and sodium borohydride, heat treating at 350-425° C., preferably 400° C., in an inert atmosphere, for 40-140 min, preferably 120 min, mixing the nano-lanthanum manganate and sodium borohydride in a molar ratio of 1:1-3.5, preferably 1:3, washing and drying the obtained product, and obtaining the lanthanum manganate catalyst rich in oxygen vacancies.

Citation Information

Cited By

  • Ternary chalcogenide composite perovskite catalytic material as well as synthesis method and application thereof

    CN120381854A

  • A ternary chalcogenide compound composite perovskite catalytic material, a synthesis method and application thereof

    CN120381854B