High-barrier high-temperature-resistant food-grade film as well as preparation method and application thereof

By using flexible enhanced gap penetration dendrimer as the intermediate adhesive layer in food-grade films, the problem of reduced flexibility caused by improved barrier performance is solved, and the effect of high barrier properties and flexibility is achieved, suitable for high temperature oil-resistant vacuum bag.

CN119036975AActive Publication Date: 2024-11-29SICHUAN GUSHUO NEW MATERIAL CO LTD

Patent Information

Application Number
CN202411203996.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-11-29
Estimated Expiration
2044-08-30

AI Technical Summary

Technical Problem

When improving the barrier properties of food-grade films, the prior art leads to a significant reduction in film flexibility, affecting the density of food packaging, especially vacuum packaging bags.

Method used

Using flexible reinforced gap-permeable dendritic polymer as the intermediate adhesive layer, mono-octyl α-cyanoacrylate, bio-methacrylate, 3-mercaptopropyltriethoxysilane and diethyl hydroxylamine. The body is prepared by divergence and convergence method to form a highly branched dendritic polymer, fills the thin film gaps and forms a dense barrier layer, improving barrier properties without reducing flexibility.

Benefits of technology

A food-grade film with high barrier properties and flexibility is achieved, maintaining a long-term and stable barrier effect, and ensuring that the polymer has excellent flexibility and strength through reasonable combination and reaction control.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119036975A_ABST
    Figure CN119036975A_ABST
Patent Text Reader

Abstract

The invention discloses a high-barrier high-temperature-resistant food-grade thin film and a preparation method and application thereof, and belongs to the field of plastic thin films, the high-barrier high-temperature-resistant food-grade thin film comprises an outer-layer thin film, a middle adhesive layer and an inner-layer thin film, the flexibility-enhanced gap permeation dendritic polymer is prepared by taking alpha-cyanoacrylate n-octyl ester as an initial core molecule, bio-based methacrylate as a main monomer, 3-mercaptopropyltriethoxysilane as a flexible chain segment monomer, diethyl hydroxylamine as an enhancing monomer and BPO as an initiator through a one-step polymerization method. DEVB is used as a cross-linking agent, and the dendritic polymer is prepared through a divergence method and a convergence method. The film prepared by the preparation method disclosed by the invention has relatively strong barrier property and relatively good flexibility.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of plastic films, and relates to a high-barrier, high-temperature-resistant food-grade film and a preparation method and application thereof. Background Art

[0002] Food-grade films in food packaging need to have both high temperature resistance and high barrier properties to meet the safety and quality requirements of food during processing, storage and transportation, especially the vacuum packaging of high-temperature oil substances.

[0003] When improving the barrier properties of the film, aluminum plating, surface coating (nanomaterials, inorganic substances), etc. are generally used at present. Although they can effectively improve the barrier properties of the film, they will also significantly reduce the flexibility of the film. If the film has low flexibility, it cannot fit the food, affecting the density of the food packaging, especially the vacuum packaging bag. Summary of the invention

[0004] The purpose of the present invention is to provide a high-barrier and high-temperature resistant food-grade film and a preparation method and application thereof, which solves the problem that the flexibility of the film is significantly reduced when the barrier performance of the film is improved.

[0005] The technical solution adopted by the present invention is as follows:

[0006] A high-barrier, high-temperature-resistant food-grade film, comprising an outer film, an intermediate adhesive layer, and an inner film, wherein the intermediate adhesive layer is a flexible, enhanced gap-penetrating dendritic polymer, and the flexible, enhanced gap-penetrating dendritic polymer is a dendritic polymer prepared by a divergent method and a convergent method using α-octyl cyanoacrylate as an initial core molecule, bio-based methacrylate as a main monomer, 3-mercaptopropyltriethoxysilane as a flexible segment monomer, diethylhydroxylamine as a reinforcing monomer, BPO as an initiator, and DEVB as a crosslinking agent;

[0007] The mass ratio of α-octyl cyanoacrylate is 10%, the mass ratio of bio-based methacrylate is 45%, the mass ratio of 3-mercaptopropyltriethoxysilane is 20%, the mass ratio of diethylhydroxylamine is 10%, the mass ratio of BPO is 5%, and the mass ratio of DEVB is 10%.

