Semi-solid thixotropic die-casting process for magnesium alloy step
The escalator steps are manufactured through magnesium alloy materials and semi-solid thixotropic die-casting process, which solves the problem of heavy and high cost of aluminum-silicon alloys, and realizes lightweight and high-strength magnesium alloy steps, reducing production costs and improving service life.
Patent Information
- Application Number
- CN202411289969.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-14
- Publication Date
- 2024-11-29
AI Technical Summary
The existing escalator steps mainly use heavy and costly aluminum-silicon alloys, which are difficult to meet the market demand for lightweight and strength indicators.
Magnesium alloy material and semi-solid thixotropic die-casting process are used to manufacture magnesium alloy steps through raw material smelting, die casting, mold opening and post-treatment steps, and the strength and service life are improved by using the fluidity and tissue density of semi-solid metals. Reduce production costs.
It realizes lightweight and low-cost production of magnesium alloy steps, improves the mechanical properties and service life of steps, saves energy and reduces mold damage.
Smart Images

Figure CN119035490A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of processing and manufacturing of escalators, and in particular to a semi-solid thixotropic die-casting process for magnesium alloy steps. Background Art
[0002] Most of the existing escalator steps are made of aluminum-silicon alloy, which is heavy and has high production and operation costs. Therefore, with the changes in the market and the promotion of lightweight, magnesium alloy steps have begun to enter the market in large quantities. In response to market demand, how to manufacture magnesium alloy steps that meet various strength indicators has become a technical problem that needs to be solved urgently. Summary of the invention
[0003] In view of this, an embodiment of the present invention provides a semi-solid thixotropic die-casting process for a magnesium alloy step to obtain a magnesium alloy step that is lightweight and meets various strength indicators, thereby reducing production costs.
[0004] An embodiment of the present invention provides a magnesium alloy stepwise semi-solid thixotropic die-casting process, which mainly includes the following steps:
[0005] S1. Raw material smelting: heating the magnesium alloy raw material to liquid state, making the liquid magnesium alloy non-dendritic, and forming a semi-solid slurry; casting the semi-solid slurry into an ingot, and cutting it into magnesium alloy particles as required;
[0006] S2, die casting: heating and melting the magnesium alloy particles to a semi-solid state, and injecting the semi-solid slurry into a die casting mold through a die casting machine for casting;
[0007] S3, mold opening and product removal: After the product is formed, the die-casting mold is opened and the slider is pulled out through the signal given by the die-casting machine, and the product is ejected;
[0008] S4. Product surface post-processing: remove burrs and flash on the product surface through post-processing grinding.
[0009] Optionally, the magnesium alloy raw material is AZ91D.
[0010] Optionally, the AZ91D comprises 8.3-9.7% Al, 0.15-0.5% Mn, 0.35-1.0% Zn, 0.1% Si, 0.03% Cu, 0.005% Fe, and the balance is Mg by weight.
[0011] Optionally, the die-casting mold is provided with an injection port, and the injection port is connected to the cavity inside the die-casting mold through a casting runner.
[0012] Optionally, the diameter of the injection port is 30 mm, the thickness of the inner gate is 3 mm, and the filling speed of the semi-solid slurry in the inner gate is 70 m / s.
[0013] Optionally, a slag ladle groove connected to the mold cavity is provided on a side of the mold cavity away from the injection port.
[0014] Optionally, during die-casting, the temperature of the die-casting mold is controlled at 220° C. by an oil temperature controller.
[0015] The embodiments of the present invention have the following beneficial effects:
[0016] 1. Magnesium alloy is used as the raw material. Compared with the traditional aluminum-silicon alloy raw material, magnesium alloy has the advantages of low density, high specific strength and specific stiffness, good damping and shock absorption performance, good heat dissipation performance, good regeneration, etc. It can effectively reduce the weight of the steps and reduce the production cost of the steps;
[0017] 2. The semi-solid thixotropic die-casting process is adopted. The semi-solid metal has better fluidity, which can better fill the mold cavity and reduce shrinkage holes and loose defects. The parts formed by the semi-solid thixotropic die-casting process have dense structure and high mechanical properties, which can effectively improve the service life of the steps. In addition, compared with the traditional liquid high-pressure die-casting process, the semi-solid thixotropic die-casting process has a lower casting temperature, which can save energy and reduce damage to the mold. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative work.
[0019] Figure 1 Comparison of the internal structures of liquid metal (left) and semi-solid metal (right);
[0020] Figure 2 It is a structural schematic diagram of a die-casting mold in an embodiment of the present invention;
[0021] The numbers in the figure represent:
[0022] 1. Injection port; 2. Casting runner; 3. Slag ladle trough; 4. Steps. DETAILED DESCRIPTION
[0023] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the present invention.
[0024] The embodiment of the present invention provides a semi-solid thixotropic die-casting process for magnesium alloy steps, which mainly includes the following steps:
[0025] S1. Raw material smelting: The magnesium alloy raw material is heated to liquid state, and the liquid magnesium alloy is non-dendriticized by stirring and other methods to form a semi-solid slurry; the semi-solid slurry is then cast into an ingot and cut into magnesium alloy particles of a certain size as required.
[0026] S2. Die casting: Heat and melt the magnesium alloy particles to a semi-solid state, and use a die casting machine to inject the semi-solid slurry into a die casting mold for casting. The magnesium alloy particles can be directly heated and melted by the heating structure of the die casting machine itself, and stored in the material chamber at the front end of the injection port, without the need for SF6 or other mixed gas protection.
