Flaky porous cobalt chloride, single-crystal cobaltosic oxide, single-crystal lithium cobalt oxide and preparation method and application thereof

Sintered metal mixture by spray drying to generate efficient sheet-like porous cobalt chloride, which solves the problems of complex processes and high cost in the prior art, realizes efficient and economical preparation of porous cobalt chloride, and improves lithium ions Diffusion and battery performance.

CN119038623AActive Publication Date: 2024-11-29GUANGDONG BRUNP RECYCLING TECH CO LTD +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411157854.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-29
Estimated Expiration
2044-08-22

AI Technical Summary

Technical Problem

The prior art is difficult to synthesize sheet-like porous cobalt chloride by co-precipitation, and the template method is complex and has high cost, so no industrial application is seen.

Method used

The metal mixture is sintered by spray drying to form a precursor with a hollow structure, and then sintered under specific temperature and time conditions to generate a sheet-like porous cobalt chloride with high tap density, specific surface area and pore volume, and further use In the preparation of single-crystal cobalt tetroxide and single-crystal lithium cobalt oxide.

Benefits of technology

It realizes efficient preparation of sheet-like porous cobalt chloride, simplifies the process flow, reduces production costs, improves lithium ion diffusion uniformity and electrochemical performance, and enhances the sintering activity and battery performance of the cathode material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119038623A_ABST
    Figure CN119038623A_ABST
Patent Text Reader

Abstract

The invention discloses flaky porous cobalt chloride, single-crystal cobaltosic oxide, single-crystal lithium cobalt oxide and a preparation method and application thereof, and belongs to the technical field of battery materials. The chemical formula of the flaky porous cobalt chloride is MxCo1-xCl2, x is more than or equal to 0 and less than or equal to 0.5, and M is a metal element except cobalt; the tap density of the flaky porous cobalt chloride is not lower than 1g / cm < 3 >, the specific surface area is not lower than 1.8 m < 2 > / g, the Dv10 is not lower than 4.5 microns, the Dv50 is not lower than 8.5 microns, and the Dv90 is not lower than 20 microns. The flaky porous cobalt chloride has relatively high tap density, relatively large specific surface area and pore volume and relatively uniform pore diameter, and is beneficial to increase of sintering activity, and when the flaky porous cobalt chloride is mixed with a lithium source for calcination, the flaky porous structure is also beneficial to uniform diffusion of lithium ions into a bulk phase of the material, so that the lithium ions are more uniformly distributed, and the performance of the material is improved. Further, the electrochemical performance of the positive electrode material and the battery is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of battery materials, and in particular to a sheet-like porous cobalt chloride, a single-crystal cobalt oxide, a single-crystal lithium cobaltate, and a preparation method and application thereof. Background Art

[0002] In recent years, due to the continuous development of new energy battery materials, the synthesis types, morphology control, and structure control of precursor materials have become increasingly rich. In order to meet the electrical performance requirements of different positive electrode materials, the synthesis requirements of precursor materials are also ever-changing, among which porous sheet precursors are very popular. However, porous sheet precursor materials are difficult to synthesize by coprecipitation. In most cases, the existing technology can only be synthesized by the template method, but this method has the defects of complex process, high cost, and difficulty in industrialization. At present, there is no existing technology for sheet-like porous cobalt chloride.

[0003] In view of this, the present invention is proposed. Summary of the invention

[0004] The purpose of the present invention includes providing a sheet-like porous cobalt chloride, single-crystal cobalt oxide, single-crystal lithium cobaltate and their preparation methods and applications to solve or improve the above-mentioned technical problems.

[0005] The present invention can be implemented like this:

[0006] In a first aspect, the present invention provides a sheet-like porous cobalt chloride, wherein the chemical formula of the sheet-like porous cobalt chloride is M x Co 1-x Cl2, 0≤x≤0.5, M is a metal element other than cobalt;

[0007] The flaky porous cobalt chloride has at least one of the following characteristics:

[0008] Feature 1: The tap density of the flaky porous cobalt chloride is not less than 1g / cm 3 ;

[0009] Feature 2: The specific surface area of ​​the flaky porous cobalt chloride is not less than 1.8m 2 / g;

[0010] Feature 3: Flake-like porous cobalt chloride D v10 Not less than 4.5μm;

[0011] Feature 4: D of lamellar porous cobalt chloride v50 Not less than 8.5μm;

[0012] Feature 5: D of lamellar porous cobalt chloride v90 Not less than 20μm;

[0013] Feature 6: The pore volume of the flaky porous cobalt chloride is not less than 0.10 cm3 / g.