[0008] The present invention selects n-octyl α-cyanoacrylate as the initial core molecule due to its property of rapid polymerization when it meets water and has an anionic surface. This property enables it to quickly and stably form a core structure in the initial stage of forming a dendritic polymer, providing a solid foundation for subsequent polymerization reactions. n-octyl α-cyanoacrylate is used as the initial core molecule, and the cyano and acrylic acid groups in its structure provide high reactivity, so that the polymerization reaction can be quickly started under the action of the initiator BPO to form a stable polymerization core; bio-based methacrylate is used as the main monomer, and is connected to the core molecule through a free radical polymerization reaction to form the main chain of the polymer. The source not only makes the polymer environmentally friendly, but also copolymerizes with other monomers through its methacrylate group to enhance the overall performance of the polymer; 3-mercaptopropyltriethoxysilane is used as a flexible segment monomer, and the sulfide bonds and silicon-oxygen bonds in its structure provide good flexibility. During the polymerization process, these flexible segments are introduced into the polymer to form side chains or hanging chains, thereby increasing the flexibility and permeability of the polymer; diethylhydroxylamine is used as a reinforcing monomer, and the nitrogen-oxygen bonds in its molecular structure can form hydrogen bonds or dipole-dipole interactions with other groups on the polymer chain, thereby enhancing the interaction force between polymer molecules and improving the strength and hardness of the polymer.

[0009] Under the action of BPO initiator, α-octyl cyanoacrylate first undergoes free radical polymerization to form a polymer core. Subsequently, monomers such as bio-based methacrylate and 3-mercaptopropyltriethoxysilane are added to the reaction system in sequence to copolymerize with the core molecule or the formed polymer chain; diethylhydroxylamine participates in the reaction as a reinforcing monomer to enhance the overall performance of the polymer through its intermolecular interaction; finally, the DEVB crosslinker connects different polymer chains to form a three-dimensional network structure.

[0010] Since the flexibility-enhanced gap-penetrating dendrimer has a highly branched structure and rich functional groups, its molecular chain can penetrate into the tiny gaps of the film. After forming a continuous covering layer on the surface of the film, the polymer branched chain can fill the gaps and form a dense barrier layer, effectively preventing the penetration of gases, liquids and other substances. In addition, the flexibility and permeability of the polymer molecular chain enable it to adapt to the slight deformation of the film without breaking or falling off, thereby maintaining a long-term and stable barrier effect.

[0011] The reason why the flexibility-enhanced gap-penetrating dendrimer has excellent flexibility is mainly due to the flexible segment monomer (3-mercaptopropyltriethoxysilane) in its molecular structure. These flexible segments form many hanging chains or branches in the polymer, which enable the polymer chain to bend and twist to a certain extent when subjected to external forces, thereby maintaining overall flexibility. At the same time, the addition of diethylhydroxylamine reinforcing monomers improves the interaction between polymer molecules, so that the polymer has high strength and hardness while maintaining flexibility; although the flexibility-enhanced gap-penetrating dendrimer has high strength and hardness, its flexibility is not affected, which is mainly due to the reasonable ratio of flexible segment monomers and reinforcing monomers in the polymer molecules and the interaction between them. The flexible segment monomers give the polymer good flexibility and elasticity, while the reinforcing monomers maintain the overall mechanical properties of the polymer by increasing the interaction between molecules. The balance between the two allows the polymer to maintain high strength while still having good flexibility; therefore, since the intermediate adhesive layer of the present invention has good flexibility, after its side chains penetrate into the gap between the outer film and the inner film, it will not significantly reduce the flexibility of the outer film and the inner film, and thus will not significantly reduce the overall flexibility of the high barrier and high temperature resistant food-grade film.