[0027] S3, mold opening and part removal: After the product is formed, the die-casting mold is opened, the slider is cored out, and the product is ejected through the signal given by the die-casting machine.
[0028] S4. Post-processing of product surface: The surface of ejected products is often accompanied by flash and burrs, which need to be removed through post-processing and grinding.
[0029] Compared with the traditional aluminum silicon alloy raw material, magnesium alloy has the advantages of low density, high specific strength and specific stiffness, good damping and shock absorption performance, good heat dissipation performance, good regeneration, etc., which can effectively reduce the weight of the steps and reduce the production cost of the steps. Specifically, the magnesium alloy raw material can be selected from AZ91D, a material with good castability; for reference, AZ91D in the embodiment of the present invention includes a weight content of 8.3-9.7% Al, 0.15-0.5% Mn, 0.35-1.0% Zn, 0.1% Si, 0.03% Cu, 0.005% Fe, and the balance is Mg.
[0030] In the semi-solid state, the metal material is neither completely liquid nor completely solid, but a special state formed by solid particles suspended in liquid metal, such as Figure 1 As shown in the figure, due to the good fluidity of semi-solid metal, it can better fill the mold cavity and reduce shrinkage and loose defects. The parts formed by the semi-solid thixocasting process have dense structure and high mechanical properties, which can effectively improve the service life of the ladder; and compared with the traditional liquid high-pressure die-casting process, the semi-solid thixocasting process has a lower casting temperature, which can save energy and reduce mold damage.
[0031] In addition, the traditional die-casting mold needs to be modified before die-casting to make it suitable for the above-mentioned semi-solid thixotropic die-casting process. Figure 2As shown, the modified die-casting mold is provided with an injection port 1, which is connected to the cavity inside the die-casting mold through a casting runner 2, so as to change the traditional cake feeding method into an injection molding method. A slag bag groove 3 connected to the cavity is also provided on the side of the cavity away from the injection port 1. The slag bag groove 3 can not only accommodate impurities such as water vapor, slag and release agent, but also play a certain exhaust role, effectively reducing air pockets in the part and avoiding the problem of insufficient casting. After the die-casting step 4 is taken out, the runner and slag bag need to be trimmed to remove.
[0032] Specifically, the die-casting machine can adopt the Buhler horizontal die-casting machine imported from Switzerland, with a slow average speed of 0.3m / s, a high-speed injection speed of 6m / s, an injection pressure of 260bar, a boost pressure building time of 40ms, a boost pressure of 650bar, and a clamping force of 2800T.
[0033] The diameter of the injection port 1 on the die-casting mold is 30 mm, the thickness of the inner gate is 3 mm, and the filling speed of the semi-solid slurry in the inner gate is 70 m / s to ensure the quality of the stepped molding.
[0034] During die-casting, the temperature of the die-casting mold is best controlled at around 220°C by an oil temperature controller; when opening the mold and taking out the parts, a robot can be used to automatically spray the release agent.
[0035] This document uses specific examples to illustrate the principles and implementation methods of the present invention. The description of the above embodiments is only used to help understand the technical solutions and core ideas of the present invention. Ordinary technicians in this field should understand that they can still modify the technical solutions recorded in the aforementioned embodiments, or replace some of the technical features therein with equivalents; and these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A semi-solid thixotropic die-casting process for magnesium alloy steps, characterized in that: The following steps are involved: S1. Raw material smelting: heating the magnesium alloy raw material to liquid state, making the liquid magnesium alloy non-dendritic, and forming a semi-solid slurry; casting the semi-solid slurry into an ingot, and cutting it into magnesium alloy particles as required; S2, die casting: heating and melting the magnesium alloy particles to a semi-solid state, and injecting the semi-solid slurry into a die casting mold through a die casting machine for casting; S3, mold opening and product removal: After the product is formed, the die-casting mold is opened and the slider is pulled out through the signal given by the die-casting machine, and the product is ejected; S4. Product surface post-processing: remove burrs and flash on the product surface through post-processing grinding.
2. The semi-solid thixotropic die-casting process of magnesium alloy step according to claim 1, characterized in that: The magnesium alloy raw material is AZ91D.
3. The semi-solid thixotropic die-casting process of magnesium alloy step according to claim 2, characterized in that: The AZ91D comprises 8.3-9.7% Al, 0.15-0.5% Mn, 0.35-1.0% Zn, 0.1% Si, 0.03% Cu, 0.005% Fe, and the balance Mg by weight.
4. The semi-solid thixotropic die-casting process of magnesium alloy step according to claim 1, characterized in that: The die-casting mold is provided with an injection port, and the injection port is connected with the cavity inside the die-casting mold through a casting flow channel.
5. The semi-solid thixotropic die-casting process of magnesium alloy step according to claim 4, characterized in that: The diameter of the injection port is 30 mm, the thickness of the inner gate is 3 mm, and the filling speed of the semi-solid slurry in the inner gate is 70 m / s.
6. The semi-solid thixotropic die-casting process of magnesium alloy step according to claim 4, characterized in that: A slag ladle groove communicated with the mold cavity is provided on one side of the mold cavity away from the injection port.
7. The semi-solid thixotropic die-casting process of magnesium alloy step according to claim 4, characterized in that: During die casting, the temperature of the die casting mold is controlled at 220° C. by an oil temperature controller.
Citation Information
Cited By
Semi-solid forming process for magnesium-aluminum alloy part of intelligent glasses
CN121874531A