Zinc oxide / silver composite photocatalytic material and preparation method thereof

Through the flower cluster nanostructure of zinc oxide/silver composite, the problems of low quantum efficiency and limited visible light absorption of zinc oxide photocatalysts are solved, and efficient photocatalytic reactions and stable performance are achieved, suitable for environmental governance and water treatment. .

CN119034735APending Publication Date: 2024-11-29BOZHOU SHANGDA ENG TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410945412.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-15
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Zinc oxide (ZnO) as a photocatalyst has problems such as low quantum efficiency and limited visible light absorption in the field of photocatalytics, which limits its application potential.

Method used

The zinc oxide/silver (ZnO/Ag) composite material is used to react zinc salt and silver salt in an alkaline solution to form a composite material with a cluster-like nanostructure, and the photocatalytic performance is improved by synergistically acting between Ag nanoparticles and ZnO.

Benefits of technology

It significantly improves the photocatalytic reaction efficiency, enhances the visible light absorption capacity, increases the specific surface area and reactive sites, ensures the uniform distribution and dispersion of Ag nanoparticles, and achieves excellent photocatalytic effects and multiple Stable performance for the second use.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119034735A_ABST
    Figure CN119034735A_ABST
Patent Text Reader

Abstract

The invention provides a ZnO / Ag composite photocatalytic material and a preparation method thereof, the ZnO / Ag composite photocatalytic material is of a flower-cluster-shaped nano structure and has good photocatalytic performance, and the visible light absorption capacity is also enhanced. Through the synergistic effect of the Ag nanoparticles and ZnO, the composite material can efficiently capture visible light in sunlight, and the photocatalytic reaction efficiency is promoted. The specific surface area is greatly increased, and the reaction process is further accelerated by abundant reaction active sites. In addition, EDS analysis confirms that elements are uniformly distributed, and effective dispersion of the Ag nano-particles and maximization of catalytic potential are guaranteed. The composite photocatalytic material not only optimizes the charge ratio of Ag / ZnO to obtain the optimal photocatalytic efficiency, but also shows good pH adaptability and stable catalytic performance after repeated use. Especially under a weak alkaline condition, the composite material shows an excellent photocatalytic effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of photocatalytic pollutant treatment, and in particular to a zinc oxide / silver composite photocatalytic material and a preparation method thereof. Background Art

[0002] Dye wastewater has become a major problem in environmental management due to its high chroma, high organic matter concentration and large fluctuations in water quality. Traditional treatment methods, such as adsorption, membrane separation and coagulation sedimentation, can achieve phase transfer of dye molecules, but they cannot completely degrade these organic substances, thus bringing the risk of secondary pollution.

[0003] Among the many emerging wastewater treatment technologies, photocatalytic technology has shown great potential in the field of dye degradation due to its significant advantages such as high efficiency, low energy consumption, easy operation, wide application range, non-toxicity and no secondary pollution.

[0004] Among them, titanium dioxide (TiO2) is a common photocatalytic material, which has a suitable semiconductor band gap width (3.2eV) and can be excited and activated by light sources below 387nm. Through modification, it is expected to directly use solar energy to drive photocatalytic reactions. However, the band gap of TiO2 is large, and higher energy is required to stimulate its photocatalytic activity, which limits its use in certain photocatalytic applications.

[0005] Zinc oxide (ZnO), as a key semiconductor photocatalytic material, has a similar bandgap to titanium dioxide (TiO2), and its bandgap is narrower and more sensitive to visible light. Its photocatalytic activity even surpasses that of TiO2 in the degradation of certain organic pollutants. However, ZnO nanostructured materials face two major challenges in practical applications: first, the rapid recombination of photogenerated electrons and holes leads to reduced quantum efficiency, and second, its absorption of visible light is extremely limited. Therefore, how to improve the quantum efficiency of ZnO and broaden the spectral response range has become a research focus in the field of photocatalysis. Summary of the invention

[0006] In order to solve the shortcomings of ZnO as a catalyst in the field of photocatalysis in the prior art, the present invention provides a zinc oxide / silver (ZnO / Ag) composite material photocatalytic material and a preparation method thereof, using zinc salt, silver salt and reducing sugar as raw materials, through a simple precipitation reaction, a zinc oxide composite material (ZnO / Ag) loaded with silver element with different feed ratios is synthesized, the composite material presents a flower cluster nanostructure, and has good photocatalytic performance.