[0012] Furthermore, the flexibility-enhanced gap-penetrating dendrimer is prepared by the following method:

[0013] S1. Under nitrogen protection, dissolving α-octyl cyanoacrylate in tetrahydrofuran to obtain α-octyl cyanoacrylate solution, adding 20% ​​by mass of bio-based methacrylate to the α-octyl cyanoacrylate solution, then stirring and heating to 60° C., adding 1% of BPO initiator, and reacting at 60° C. for 12 hours to obtain a first-generation dendritic polymer;

[0014] S2, mixing bio-based methacrylate, 3-mercaptopropyltriethoxysilane and diethylhydroxylamine in proportion to form a prepolymerization system;

[0015] S3, dissolving the remaining 4% of the initiator BPO in the bio-based methacrylate to obtain an initiator solution;

[0016] S4, slowly adding the prepolymer system obtained in step S2 to the first generation dendritic polymer obtained in step S1, stirring and heating to 80° C., adding the initiator solution obtained in step S3, and continuing to stir and react for 6 hours to obtain the dendritic polymer;

[0017] S5. Add 5% by weight of crosslinking agent DEVB to the dendritic polymer obtained in step S4, and continue to react at 80° C. with stirring for 30-60 minutes to converge the network structure and obtain a gap-penetrating dendritic polymer with enhanced flexibility.

[0018] The present invention adopts a divergent method and a convergent method; the divergent method: starting from the core of α-octyl cyanoacrylate, gradually adding monomers such as bio-based methacrylate and 3-mercaptopropyltriethoxysilane to the outside to form a dendritic structure. As the reaction proceeds, the polymer chain continues to grow, and the number of branches gradually increases to form a highly branched structure. The convergent method: based on the divergent method, a cross-linking agent is used to connect the polymer chains to form a complete three-dimensional network structure. This method helps to control the final morphology and performance of the polymer, ensuring that the polymer has excellent flexibility, strength and barrier properties.

[0019] Furthermore, the outer film comprises the following components in parts by weight: 60 parts of linear low-density polyethylene, 5 parts of light stabilizer, 5 parts of lubricant, 5 parts of antistatic agent, and 30 parts of ethylene-vinyl acetate copolymer.

[0020] The outer layer film of the present invention combines the strength and toughness of LLDPE, the transparency and temperature resistance of EVA, the light aging protection of the light stabilizer, the processing performance improvement of the lubricant and the antistatic effect of the antistatic agent to form a film material with excellent comprehensive performance, which is suitable for the complex environment of the outer layer.

[0021] Furthermore, the inner film comprises the following components in parts by weight: 50 parts of high-density polyethylene, 35 parts of ethylene-vinyl acetate copolymer, and 10 parts of nano-silicon dioxide.

[0022] The inner film is in direct contact with food and needs to have good high temperature resistance. Therefore, the present invention adds nano silicon dioxide to the polyethylene film, which helps to improve the high temperature resistance of the film.

[0023] Furthermore, the light stabilizer is a hindered amine light stabilizer HALS, the lubricant is erucamide, and the antistatic agent is amide phosphate.

[0024] Furthermore, the total thickness of the outer film, the middle adhesive layer and the inner film is 0.28 mm, wherein the thickness of the outer film is 0.12 mm, the thickness of the inner film is 0.1 mm, and the thickness of the middle adhesive layer is 0.06 mm.

[0025] In actual use, the present invention optimizes the thickness of each layer.

[0026] The method for preparing a high-barrier and high-temperature resistant food-grade film comprises the following steps:

[0027] A. Preparing an outer film material: melt-blending 60 parts of linear low-density polyethylene, 5 parts of a light stabilizer, 5 parts of a lubricant, 5 parts of an antistatic agent, and 30 parts of an ethylene-vinyl acetate copolymer to obtain an outer film material;

[0028] B. Preparation of inner film material: melt blending 50 parts of high-density polyethylene, 35 parts of ethylene-vinyl acetate copolymer, and 10 parts of nano-silicon dioxide to obtain the inner film material;

[0029] C. Preparation of intermediate adhesive layer materials:

[0030] S1. Under nitrogen protection, dissolving α-octyl cyanoacrylate in tetrahydrofuran to obtain α-octyl cyanoacrylate solution, adding 20% ​​by mass of bio-based methacrylate to the α-octyl cyanoacrylate solution, then stirring and heating to 60° C., adding 1% of BPO initiator, and reacting at 60° C. for 12 hours to obtain a first-generation dendritic polymer;