[0014] In an alternative embodiment, 0≤x≤0.04.

[0015] In an optional embodiment, M includes at least one of Al, Ti, Cr, Mn, Fe, Ni, Cu, Zn, Sn, Zr, Mo, Nb, Y, W, In and Ge.

[0016] In a second aspect, the present invention provides a method for preparing flaky porous cobalt chloride as described in the aforementioned embodiment, comprising the following steps: spray-drying a metal mixture matching M and Co in the chemical formula according to a preset chemical formula to obtain a precursor having a hollow structure; and sintering the precursor to obtain flaky porous cobalt chloride.

[0017] In an alternative embodiment, the sources of the metals in the metal mixture are all in the form of chloride salts.

[0018] In an optional embodiment, the total concentration of the metal salt in the metal mixture is 1 mol / L to 3 mol / L.

[0019] In an optional embodiment, the spray drying temperature is 150°C to 350°C.

[0020] In an optional embodiment, the spray drying temperature is 240°C to 260°C.

[0021] In an optional embodiment, the D of the dried material obtained after spray drying is 50 4μm~25μm.

[0022] In an optional embodiment, the sintering temperature is 400° C. to 580° C., and the sintering time is 0.5 h to 12 h.

[0023] In an optional embodiment, the sintering temperature is not less than 500° C. and less than 580° C., and the sintering time is 2 h to 5 h;

[0024] In an optional embodiment, the heating rate during the sintering process is 4° C. / min to 6° C. / min.

[0025] In a third aspect, the present invention provides a single crystal cobalt oxide, which is obtained by sintering the flaky porous cobalt chloride of the aforementioned embodiment at a temperature not lower than 580°C.

[0026] In a fourth aspect, the present invention provides a single-crystal lithium cobalt oxide, wherein the raw materials for preparing the single-crystal lithium cobalt oxide include the flaky porous cobalt chloride of the aforementioned embodiment and / or the single-crystal cobalt oxide of the aforementioned embodiment.

[0027] In a fifth aspect, the present invention provides a method for preparing single-crystalline lithium cobalt oxide of the aforementioned embodiment, comprising the following steps: mixing a cobalt source and a lithium source and then calcining them; wherein the cobalt source comprises the flaky porous cobalt chloride of the aforementioned embodiment and / or the single-crystalline cobalt oxide of the aforementioned embodiment.

[0028] In an alternative embodiment, the molar ratio of cobalt in the cobalt source to lithium in the lithium source is from 1:1 to 1:1.05.

[0029] In an optional embodiment, the calcination temperature is 800° C. to 1100° C., and the calcination time is 4 h to 20 h.

[0030] In an alternative embodiment, the calcination temperature is 900°C to 950°C.

[0031] In a sixth aspect, the present invention provides a positive electrode plate, wherein the active material in the positive electrode plate includes the single crystal lithium cobalt oxide of the aforementioned embodiment.

[0032] In a seventh aspect, the present invention provides a battery comprising the positive electrode sheet of the aforementioned embodiment.

[0033] The beneficial effects of the present invention include:

[0034] The present invention proposes for the first time a cobalt chloride with a flaky porous structure and a preparation method thereof. The flaky porous cobalt chloride can have a higher tap density, a larger specific surface area and a pore volume, and a relatively uniform pore size, which is beneficial to increasing the sintering activity. When mixed with a lithium source and calcined, the flaky porous structure is also beneficial to the uniform diffusion of lithium ions into the bulk phase of the material, making the lithium ion distribution more uniform, thereby facilitating the improvement of the electrochemical performance of the positive electrode material and the battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0036] Figure 1 This is a SEM image of the dried material obtained by spray drying in Example 1;