[0007] The first aspect of the present invention is to provide a method for preparing a zinc oxide / silver (ZnO / Ag) composite photocatalytic material, the steps comprising:

[0008] Zinc (Zn2+ ) salt, silver (Ag + ) salt is placed in a first solvent and mixed to obtain a solution A;

[0009] placing a base and a reducing sugar in a second solvent and mixing them to obtain a solution B;

[0010] The solution A is mixed with the solution B to react, thereby obtaining a reaction product, namely, a ZnO / Ag composite photocatalytic material.

[0011] Preferably, the zinc salt may be an inorganic acid salt or an organic acid salt, and is preferably selected from one or more combinations of Zn(NO3)2, ZnCO3, ZnSO4, ZnCl2, ZnBr2, Zn(CH3COO)2, and Zn(HCOO)2.

[0012] More preferably, the zinc salt is a water-soluble or alcohol-soluble salt.

[0013] More preferably, the zinc salt may be provided in the form of a hydrate, an aqueous solution or an alcohol solution.

[0014] Preferably, the silver salt may be an inorganic acid salt or an organic acid salt, and is preferably one or more combinations selected from Ag(CO2CH3), AgNO3, Ag2CO3, Ag2SO4.

[0015] More preferably, the silver salt is a water-soluble or alcohol-soluble salt.

[0016] More preferably, the silver salt may be provided in the form of a hydrate, an aqueous solution or an alcohol solution.

[0017] Preferably, the weight ratio of the zinc salt (preferably, calculated as a hydrate of Zn(NO3)2) to the silver salt (preferably, calculated as AgNO3) is (50-550):1, preferably (70-530):1, and more preferably (100-500):1. Specifically, the weight ratio of the zinc salt (preferably, calculated as a hydrate of Zn(NO3)2) to the silver salt (preferably, calculated as AgNO3) can be one of 487:1, 432:1, 417:1, 364:1, 207:1, 137:1, 126:1, and 103:1.

[0018] Preferably, the first solvent can be one or more of water, alcohol, ether, ester, ketone, halogenated hydrocarbon, aromatic hydrocarbon, and ionic liquid, and is preferably selected from: water, N,N-dimethylformamide solution, methanol, ethanol, ether, tetrahydrofuran, dichloromethane, carbon tetrachloride, ethyl acetate, acetone, N-methylpyrrolidone, toluene, ionic liquid (such as 1-butyl-3-methylimidazolium hexafluorophosphate) and mixed in one or more combinations of solvents.

[0019] Preferably, the base is selected from one or more of sodium hydroxide (NaOH), sodium bicarbonate (NaHCO3), sodium carbonate (Na2CO3), potassium hydroxide (KOH), lithium hydroxide (LiOH), calcium hydroxide (Ca(OH)2), magnesium hydroxide (Mg(OH)2), barium hydroxide (Ba(OH)2), and aqueous ammonia (NH3·H2O).

[0020] More preferably, the base described in the present application is one or more selected from sodium hydroxide (NaOH), potassium hydroxide (KOH), and ammonia water (NH3·H2O).

[0021] More preferably, the concentration of the alkali in solution B (preferably, calculated as sodium hydroxide) is 60-120 g / L, preferably 70-100 g / L, more preferably 75-80 g / L.

[0022] In a preferred embodiment, the reducing sugar may be selected from monosaccharides and / or disaccharides, such as the reducing sugar may be one or more of glucose, fructose, galactose, lactose and maltose.

[0023] Meanwhile, the reducing sugar may also be a substance that can be degraded into reducing sugar in solution A and / or solution B, such as sucrose, starch, etc.

[0024] More preferably, the reducing sugar described in the present application is selected from one or more of glucose and fructose.

[0025] More preferably, the concentration of the reducing sugar (preferably, calculated as glucose) in solution B is 5-20 g / L, preferably 6-18 g / L, more preferably 8-12 g / L.