[0031] S2, mixing bio-based methacrylate, 3-mercaptopropyltriethoxysilane and diethylhydroxylamine in proportion to form a prepolymerization system;

[0032] S3, dissolving the remaining 4% of the initiator BPO in the bio-based methacrylate to obtain an initiator solution;

[0033] S4, slowly adding the prepolymer system obtained in step S2 to the first generation dendritic polymer obtained in step S1, stirring and heating to 80° C., adding the initiator solution obtained in step S3, and continuing to stir and react for 6 hours to obtain the dendritic polymer;

[0034] S5, adding 5% by weight of a crosslinking agent DEVB to the dendritic polymer obtained in step S4, and continuing to react at 80° C. with stirring for 30-60 minutes to converge the network structure, thereby obtaining a gap-penetrating dendritic polymer with enhanced flexibility;

[0035] D. Use a multi-layer co-extrusion film blowing machine to co-extrude, compound, and blow-form the outer film material, the middle adhesive layer material, and the inner film material to obtain a high-barrier and high-temperature resistant food-grade film with a three-layer structure, wherein the high-barrier and high-temperature resistant food-grade film includes an outer film, a middle adhesive layer, and an inner film.

[0036] Furthermore, the multi-layer co-extrusion film blowing machine adopts a GY-1600SB multi-layer co-extrusion film blowing machine.

[0037] Furthermore, the reaction time of S5 is 45 minutes.

[0038] The high-barrier and high-temperature-resistant food-grade film is used as a high-temperature and oil-resistant vacuum bag in the food field.

[0039] In summary, due to the adoption of the above technical solution, the beneficial effects of the present invention are:

[0040] 1. In a high-barrier and high-temperature resistant food-grade film, the gap-penetrating dendritic polymer with enhanced flexibility has a highly branched structure and rich functional groups, and its molecular chain can penetrate into the tiny gaps of the film. After forming a continuous covering layer on the surface of the film, the polymer branch chains can fill the gaps and form a dense barrier layer, effectively preventing the penetration of gases, liquids and other substances. Therefore, the present invention uses the gap-penetrating dendritic polymer with enhanced flexibility as the intermediate adhesive layer, which can effectively improve the barrier properties of the outer film and the inner film, replacing the existing method of improving the barrier properties by coating inorganic substances.

[0041] 2. The flexibility and permeability of the polymer molecular chain in the flexible gap-penetrating dendritic polymer of the present invention enable it to adapt to the slight deformation of the film without being easily broken or falling off, thereby maintaining a long-term and stable barrier effect;

[0042] 3. The middle adhesive layer of the present invention has good flexibility. After its side chains penetrate into the gap between the outer film and the inner film, the flexibility of the outer film and the inner film will not be significantly reduced, and thus the overall flexibility of the high barrier and high temperature resistant food grade film will not be significantly reduced;

[0043] 4. The present invention adopts a combination of divergent method and convergent method to prepare flexibility-enhanced gap-penetrating dendritic polymer, which helps to control the final morphology and performance of the polymer and ensure that the polymer has excellent flexibility and strength. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the following briefly introduces the drawings required for use in the embodiments. It should be understood that the following drawings only illustrate certain embodiments of the present invention and should not be regarded as limiting the scope. For those skilled in the art, other related drawings can be obtained based on these drawings without creative work, among which:

[0045] Figure 1 This is a SEM image of a high-barrier, high-temperature-resistant food-grade film. DETAILED DESCRIPTION

[0046] In order to make the purpose, technical scheme and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention, that is, the embodiments described are only part of the embodiments of the present invention, rather than all of the embodiments. The components of the embodiments of the present invention described and shown in the drawings herein can be arranged and designed in various different configurations.

[0047] Therefore, the following detailed description of the embodiments of the present invention provided in the accompanying drawings is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without making creative work are within the scope of protection of the present invention.

[0048] It should be noted that relational terms such as "first" and "second" are used only to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise a ..." do not exclude the existence of other identical elements in the process, method, article or device including the elements.

[0049] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.