[0037] Figure 2 This is a SEM image of the flaky porous cobalt chloride obtained by sintering in Example 1;

[0038] Figure 3 XRD diagram of the material before and after sintering in Example 1;

[0039] Figure 4This is a SEM image of the lithium cobalt oxide positive electrode material prepared in Example 1;

[0040] Figure 5 This is the XRD diagram of the lithium cobalt oxide positive electrode material prepared in Example 1. DETAILED DESCRIPTION

[0041] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0042] The following is a detailed description of the flaky porous cobalt chloride, single-crystal cobalt oxide, single-crystal lithium cobalt oxide, and their preparation methods and applications provided by the invention.

[0043] The present invention provides a flaky porous cobalt chloride, the chemical formula of which is M x Co 1-x Cl2, 0≤x≤0.5, M is a metal element other than cobalt.

[0044] In some optional embodiments, x can be 0, 0.1, 0.2, 0.3, 0.4 or 0.5, etc., or other values ​​within the range of 0 to 0.5. In some embodiments, 0≤x≤0.04, such as x can be 0, 0.01, 0.02, 0.03 or 0.04, etc.

[0045] In some optional embodiments, the sheet-like porous cobalt chloride may have a small amount of crystal water. In some optional embodiments, M may exemplarily but non-limitingly include at least one of Al, Ti, Cr, Mn, Fe, Ni, Cu, Zn, Sn, Zr, Mo, Nb, Y, W, In and Ge.

[0046] In some embodiments, the tap density (TD) of the sheet-like porous cobalt chloride is not less than 1 g / cm 3 , such as 1.14 g / cm 3 ~1.68g / cm 3 , for example, it can be 1.14 g / cm 3 , 1.21g / cm 3 , 1.22g / cm 3 , 1.29g / cm 3 , 1.35g / cm 3 or 1.78 g / cm 3 etc., and can also be 1.14 g / cm 3 ~1.68g / cm 3 Other values ​​within the range.

[0047] In some embodiments, the specific surface area (BET) of the flaky porous cobalt chloride is not less than 1.8 m 2 / g, such as 1.95g / cm 3 ~3.45g / cm 3 , for example, it can be 1.95 g / cm 3 , 2.10g / cm 3 , 2.14g / cm 3 , 2.44g / cm 3 , 2.52g / cm 3 or 3.45g / cm 3 etc., and can also be 1.95g / cm 3 ~3.45g / cm 3 Other values ​​within the range.

[0048] In some embodiments, the D of the flaky porous cobalt chloride is v10 Not less than 4.5 μm, such as 4.52 μm to 12.13 μm, for example, 4.52 μm, 7.14 μm, 8.40 μm, 8.59 μm, 10.58 μm, 11.42 μm or 12.13 μm, etc., or other values ​​within the range of 4.52 μm to 12.13 μm.

[0049] In some embodiments, the D of the flaky porous cobalt chloride is v50 Not less than 8.5 μm, such as 8.61 μm to 20.51 μm, for example, 8.61 μm, 10.44 μm, 12.61 μm, 15.73 μm, 16.86 μm, 18.85 μm or 20.51 μm, etc., or other values ​​within the range of 8.61 μm to 20.51 μm.

[0050] In some embodiments, the D of the flaky porous cobalt chloride is v90 Not less than 20 μm, such as 22.34 μm to 60.68 μm, for example, 22.34 μm, 40.48 μm, 40.71 μm, 55.72 μm, 58.67 μm, 60.59 μm or 60.68 μm, etc., or other values ​​within the range of 22.34 μm to 60.68 μm.

[0051] In some embodiments, the pore volume of the flaky porous cobalt chloride is not less than 0.10 cm 3 / g, such as 0.16cm 3 / g~0.31cm 3 / g, for example, 0.16 cm 3 / g, 0.2cm 3 / g, 0.24cm 3 / g, 0.26cm 3 / g, 0.28cm 3 / g or 0.31cm 3 / g, etc., can also be 0.16cm 3 / g~0.31cm 3 / Other values ​​within the range of g.