[0026] Preferably, the second solvent can be one or more of water, alcohol, ether, ester, ketone, halogenated hydrocarbon, aromatic hydrocarbon, and ionic liquid, and is preferably selected from: water, N,N-dimethylformamide solution, methanol, ethanol, ether, tetrahydrofuran, dichloromethane, carbon tetrachloride, ethyl acetate, acetone, N-methylpyrrolidone, toluene, ionic liquid (such as 1-butyl-3-methylimidazolium hexafluorophosphate) and mixed in one or more combinations of solvents.

[0027] In a preferred embodiment, before the B solution is mixed with the A solution, the temperature of the B solution is 50-100°C, preferably 60-80°C, and more preferably 70-75°C.

[0028] Preferably, before the B solution is mixed with the A solution, the B solution is heated.

[0029] In a preferred embodiment, the A solution and the B solution are mixed by adding the A solution into the B solution dropwise.

[0030] In a preferred embodiment, the reaction temperature of solution A and solution B is 50-100°C, preferably 60-80°C, more preferably 70-75°C.

[0031] In a preferred embodiment, the reaction product is further washed, and more preferably, after washing, the reaction product is further dried.

[0032] Preferably, the cleaning solvent used for the cleaning is one or more of water, ethanol and methanol.

[0033] Preferably, the drying temperature of the reaction product is 50-100°C, preferably 55-80°C, more preferably 60-75°C.

[0034] The second aspect of the present application is to provide a photocatalyst, preferably a photocatalyst with good photocatalytic performance, namely the zinc oxide / silver (ZnO / Ag) composite photocatalytic material described in the present application.

[0035] Preferably, the composite photocatalytic material is obtained by the above-mentioned preparation method of the present application.

[0036] In a preferred embodiment, the structure of the ZnO / Ag composite photocatalytic material is a nanostructure, preferably a flower cluster nanostructure.

[0037] In a preferred embodiment, the reaction product includes Ag and ZnO.

[0038] Preferably, based on the total mass of the reaction product, the mass fraction of Ag is 0.2-10wt%, preferably 0.3-5wt%, more preferably 0.5-3wt%, more preferably 0.5-2wt%.

[0039] Specifically, based on the total mass of the reaction product, the mass fraction of Ag may be one or more of 0.5 wt%, 1 wt%, 1.5 wt%, 2 wt%, 2.5 wt%, and 3 wt%.

[0040] The third aspect of the present application is to provide a photocatalytic method, comprising performing photocatalysis using the photocatalyst described in the present application.

[0041] In a preferred embodiment, the photocatalysis is carried out under alkaline conditions.

[0042] Preferably, the alkaline condition has a pH value of 8-10, more preferably 8.5-9.

[0043] In a preferred embodiment, in the photocatalyst, the ratio of Ag in the ZnO / Ag composite material is preferably one or more of 0.5wt%, 1wt%, 1.5wt%, 2wt%, 2.5wt%, 3wt%.

[0044] Compared with the prior art, the present invention has the following technical effects:

[0045] The present invention provides a ZnO / Ag composite photocatalytic material and a preparation method thereof, wherein the ZnO / Ag composite photocatalytic material presents a flower cluster nanostructure, has good photocatalytic performance, and has enhanced visible light absorption capacity. The present invention uses the synergistic effect of Ag nanoparticles and ZnO, and the composite material can efficiently capture visible light in sunlight and promote the efficiency of photocatalytic reaction. The substantial increase in its specific surface area and the abundant reactive active sites further accelerate the reaction process. In addition, the EDS analysis of the present invention confirms the uniform distribution of elements, ensuring the effective dispersion of Ag nanoparticles and the maximization of catalytic potential. The composite photocatalytic material not only optimizes the Ag / ZnO feed ratio to obtain the best photocatalytic efficiency, but also exhibits good pH adaptability and stable catalytic performance after multiple uses. Especially under weakly alkaline conditions, the composite material exhibits an excellent photocatalytic effect, has a strong mineralization ability, effectively degrades organic pollutants, provides an efficient and low-cost solution for the fields of environmental governance and water treatment, and exhibits broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0046] Figure 1 The X-ray diffraction (XRD) diagrams of pure phase ZnO and ZnO / Ag composite materials obtained in the examples of the present invention are shown.

[0047] Figure 2 These are scanning electron microscope (SEM) images at different magnifications of the synthesized 1.5 wt % ZnO / Ag sample obtained in an example of the present invention.