[0050] Example 1

[0051] A high-barrier, high-temperature-resistant food-grade film provided by a preferred embodiment of the present invention comprises an outer film, an intermediate adhesive layer, and an inner film, wherein the intermediate adhesive layer is a flexible enhanced gap-penetrating dendritic polymer, and the flexible enhanced gap-penetrating dendritic polymer is a dendritic polymer prepared by a divergent method and a convergent method using α-octyl cyanoacrylate as an initial core molecule, bio-based methacrylate as a main monomer, 3-mercaptopropyltriethoxysilane as a flexible segment monomer, diethylhydroxylamine as a reinforcing monomer, BPO as an initiator, and DEVB as a cross-linking agent;

[0052] The mass ratio of α-octyl cyanoacrylate is 10%, the mass ratio of bio-based methacrylate is 45%, the mass ratio of 3-mercaptopropyltriethoxysilane is 20%, the mass ratio of diethylhydroxylamine is 10%, the mass ratio of BPO is 5%, and the mass ratio of DEVB is 10%.

[0053] The flexibility-enhanced gap-penetrating dendrimer is prepared by the following method:

[0054] S1. Under nitrogen protection, dissolving α-octyl cyanoacrylate in tetrahydrofuran to obtain α-octyl cyanoacrylate solution, adding 20% ​​by mass of bio-based methacrylate to the α-octyl cyanoacrylate solution, then stirring and heating to 60° C., adding 1% of BPO initiator, and reacting at 60° C. for 12 hours to obtain a first-generation dendritic polymer;

[0055] S2, mixing bio-based methacrylate, 3-mercaptopropyltriethoxysilane and diethylhydroxylamine in proportion to form a prepolymerization system;

[0056] S3, dissolving the remaining 4% of the initiator BPO in the bio-based methacrylate to obtain an initiator solution;

[0057] S4, slowly adding the prepolymer system obtained in step S2 to the first generation dendritic polymer obtained in step S1, stirring and heating to 80° C., adding the initiator solution obtained in step S3, and continuing to stir and react for 6 hours to obtain the dendritic polymer;

[0058] S5. Add 5% by weight of crosslinking agent DEVB to the dendritic polymer obtained in step S4, and continue to stir and react at 80° C. for 30 minutes to converge the network structure and obtain a gap-penetrating dendritic polymer with enhanced flexibility.

[0059] The outer film comprises the following components in parts by weight: 60 parts of linear low-density polyethylene, 5 parts of light stabilizer, 5 parts of lubricant, 5 parts of antistatic agent, and 30 parts of ethylene-vinyl acetate copolymer.

[0060] The inner film comprises the following components in parts by weight: 50 parts of high-density polyethylene, 35 parts of ethylene-vinyl acetate copolymer, and 10 parts of nano silicon dioxide.

[0061] The light stabilizer is a hindered amine light stabilizer HALS, the lubricant is erucamide, and the antistatic agent is amide phosphate.

[0062] The total thickness of the outer film, the middle adhesive layer and the inner film is 0.28 mm, of which the thickness of the outer film is 0.12 mm, the thickness of the inner film is 0.1 mm, and the thickness of the middle adhesive layer is 0.06 mm.

[0063] The above-mentioned method for preparing a high-barrier and high-temperature resistant food-grade film comprises the following steps:

[0064] A. Preparation of outer film material: melt blending 60 parts of linear low-density polyethylene, 5 parts of light stabilizer, 5 parts of lubricant, 5 parts of antistatic agent and 30 parts of ethylene-vinyl acetate copolymer to obtain outer film material;

[0065] B. Preparation of inner film material: melt blending 50 parts of high-density polyethylene, 35 parts of ethylene-vinyl acetate copolymer, and 10 parts of nano-silicon dioxide to obtain the inner film material;

[0066] C. Preparation of intermediate adhesive layer materials:

[0067] S1. Under nitrogen protection, dissolving α-octyl cyanoacrylate in tetrahydrofuran to obtain α-octyl cyanoacrylate solution, adding 20% ​​by mass of bio-based methacrylate to the α-octyl cyanoacrylate solution, then stirring and heating to 60° C., adding 1% of BPO initiator, and reacting at 60° C. for 12 hours to obtain a first-generation dendritic polymer;

[0068] S2, mixing bio-based methacrylate, 3-mercaptopropyltriethoxysilane and diethylhydroxylamine in proportion to form a prepolymerization system;