[0052] As mentioned above, the flaky porous cobalt chloride provided by the present invention has a higher tap density, a larger specific surface area and pore volume, and a relatively uniform pore size, which is beneficial to increase the sintering activity, and when mixed with a lithium source and calcined, the above-mentioned flaky porous structure is also beneficial to the uniform diffusion of lithium ions into the bulk phase of the material, making the lithium ion distribution more uniform, which is beneficial to improve the electrochemical performance of the positive electrode material and the battery.

[0053] Correspondingly, the present invention also provides a method for preparing the above-mentioned flaky porous cobalt chloride, which may include the following steps: spray-drying a metal mixture matching M and Co in the chemical formula according to a preset chemical formula to obtain a precursor with a hollow structure; and sintering the precursor to obtain a flaky porous cobalt chloride.

[0054] In the specific operation, the metal mixed solution can be prepared according to the molar ratio of M to Co in the preset chemical formula and the specific element used for M.

[0055] The sources of the metals in the above metal mixture are all in the form of chloride salts.

[0056] In some optional embodiments, the total concentration of metal salts in the metal mixture can be 1 mol / L to 3 mol / L, such as 1 mol / L, 1.5 mol / L, 2 mol / L, 2.5 mol / L or 3 mol / L, etc., or other values ​​within the range of 1 mol / L to 3 mol / L.

[0057] In some optional embodiments, the spray drying temperature can be 150° C. to 350° C., such as 150° C., 180° C., 200° C., 220° C., 250° C., 280° C., 300° C., 320° C. or 350° C., or other values ​​within the range of 150° C. to 350° C. In some typical embodiments, the spray drying temperature is 240° C. to 260° C., such as 240° C., 245° C., 250° C., 255° C. or 260° C.

[0058] If the spray drying temperature is lower than 150°C, it is not conducive to the volatilization of moisture in the material; if the spray drying temperature is higher than 350°C, the spray energy consumption increases, the equipment bearing capacity is limited, and a transition phase of a mixture of cobalt chloride and cobalt tetroxide will be obtained with low purity.

[0059] D of the dry material obtained after spray drying 50 It is 4 μm to 25 μm, such as 4 μm, 6 μm, 10 μm, 15 μm, 20 μm or 25 μm, and can also be other values ​​within the range of 4 μm to 25 μm.

[0060] As mentioned above, the dried material obtained by the above-mentioned spray drying has the advantages of good consistency, high purity, few impurities, high crystallinity and low water content, and the dried material has a hollow structure.

[0061] In some optional embodiments, the sintering temperature is 400° C. to 580° C., and the sintering time is 0.5 h to 12 h.

[0062] Among them, the sintering temperature can be, for example, 400°C, 420°C, 450°C, 480°C, 500°C, 520°C, 550°C, 570°C or 580°C, or other values ​​within the range of 400°C to 580°C. In some typical embodiments, the sintering temperature is not less than 500°C and less than 580°C. Under the condition of a sintering temperature of 580°C, the material obtained by sintering, in addition to the flaky porous cobalt chloride, also contains a small amount of cobalt tetroxide. It should be emphasized that if the sintering temperature is too low, the flaky porous chloride cannot be obtained. The reason is that the sintering temperature is too low, and the corresponding sintered material still retains the spherical morphology after spraying, and no breakage occurs.

[0063] The sintering time can be, for example, 0.5 h, 1 h, 2 h, 3 h, 4 h, 5 h, 6 h, 7 h, 8 h, 9 h, 10 h, 11 h or 12 h, or other values ​​within the range of 0.5 h to 12 h. In some typical embodiments, the sintering time is 2 h to 5 h.

[0064] In some optional embodiments, the heating rate during sintering can be 4°C / min to 6°C / min, such as 4°C / min, 4.5°C / min, 5°C / min, 5.5°C / min or 6°C / min, or other values ​​within the range of 4°C / min to 6°C / min. In some typical embodiments, the heating rate during sintering is 5°C / min.

[0065] If the heating rate is too high, the material after sintering will be severely agglomerated, affecting the flow of the material; if the heating rate is too low, the heating time will be slow and the efficiency will be low.