[0048] Figure 3 Scanning electron microscope images of the 1.5wt% ZnO / Ag sample obtained in an example of the present invention at different magnifications (ab); X-ray energy dispersive (EDS) surface scanning image (dg) and EDS elemental analysis spectrum and illustration of its analysis results (c).

[0049] Figure 4 The Fourier transform infrared absorption spectra of the pure phase ZnO and 1.5wt% ZnO / Ag samples obtained in the examples of the present invention are shown.

[0050] Figure 5 The nitrogen adsorption-desorption isotherms and the corresponding pore size distribution diagrams obtained in the examples of the present invention are as follows: (ab) 1.5 wt% ZnO / Ag sample; (cd) pure phase ZnO.

[0051] Figure 6 50 mg of 1.5 wt% ZnO / Ag sample obtained in the present invention was mixed with 50 mL of 100 mg·L -1Adsorption of methylene blue (MB) solution: The adsorption conditions are neutral and room temperature 25°C.

[0052] Figure 7 The UV-visible diffuse reflectance spectra of the pure phase ZnO obtained in the embodiment of the present invention and the ZnO / Ag samples with different feed ratios are shown.

[0053] Figure 8 The (Ahv)2-hv curves of the pure phase ZnO obtained in the examples of the present invention and the ZnO / Ag samples with different feed ratios.

[0054] Fig. 9 The figure shows the change of the decolorization rate of MB solution photocatalyzed by ZnO / Ag samples with different feed ratios under neutral conditions over time obtained in the examples of the present invention.

[0055] Fig.10 The decolorization rate of the 1.5wt% ZnO / Ag sample for MB solution changes over time under different pH conditions obtained in the examples of the present invention.

[0056] Fig.11 The effect of the pre-treatment stirring time on the decolorization rate of the MB solution obtained in the examples of the present invention.

[0057] Table 1 shows the mineralization of the ZnO / Ag sample obtained in the embodiment of the present invention to the MB solution.

[0058] Fig.12 The decolorization rate of the MB solution obtained in the embodiment of the present invention changes with the number of times the ZnO / Ag sample photocatalyst is used. DETAILED DESCRIPTION

[0059] The present invention provides a ZnO / Ag composite material photocatalytic material and a preparation method thereof. In order to make the purpose, technical solution and effect of the present invention clearer and more specific, the present invention is further described in detail with reference to the accompanying drawings and examples. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0060] It should be noted that the terms "first", "second", etc. in the specification and claims of the present invention and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchanged under appropriate circumstances. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions. For example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.

[0061] Example 1

[0062] (1) Dissolve 2.0 g of sodium hydroxide and 0.3 g of glucose in 25 mL of deionized water and stir evenly on a magnetic stirrer to form solution B;

[0063] (2) Take 7.5 g of zinc nitrate hexahydrate, dissolve it in 25 mL of deionized water, place it on a magnetic stirrer and stir it for a period of time to fully dissolve it, to prepare solution C.

[0064] (3) Place solution B in a 70°C constant temperature water bath. After the temperature stabilizes, add solution C dropwise into solution B under magnetic stirring. After the addition is complete, keep the mixture warm for a period of time and then cool it to room temperature. Separate the precipitate by centrifugation, wash it three times with deionized water and ethanol, and dry it in a 60°C constant temperature box to obtain a pure phase zinc oxide (ZnO) sample.

[0065] Example 2

[0066] (1) Take zinc nitrate hexahydrate and add silver nitrate in a weight ratio of zinc nitrate hexahydrate to silver nitrate of 417:1, 207:1, 137:1, and 103:1, dissolve in 25 mL of deionized water, place on a magnetic stirrer and stir for a period of time to fully mix, to prepare solution A.

[0067] (2) Dissolve 2.0 g of sodium hydroxide and 0.3 g of glucose in 25 mL of deionized water and stir evenly on a magnetic stirrer to form solution B;

[0068] (3) Place solution B in a 70°C constant temperature water bath. After the temperature stabilizes, add solution A dropwise into solution B under magnetic stirring. After the addition is complete, keep the mixture warm for a while and cool to room temperature. The precipitate was separated by centrifugation, washed three times with deionized water and ethanol, and then dried in a thermostat at 60°C to obtain ZnO / Ag composite material samples with different feed ratios, which were recorded as 0.5wt% ZnO / Ag (in the ZnO / Ag composite material, the proportion of Ag was 0.5wt% based on the total mass of the composite material), 1wt% ZnO / Ag (in the ZnO / Ag composite material, the proportion of Ag was 1wt% based on the total mass of the composite material), 1.5wt% ZnO / Ag (in the ZnO / Ag composite material, the proportion of Ag was 1.5wt% based on the total mass of the composite material) and 2.0wt% ZnO / Ag samples (in the ZnO / Ag composite material, the proportion of Ag was 2.0wt% based on the total mass of the composite material).