[0069] S3, dissolving the remaining 4% of the initiator BPO in the bio-based methacrylate to obtain an initiator solution;

[0070] S4, slowly adding the prepolymer system obtained in step S2 to the first generation dendritic polymer obtained in step S1, stirring and heating to 80° C., adding the initiator solution obtained in step S3, and continuing to stir and react for 6 hours to obtain the dendritic polymer;

[0071] S5, adding 5% by weight of a crosslinking agent DEVB to the dendritic polymer obtained in step S4, and continuing to react at 80° C. with stirring for 30 minutes to converge the network structure, thereby obtaining a gap-penetrating dendritic polymer with enhanced flexibility;

[0072] D. Use a multi-layer co-extrusion film blowing machine to co-extrude, compound, and blow-form the outer film material, the middle adhesive layer material, and the inner film material to obtain a high-barrier and high-temperature resistant food-grade film with a three-layer structure, wherein the high-barrier and high-temperature resistant food-grade film includes an outer film, a middle adhesive layer, and an inner film.

[0073] The multi-layer co-extrusion film blowing machine adopts a GY-1600SB multi-layer co-extrusion film blowing machine.

[0074] Figure 1 This is a SEM image of the outer surface of the high-barrier, high-temperature-resistant food-grade film prepared in the present invention. It can be clearly seen from the image that there are fillers in the pores in the film, and the barrier performance is enhanced after the fillers are in the pores.

[0075] Example 2

[0076] This embodiment is based on the embodiment 1. The difference between this embodiment and the embodiment 1 is that the reaction time in step S5 of this embodiment is 45 minutes.

[0077] Example 3

[0078] This embodiment is based on the embodiment 1. The difference between this embodiment and the embodiment 1 is that the reaction time in step S5 of this embodiment is 60 minutes.

[0079] Comparative Example 1

[0080] Based on Example 1, this comparative example is different from Example 1 in that the mass ratio of α-octyl cyanoacrylate in the comparative example is 10%, the mass ratio of bio-based methacrylate is 45%, the mass ratio of 3-mercaptopropyltriethoxysilane is 10%, the mass ratio of diethylhydroxylamine is 10%, the mass ratio of BPO is 5%, and the mass ratio of DEVB is 10%.

[0081] Comparative Example 2

[0082] Based on Example 1, this comparative example is different from Example 1 in that the mass ratio of α-octyl cyanoacrylate in the comparative example is 10%, the mass ratio of bio-based methacrylate is 45%, the mass ratio of 3-mercaptopropyltriethoxysilane is 15%, the mass ratio of diethylhydroxylamine is 5%, the mass ratio of BPO is 5%, and the mass ratio of DEVB is 10%.

[0083] Comparative Example 3

[0084] Based on Example 1, the difference between this comparative example and Example 1 is that the high barrier and high temperature resistant food grade film in this comparative example does not include an intermediate adhesive layer.

[0085] Comparative Example 4

[0086] Based on Example 1, the difference between this comparative example and Example 1 is that the intermediate adhesive layer in this comparative example does not include 3-mercaptopropyltriethoxysilane.

[0087] Comparative Example 5

[0088] Based on Example 1, the difference between this comparative example and Example 1 is that the intermediate adhesive layer in this comparative example does not include diethylhydroxylamine.

[0089] Comparative Example 6

[0090] Based on Example 1, this comparative example is different from Example 1 in that the intermediate adhesive layer in this comparative example does not include bio-based methacrylate.

[0091] Comparative Example 7

[0092] Based on Example 1, the difference between this comparative example and Example 1 is that the reaction time in step S5 in this comparative example is 65 minutes.

[0093] Comparative Example 8

[0094] Based on Example 1, the difference between this comparative example and Example 1 is that the reaction time in step S5 in this comparative example is 25 minutes.

[0095] Test Example 1

[0096] The tensile strength, elongation at break, hardness, thermal weight loss temperature, and glass transition temperature (Tg) of the flexible enhanced gap-penetrating dendritic polymers prepared in Examples 1-3 and Comparative Examples 1, 2, 4, 5, 6, 7, and 8 after curing were tested; the test results are shown in Table 1.