[0066] As mentioned above, the metal mixture is first spray-dried to obtain a dry material with a hollow spherical structure; the dry material is then sintered under the above conditions, and when the heating temperature rises to a certain temperature during sintering, a certain pressure difference is generated inside and outside the hollow spherical structure, causing the hollow spherical structure to break and collapse, forming a porous sheet structure. Among them, the main reasons for the pressure difference include: after the temperature rises, the internal pressure of the hollow spherical structure increases, and gas is generated and breaks out, and finally the hollow spherical structure collapses into a sheet structure.

[0067] The preparation method of the flaky porous cobalt chloride provided by the invention has simple process, short flow, low production cost, easy industrialization, efficient and fast batch production, and is economical and efficient.

[0068] In addition, the present invention also provides a single crystal cobalt oxide, which is obtained by sintering the above-mentioned flaky porous cobalt chloride at a temperature not lower than 580°C.

[0069] By sintering the flaky porous cobalt chloride at the above temperature, the flaky porous cobalt chloride can be oxidized to generate tricobalt tetroxide.

[0070] In other embodiments, the hollow structure can be directly obtained by sintering the precursor at a temperature not lower than 580° C., and the heating rate of the sintering process can also be 4° C. / min to 6° C. / min.

[0071] In addition, the present invention also provides a single-crystal lithium cobalt oxide, wherein the raw materials for preparing the single-crystal lithium cobalt oxide include the flaky porous cobalt chloride of the aforementioned embodiment and / or the single-crystal cobalt oxide of the aforementioned embodiment.

[0072] Correspondingly, the present invention also provides a method for preparing the above-mentioned single-crystal lithium cobalt oxide, which may include the following steps: mixing a cobalt source and a lithium source and then calcining them; wherein the cobalt source includes the above-mentioned flaky porous cobalt chloride and / or the above-mentioned single-crystal cobalt oxide.

[0073] For example, in some embodiments, the cobalt source is only flaky porous cobalt chloride; in other embodiments, the cobalt source is only single-crystalline cobalt oxide; in other embodiments, the cobalt source contains both flaky porous cobalt chloride and single-crystalline cobalt oxide.

[0074] In some optional embodiments, the molar ratio of cobalt in the cobalt source to lithium in the lithium source can be 1:1 to 1:1.05, such as 1:1, 1:1.01, 1:1.02, 1:1.03, 1:1.04 or 1:1.05, or other values ​​within the range of 1:1 to 1:1.05.

[0075] In some optional embodiments, the calcination temperature is 800° C. to 1100° C., such as 800° C., 850° C., 900° C., 950° C., 1000° C., 1050° C. or 1100° C., etc., and may also be other values ​​within the range of 800° C. to 1100° C. In some more typical embodiments, the calcination temperature is 900° C. to 950° C.

[0076] In some optional embodiments, the calcination time is 4 h to 20 h, such as 4 h, 8 h, 12 h, 16 h or 20 h, etc., and may also be other values ​​within the range of 4 h to 20 h.

[0077] By using flaky porous cobalt chloride in the cobalt source, the calcination activity can be improved during the calcination process, so that lithium ions can be more evenly diffused into the bulk phase of the material, and the lithium ions are more evenly distributed, thereby obtaining a lithium cobalt oxide positive electrode material with uniform distribution of chemical elements.

[0078] In some embodiments, the 0.2C discharge capacity of the single crystal lithium cobalt oxide is not less than 172 mAh / g, such as 172.51 mAh / g to 181.02 mAh / g.

[0079] In some embodiments, the 0.33C discharge capacity of single crystal lithium cobalt oxide is not less than 168 mAh / g, such as 168.06 mAh / g to 179.11 mAh / g.

[0080] In some embodiments, the capacity retention rate of single crystal lithium cobalt oxide after 200 cycles at 0.33C is not less than 83%, such as 83.06% to 89.56%.

[0081] In addition, the present invention also provides a positive electrode plate, in which the active material includes the above-mentioned single crystal lithium cobalt oxide.

[0082] The present invention also provides a battery cell, which includes the above-mentioned positive electrode plate.

[0083] For example, the battery cells may be used in, but are not limited to, electrical devices such as vehicles, ships or aircraft.