[0069] Figure 1The X-ray diffraction patterns of pure ZnO in Example 1 and ZnO / Ag samples in Example 2 are shown. The results show that the positions of the main diffraction peaks (100), (002), (101), (102), (103) and (110) of each sample are consistent with the diffraction data of the hexagonal wurtzite structure (JCPDS No.36-1451), verifying that the synthesized sample is a hexagonal phase ZnO, in which the diffraction peak of Ag shows an increasing trend with the increase of Ag content. When the Ag content in the sample is low (0.5wt%), the diffraction peak of Ag is not easy to appear. When the Ag content increases to 1wt%, the diffraction peak (111) begins to appear; when the Ag content reaches 2wt%, its diffraction peaks (111) and (220) are both revealed, and their positions are consistent with the Ag data of the face-centered cubic structure (JCPDS No.04-0783).

[0070] Figure 2 The SEM images of 1.5wt% ZnO / Ag samples at different magnifications are shown. As can be seen from the figure, the synthesized composite sample presents a flower cluster nanostructure, which is composed of nanorods with a length of about 200-300nm. The morphology of the nanorods is uneven, showing a morphology of thin ends and thick middle. It may be that the tops of some nanorods are "dissolved" during the reaction process. The final formation of the flower cluster may be due to the high surface energy at the junction of the double-section rods, the large number of active sites, and the easy secondary nucleation, which in turn forms secondary dendrites.

[0071] Figure 3 The EDS surface scanning image (eg) and EDS elemental analysis results (Figure c) of the 1.5wt% ZnO / Ag sample are shown. The results of the micro-area surface scanning of the three elements Ag, Zn and O correspond to the red area, green area and blue area respectively, and these three elements are evenly distributed in the synthesized zinc oxide and silver composite sample. The red area corresponding to the Ag element is not obvious, which may be due to its low content. Figure 3 The peaks of Ag, Zn and O were found in c, proving the presence of three elements Ag, Zn and O in the prepared 1.5wt% ZnO / Ag sample.

[0072] Figure 4They are the infrared spectra of ZnO and 1.5wt% ZnO / Ag samples. The infrared spectra of 1.5wt% ZnO / Ag sample are similar to those of pure ZnO. The vibration absorption peak of Zn-O bond at 483nm appears red-shifted in the composite sample, which is caused by the interaction between Ag and ZnO in the ZnO / Ag composite. They both have an infrared absorption peak at 3500cm-1, which is caused by the vibration of OH in adsorbed water. The strong absorption peak of unsaturated ketone and alkene at 1643cm-1 in the composite is caused by the stretching vibration of C=C. These C=O, C=C and CH bonds all come from the collision reaction of different functional groups during the synthesis of the sample, indicating that unreacted glucose remains on the surface of the synthesized 1.5wt% ZnO / Ag sample, which is consistent with the detection of C element in EDS analysis.

[0073] Figure 5 The nitrogen adsorption-desorption isotherms and the corresponding pore size distribution diagram of the synthesized 1.5wt% ZnO / Ag composite sample are shown. According to the classification of adsorption-desorption isotherms by the International Union of Pure and Applied Chemistry (IUPAC), the synthesized samples all belong to type II adsorption-desorption isotherms. The adsorption and desorption curves in the figure do not overlap, that is, the adsorption and desorption are not completely reversible, which is called the hysteresis effect and belongs to the H3 type hysteresis loop. This adsorption-desorption curve usually appears in slit pore structures, indicating that the 1.5wt% ZnO / Ag composite material has a mesoporous structure. According to BJH theoretical calculations, the pore size range of pure phase ZnO is 0-70nm, and the specific surface area is 19.396m2 / g. The specific surface area (22.955m2 / g) of the synthesized ZnO / Ag composite has increased, indicating that the activation area of ​​the catalytic reaction and the adsorption capacity of the composite can be increased, thereby improving its photocatalytic performance. The pore size range (0-80 nm) did not change significantly, which may be due to the smaller amount of Ag deposition.