[0097] The detection methods of tensile strength, elongation at break, hardness, thermal weight loss temperature and glass transition temperature of the flexible enhanced gap infiltration dendritic polymer after curing are prior art and will not be elaborated in detail here.

[0098] Table 1 Performance test of flexible enhanced gap-penetrating dendrimer after curing

[0099]

[0100]

[0101] Test Example 2

[0102] The porosity and elongation at break of the high barrier and high temperature resistant food grade films prepared in Examples 1-3 and Comparative Examples 1-8 were tested. The test results are shown in Table 2.

[0103] Table 2 Test results of high barrier and high temperature resistant food grade films

[0104]

[0105]

[0106] Combining the data in Table 1 and Table 2, Example 2 of the present invention is the best ratio, and its flexibility and mechanical strength are balanced, with both high mechanical strength and good flexibility; comparing Comparative Example 3 with Example 2, the present invention does reduce the overall flexibility of the film after adding the intermediate adhesive layer, but the degree of reduction is small, indicating that the intermediate adhesive layer of the present invention has little effect on the overall flexibility of the film. Combining the porosity in Table 2 of the present invention, the porosity of the film of the present invention is less than 5%, indicating that it has strong barrier properties; comparing Comparative Example 3 with Example 2, the present invention adds the intermediate adhesive layer, and the porosity is reduced, indicating that the intermediate adhesive layer of the present invention can significantly improve the barrier properties of the film.

[0107] The above description is only a preferred embodiment of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions and improvements made by any technician familiar with the field within the spirit and principle of the present invention should be included in the scope of protection of the present invention.

Claims

1. A high barrier and high temperature resistant food grade film, comprising an outer film, an intermediate adhesive layer, and an inner film, characterized in that: The intermediate adhesive layer is a gap-penetrating dendrimer with enhanced flexibility, which is a dendrimer prepared by a divergent method and a convergent method using octyl α-cyanoacrylate as an initial core molecule, bio-based methacrylate as a main monomer, 3-mercaptopropyltriethoxysilane as a flexible segment monomer, diethylhydroxylamine as a reinforcing monomer, BPO as an initiator, and DEVB as a cross-linking agent; The mass ratio of α-octyl cyanoacrylate is 10%, the mass ratio of bio-based methacrylate is 45%, the mass ratio of 3-mercaptopropyltriethoxysilane is 20%, the mass ratio of diethylhydroxylamine is 10%, the mass ratio of BPO is 5%, and the mass ratio of DEVB is 10%.

2. The high barrier and high temperature resistant food grade film according to claim 1, characterized in that: The flexibility-enhanced gap-penetrating dendrimer is prepared by the following method: S1. Under nitrogen protection, dissolving α-octyl cyanoacrylate in tetrahydrofuran to obtain α-octyl cyanoacrylate solution, adding 20% ​​by mass of bio-based methacrylate to the α-octyl cyanoacrylate solution, then stirring and heating to 60° C., adding 1% of BPO initiator, and reacting at 60° C. for 12 hours to obtain a first-generation dendritic polymer; S2, mixing bio-based methacrylate, 3-mercaptopropyltriethoxysilane and diethylhydroxylamine in proportion to form a prepolymerization system; S3, dissolving the remaining 4% of the initiator BPO in the bio-based methacrylate to obtain an initiator solution; S4, slowly adding the prepolymer system obtained in step S2 to the first generation dendritic polymer obtained in step S1, stirring and heating to 80° C., adding the initiator solution obtained in step S3, and continuing to stir and react for 6 hours to obtain the dendritic polymer; S5. Add 5% by weight of crosslinking agent DEVB to the dendritic polymer obtained in step S4, and continue to react at 80° C. with stirring for 30-60 minutes to converge the network structure and obtain a gap-penetrating dendritic polymer with enhanced flexibility.

3. The high barrier and high temperature resistant food grade film according to claim 1, characterized in that: The outer film comprises the following components in parts by weight: 60 parts of linear low-density polyethylene, 5 parts of light stabilizer, 5 parts of lubricant, 5 parts of antistatic agent, and 30 parts of ethylene-vinyl acetate copolymer.