[0084] The present invention also provides a battery comprising the above battery monomer, which can be a lithium ion battery or a sodium ion battery.

[0085] The present invention also provides an electric device, which includes the above-mentioned battery cell and / or battery. As an example, the electric device can be, but not limited to, a mobile phone, a tablet, a laptop computer, an electric toy, an electric tool, a battery car, an electric car, a ship, a spacecraft, etc. Among them, the electric toy can include a fixed or mobile electric toy, such as a game console, an electric car toy, an electric ship toy, and an electric airplane toy, etc., and the spacecraft can include an airplane, a rocket, a space shuttle, and a spacecraft, etc.

[0086] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.

[0087] Example 1

[0088] This embodiment provides a single crystal lithium cobalt oxide, and the preparation method thereof includes:

[0089] S1: Preparation of lamellar porous cobalt chloride.

[0090] S11: Prepare 3 mol / L cobalt chloride metal liquid.

[0091] S12: spray drying the cobalt chloride metal liquid at 260°C until the D 50 is 15μm.

[0092] The scanning electron microscope image of the dried material is as follows Figure 1 As shown by Figure 1 It can be seen that the spray-dried material has good sphericity and a hollow structure. The XRD diagram of the dried material is as follows Figure 3 shown.

[0093] S13: Take 2 kg of the above dry material and put it into a sagger, and sinter it at high temperature in a box furnace at a heating rate of 5°C / min, raise the temperature to 580°C, and keep it warm for 3 hours to finally obtain a flaky porous cobalt chloride material (chemical formula: CoCl2).

[0094] The scanning electron microscope image of the sintered product after sintering is as follows Figure 2 As shown, the XRD pattern is Figure 3 As shown. Figure 3 It can be seen that the material obtained by spraying has good crystallinity and is a cobalt chloride material; the material after sintering is in flake form, which is unoxidized cobalt chloride mixed with a trace amount of cobalt oxide, because at 580°C, it is just the temperature node at which cobalt chloride is oxidized to cobalt tetroxide, so a peak of trace cobalt tetroxide appears in XRD.

[0095] S2: Preparation of single crystal lithium cobalt oxide.

[0096] The sintered product was mixed with lithium carbonate (the molar ratio of Co in the sintered product to Li in the lithium carbonate was 1:1.05) to obtain a mixture; the mixture was calcined at 900° C. for 6 h to obtain a lithium cobalt oxide positive electrode material with a single crystal structure.

[0097] The SEM image of the lithium cobalt oxide positive electrode material is as follows Figure 4 As shown, the XRD pattern of the lithium cobalt oxide positive electrode material is as follows Figure 5 shown.

[0098] Example 2

[0099] This embodiment provides a single crystal lithium cobalt oxide, and the preparation method thereof includes:

[0100] S1: Preparation of lamellar porous cobalt chloride.

[0101] S11: preparing a metal mixed solution with a total metal concentration of 3 mol / L, wherein the metal elements in the metal mixed solution are Al and Co, and the molar ratio of Al to Co is 2:98. Al is provided by aluminum chloride, and Co is provided by cobalt chloride.

[0102] S12: spray drying the cobalt chloride metal liquid at 260°C until the D 50 is 20μm.

[0103] S13: Take 2 kg of the above dried material and put it into a sagger, and sinter it in a box furnace at a high temperature. The heating rate is 5 ° C / min, and the temperature is raised to 520 ° C. The temperature is kept for 3 hours, and finally a flaky porous cobalt chloride material (chemical formula: Al 0.02 Co 0.98 Cl2).

[0104] S2: Preparation of single crystal lithium cobalt oxide.

[0105] The sintered product was mixed with lithium carbonate (the molar ratio of Co in the sintered product to Li in the lithium carbonate was 1:1.05) to obtain a mixture; the mixture was calcined at 910° C. for 6 h to obtain a lithium cobalt oxide positive electrode material with a single crystal structure.

[0106] Example 3

[0107] This embodiment provides a single crystal lithium cobalt oxide, and the preparation method thereof includes:

[0108] S1: Preparation of lamellar porous cobalt chloride.