[0074] Figure 6 It shows that when the time is 80-100 min, the MB concentration is almost unchanged. We can think that the 1.5wt% ZnO / Ag composite sample has reached the adsorption equilibrium for MB, and only 5.7% MB is adsorbed and removed at this time. Calculation shows that the apparent adsorption amount of MB in water adsorbed by 1 gram of 1.5wt% ZnO / Ag sample is about 5.7mg.

[0075] Figure 7The UV-visible diffuse reflectance spectra of ZnO / Ag composites and pure ZnO powder with different feed ratios are shown. As can be seen from the figure, the UV-visible diffuse reflectance spectrum of pure ZnO has only a characteristic absorption edge near 400nm. The UV-visible diffuse reflectance spectra of all synthesized ZnO / Ag composite samples, in addition to the characteristic absorption edge near 400nm, also have a peak near 450nm. This is the characteristic absorption peak of metal Ag, which is caused by the surface plasma effect of metal Ag, and the absorption peak of each composite sample is enhanced as the Ag ratio increases. This result further indicates the presence of metal Ag, which is consistent with the XRD analysis results. Compared with pure ZnO, the ZnO / Ag composite also has an absorption peak in the visible light region, so it can fully utilize the visible light part of sunlight, greatly increasing the light absorption efficiency.

[0076] Figure 8 The (Ahv) of pure ZnO and ZnO / Ag composite samples with different feed ratios are presented. 2 -hv curve. From the figure, we can see that the (Ahv) of ZnO / Ag composite samples with different feed ratios 2 -hv curve morphology is similar. By making a tangent to the obtained curve, it can be obtained that the band gap width of the synthesized pure ZnO is 3.25eV, which is basically consistent with its theoretical value of 3.2eV. The band gap width of the composites is smaller than that of pure ZnO, among which the band gap width of 1.5wt% ZnO / Ag sample is the smallest, which is 3.08eV. This indicates that after compounding with heavy metal Ag, the surface plasma effect of Ag effectively broadens the light absorption range of ZnO.

[0077] Fig. 9The figure shows the decolorization of methylene blue (MB) solution by synthesized ZnO / Ag samples with different feed ratios. It can be seen from the figure that pure ZnO has a certain decolorization effect on MB solution within a reaction time of 100 minutes, and its decolorization rate is 32.3%. The decolorization rates of the other ZnO / Ag samples with different feed ratios are all higher than that of pure zinc oxide, indicating that compounding with Ag is indeed an effective means to improve the photocatalytic performance of ZnO. Among them, the 1.5wt% ZnO / Ag sample has the highest decolorization rate for methylene blue solution. When the reaction is carried out for about 40 minutes, the decolorization rate basically reaches about 67.7% and remains unchanged. When the feed ratio of Ag to ZnO is lower than 1.5wt%, the decolorization rate of the sample for methylene blue solution shows an upward trend with the increase of the Ag ratio, while when the Ag to ZnO ratio increases to 2wt%, the decolorization rate decreases instead. It can be seen that under the reaction conditions, the feed ratio of Ag to ZnO has an important influence on the decolorization performance of the composite photocatalyst, and there is an optimal range of about 1.5%. This may be because as the proportion of Ag increases, the photogenerated electrons cannot react with dissolved oxygen in time when they are transferred to Ag, resulting in electron aggregation, generating a large delocalization energy, and having a greater attraction to holes. At this time, the photogenerated electrons will recombine with holes, thereby increasing the photogenerated electron-hole coincidence rate and reducing the catalytic efficiency.

[0078] Fig.10 As shown in the figure, when the 1.5wt% ZnO / Ag composite sample acts on the photocatalytic system of MB solution in alkaline conditions, i.e., pH greater than 7, the decolorization rate of the composite sample for MB solution is higher than that under neutral (pH=7) and acidic conditions (pH=5). When the system is in weak alkalinity and pH=9, the decolorization rate of MB solution reaches a maximum value of 67.2%.