4. The high barrier and high temperature resistant food grade film according to claim 1, characterized in that: The inner film comprises the following components in parts by weight: 50 parts of high-density polyethylene, 35 parts of ethylene-vinyl acetate copolymer, and 10 parts of nano silicon dioxide.

5. The high barrier and high temperature resistant food grade film according to claim 3, characterized in that: The light stabilizer is a hindered amine light stabilizer HALS, the lubricant is erucamide, and the antistatic agent is amide phosphate.

6. The high barrier and high temperature resistant food grade film according to claim 1, characterized in that: The total thickness of the outer film, the middle adhesive layer and the inner film is 0.28 mm, of which the thickness of the outer film is 0.12 mm, the thickness of the inner film is 0.1 mm, and the thickness of the middle adhesive layer is 0.06 mm.

7. A method for preparing a high barrier and high temperature resistant food grade film according to any one of claims 1 to 6, characterized in that: The following steps are involved: A. Preparation of outer film material: melt blending 60 parts of linear low-density polyethylene, 5 parts of light stabilizer, 5 parts of lubricant, 5 parts of antistatic agent and 30 parts of ethylene-vinyl acetate copolymer to obtain outer film material; B. Preparation of inner film material: melt blending 50 parts of high-density polyethylene, 35 parts of ethylene-vinyl acetate copolymer, and 10 parts of nano-silicon dioxide to obtain the inner film material; C. Preparation of intermediate adhesive layer materials: S1. Under nitrogen protection, dissolving α-octyl cyanoacrylate in tetrahydrofuran to obtain α-octyl cyanoacrylate solution, adding 20% ​​by mass of bio-based methacrylate to the α-octyl cyanoacrylate solution, then stirring and heating to 60° C., adding 1% of BPO initiator, and reacting at 60° C. for 12 hours to obtain a first-generation dendritic polymer; S2, mixing bio-based methacrylate, 3-mercaptopropyltriethoxysilane and diethylhydroxylamine in proportion to form a prepolymerization system; S3, dissolving the remaining 4% of the initiator BPO in the bio-based methacrylate to obtain an initiator solution; S4, slowly adding the prepolymer system obtained in step S2 to the first generation dendritic polymer obtained in step S1, stirring and heating to 80° C., adding the initiator solution obtained in step S3, and continuing to stir and react for 6 hours to obtain the dendritic polymer; S5, adding 5% by weight of a crosslinking agent DEVB to the dendritic polymer obtained in step S4, and continuing to react at 80° C. with stirring for 30-60 minutes to converge the network structure, thereby obtaining a gap-penetrating dendritic polymer with enhanced flexibility; D. Use a multi-layer co-extrusion film blowing machine to co-extrude, compound, and blow-form the outer film material, the middle adhesive layer material, and the inner film material to obtain a high-barrier and high-temperature resistant food-grade film with a three-layer structure, wherein the high-barrier and high-temperature resistant food-grade film includes an outer film, a middle adhesive layer, and an inner film.

8. The method for preparing a high barrier and high temperature resistant food grade film according to claim 7, characterized in that: The multi-layer co-extrusion film blowing machine adopts a GY-1600SB multi-layer co-extrusion film blowing machine.

9. The method for preparing a high barrier and high temperature resistant food grade film according to claim 7, characterized in that: The reaction time of S5 is 45 minutes.

10. The use of a high barrier and high temperature resistant food grade film according to claim 1, characterized in that: The high-barrier and high-temperature-resistant food-grade film is used as a high-temperature and oil-resistant vacuum bag in the food field.

Citation Information

Patent Citations

  • Encapsulation barrier stack comprising dendrimer encapsulated nanoparticles

    AU2014260477A1

  • Bio-based high-barrier two-way stretch polyester film with good toughness and preparation method of bio-based high-barrier two-way stretch polyester film

    CN117601539A

  • High-barrier polyvinyl alcohol biaxially oriented film and preparation method thereof

    CN118288653A

  • Improvements in or relating to hollow articles

    GB0005664D0

  • Thermally-conductive polymer and components

    US20210016542A1

Cited By

  • Recyclable high-barrier anti-ultraviolet composite film and food packaging bag

    CN120116574A