[0079] Fig.11 It shows that when the stirring time is too short (30min), the composite sample synthesized has the worst decolorization ability for MB solution, only 57.7%. This may be due to the fact that the reactants are not completely dissolved in water, resulting in insufficient subsequent precipitation reaction. In this case, it will not only affect the morphological characteristics of the product but also reduce the actual amount of Ag and ZnO composite. With the increase of stirring time, the decolorization rate of MB solution increases significantly. The composite sample prepared under the condition of stirring for 60min pretreatment has the strongest decolorization ability of 69%. Too long stirring time will reduce the decolorization rate of the sample. It is speculated that excessive stirring may destroy the precursor structure and affect the formation of subsequent composite samples.

[0080] Table 1 shows the mineralization of the ZnO / Ag samples obtained in the present invention for MB solution. The results show that the ZnO / Ag composite samples synthesized with different feed ratios have significant differences in COD and T℃ removal rates for MB solution. Among them, the 1.5wt% ZnO / Ag sample with the highest mineralization has COD and T℃ removal rates of 41% and 35.7% for MB solution, respectively.

[0081] Table 1. Mineralization of ZnO / Ag samples to MB solution

[0082]

[0083] Fig.12 The decolorization rate of MB solution obtained by the implementation of the present invention changes with the number of times the ZnO / Ag sample photocatalyst is used. Here, the best performance 1.5wt%, the second best performance 1wt% ZnO / Ag composite sample and the pure phase ZnO sample are selected for investigation. The results show that the photocatalytic performance of the three selected catalysts does not change significantly with the increase in the number of times used. Among them, the decolorization rate of the MB solution of the 1.5wt% ZnO / Ag composite sample decreased from 67% to 63.6% after being used 5 times. It can be considered that within a certain number of catalytic reactions, the catalytic performance of the catalyst sample is very stable. The decolorization rates of the 1wt% ZnO / Ag composite sample and pure ZnO with the same number of uses decreased from 50.09% and 30.75% to 48.2% and 27.8%, respectively. Therefore, the synthesized 1.5wt% ZnO / Ag composite sample has a good photocatalytic effect and has potential photocatalytic application prospects.

[0084] Therefore, the embodiment of the present invention provides a ZnO / Ag composite photocatalytic material and a simple preparation method thereof. The ZnO / Ag composite exhibits a unique flower cluster-like nanostructure, which not only greatly improves the photocatalytic performance, but also significantly enhances the light absorption capacity in the visible light region (such as Figure 7 This is due to the introduction of Ag nanoparticles and their synergistic effect with ZnO. This structural feature enables the composite to more effectively capture and utilize the visible light portion of sunlight, thereby significantly improving the efficiency of the photocatalytic reaction.

[0085] Compared with pure ZnO, the specific surface area of ​​ZnO / Ag composites is significantly increased (e.g. Figure 5 As shown in Figure 2), it provides more activation areas and enhanced adsorption capacity for the catalytic reaction, promoting the effective conversion of the reactants. Figure 2 (as shown) not only enriches the surface morphology of the material, but also creates more reactive active sites, further accelerating the photocatalytic process.

[0086] According to the EDS analysis of this embodiment ( Figure 3 The uniform distribution of Ag, Zn and O elements in the ZnO / Ag composite was confirmed, ensuring the effective dispersion of Ag nanoparticles in the ZnO matrix and maximizing the catalytic potential of Ag. In addition, by embedding Ag nanoparticles in the ZnO matrix, the aggregation and deactivation of Ag were effectively prevented, and the stability and service life of the catalyst were improved.

[0087] The experimental results of this example also show that the decolorization rate of ZnO / Ag composite for methylene blue (MB) solution is much higher than that of pure ZnO (such as Fig. 9 The results show that, especially when the Ag loading is 1.5wt%, the composite exhibits the best photocatalytic activity and can achieve a high decolorization rate in a short time. This discovery reveals the importance of optimizing the feed ratio of Ag to ZnO and provides a scientific basis for obtaining the highest photocatalytic efficiency.

[0088] In addition, the ZnO / Ag composite also exhibits good pH adaptability (e.g. Fig.10 The decolorization effect of MB solution was better under alkaline conditions, showing its wide applicability under different environmental conditions. More impressively, the composite can still maintain stable catalytic performance after multiple uses (as shown in Fig.12 The durability and reusability of the 1.5wt% ZnO / Ag sample provide a strong guarantee for cost control and efficiency improvement in practical applications.

[0089] In terms of mineralization ability, the ZnO / Ag composite has significant COD and T℃ removal rates for MB solution, especially the 1.5wt% ZnO / Ag sample, which exhibits strong mineralization ability (as shown in Table 1), and can effectively degrade and transform organic pollutants into harmless substances, providing new solutions for environmental governance and water treatment.

[0090] In summary, the ZnO / Ag composite photocatalytic material of the embodiment of the present invention shows significant advantages in terms of light absorption range, photocatalytic performance, feed ratio optimization, pH adaptability, catalytic stability, mineralization ability, and morphology and structure. The embodiment of the present invention has a simple preparation process, mild reaction conditions, and low production cost, and has extremely broad application prospects. Especially under weakly alkaline conditions, the excellent photocatalytic effect exhibited by its composite material further highlights its great potential in the field of environmental purification.

[0091] The specific embodiments of the present invention are described in detail above, but they are only examples, and the present invention is not limited to the specific embodiments described above. For those skilled in the art, any equivalent modifications and substitutions made to the present invention are also within the scope of the present invention. Therefore, the equalization changes and modifications made without departing from the spirit and scope of the present invention should be included in the scope of the present invention.

Claims

1. A method for preparing a zinc oxide / silver composite photocatalytic material, comprising: placing a zinc salt and a silver salt in a first solvent and mixing them to obtain a solution A; placing a base and a reducing sugar in a second solvent and mixing them to obtain a solution B; The solution A is mixed with the solution B to react, thereby obtaining a reaction product, namely, a ZnO / Ag composite photocatalytic material.

2. The preparation method according to claim 1, characterized in that: The zinc salt may be one or more combinations selected from Zn(NO3)2, ZnCO3, ZnSO4, ZnCl2, ZnBr2, Zn(CH3COO)2, Zn(HCOO)2; and / or The zinc salt is a water-soluble or alcohol-soluble salt; and / or The zinc salt is provided in the form of a hydrate, an aqueous solution or an alcohol solution.

3. The preparation method according to claim 1, characterized in that: The silver salt may be one or more combinations selected from Ag(CO2CH3), AgNO3, Ag2CO3, Ag2SO4; and / or The silver salt is a water-soluble or alcohol-soluble salt; and / or The silver salt is provided in the form of its hydrate, aqueous solution or alcohol solution.

4. The preparation method according to claim 1, characterized in that: The alkali includes one or more of sodium hydroxide, sodium bicarbonate, sodium carbonate, potassium hydroxide, lithium hydroxide, calcium hydroxide, magnesium hydroxide, barium hydroxide, and ammonia water.

5. The preparation method according to claim 1, characterized in that: The reducing sugar may be selected from monosaccharides and / or disaccharides, such as the reducing sugar may be one or more of glucose, fructose, galactose, lactose, and maltose; and / or The reducing sugar may also be a substance that can be degraded into reducing sugar in solution A and / or solution B, such as sucrose, starch, and the like.

6. The preparation method according to claim 5, characterized in that: The reducing sugar is glucose or fructose; and / or The concentration of the reducing sugar in solution B is 5-20 g / L, preferably 6-18 g / L, more preferably 8-12 g / L.

7. The preparation method according to claim 1, characterized in that: Before the B solution is mixed with the A solution, the temperature of the B solution is 50-100°C, preferably 60-80°C, more preferably 70-75°C.

8. The preparation method according to claim 1, characterized in that: Based on the total mass of the reaction product, the mass fraction of Ag is 0.2-10wt%, preferably 0.3-5wt%, and more preferably 0.5-2wt%.

9. A photocatalyst, namely the zinc oxide / silver composite photocatalytic material, characterized in that: Obtained based on the preparation method according to any one of claims 1 to 8.

10. A photocatalytic method, characterized in that: The steps include: Photocatalysis is carried out using the photocatalyst according to claim 9.

Citation Information

Patent Citations

  • Silver quantum dot magnetic zinc oxide photocatalytic material and preparation method

    CN111617770A

  • Photocatalytic material for degrading tetracycline in wastewater and preparation method thereof

    GB202216790D0