[0109] S11: preparing a metal mixture with a total metal concentration of 2.5 mol / L, wherein the metal elements in the metal mixture are Ni and Co, and the molar ratio of Ni to Co in the metal mixture is 4:96, wherein Ni is provided by nickel chloride, and Co is provided by cobalt chloride.

[0110] S12: spray-dry the cobalt chloride metal solution at 250°C until the D 50 is 10μm.

[0111] S13: 2 kg of the above dried material was put into a sagger and sintered in a box furnace at a high temperature. The heating rate was 5 °C / min, the temperature was raised to 550 °C, and the temperature was kept for 3 hours. Finally, a flaky porous cobalt chloride material (chemical formula: Ni 0.04 Co 0.96 Cl2).

[0112] S2: Preparation of single crystal lithium cobalt oxide.

[0113] The sintered product was mixed with lithium carbonate (the molar ratio of Co in the sintered product to Li in the lithium carbonate was 1:1.05) to obtain a mixture; the mixture was calcined at 900° C. for 6 h to obtain a lithium cobalt oxide positive electrode material with a single crystal structure.

[0114] Example 4

[0115] This embodiment provides a single crystal lithium cobalt oxide, and the preparation method thereof includes:

[0116] S1: Preparation of lamellar porous cobalt chloride.

[0117] S11: preparing a metal mixture with a total metal concentration of 2.5 mol / L, wherein the metal elements in the metal mixture are Ni, Mn and Co, and the molar ratio of Ni, Mn and Co in the metal mixture is 4:4:92, wherein Ni is provided by nickel chloride, Mn is provided by manganese chloride, and Co is provided by cobalt chloride.

[0118] S12: spray-dry the cobalt chloride metal solution at 240°C until the D 50 is 12μm.

[0119] S13: Take 2 kg of the above dried material and put it into a sagger, and sinter it in a box furnace at a high temperature. The heating rate is 5 ° C / min, and the temperature is raised to 500 ° C. The temperature is kept for 2 hours, and finally a flaky porous cobalt chloride material (chemical formula: Ni 0.04 Mn 0.04 Co 0.92 Cl2).

[0120] S2: Preparation of single crystal lithium cobalt oxide.

[0121] The sintered product was mixed with lithium carbonate (the molar ratio of Co in the sintered product to Li in the lithium carbonate was 1:1.05) to obtain a mixture; the mixture was calcined at 930° C. for 6 h to obtain a lithium cobalt oxide positive electrode material with a single crystal structure.

[0122] Example 5

[0123] This embodiment provides a single crystal lithium cobalt oxide, and the preparation method thereof includes:

[0124] S1: Preparation of lamellar porous cobalt chloride.

[0125] S11: preparing a metal mixture with a total metal concentration of 2.2 mol / L, wherein the metal elements in the metal mixture are Ni, Mn, Co and Mg, and the molar ratio of Ni, Mn, Co and Mg in the metal mixture is 4:4:90:2, wherein Ni is provided by nickel chloride, Mn is provided by manganese chloride, Co is provided by cobalt chloride, and Mg is provided by magnesium chloride;

[0126] S12: spray-dry the cobalt chloride metal solution at 240°C until the D 50 is 20μm.

[0127] S13: Take 2 kg of the above dried material and put it into a sagger, and sinter it in a box furnace at a high temperature. The heating rate is 5 ° C / min, and the temperature is raised to 500 ° C. The temperature is kept for 5 hours, and finally a flaky porous cobalt chloride material (chemical formula: Ni 0.04 Mn 0.04 Co 0.90 Mg 0.02 Cl2).

[0128] S2: Preparation of single crystal lithium cobalt oxide.

[0129] The sintered product was mixed with lithium carbonate (the molar ratio of Co in the sintered product to Li in the lithium carbonate was 1:1.05) to obtain a mixture; the mixture was calcined at 950° C. for 6 h to obtain a lithium cobalt oxide positive electrode material with a single crystal structure.

[0130] Example 6

[0131] This embodiment provides a single crystal lithium cobalt oxide, and the preparation method thereof includes:

[0132] S1: Preparation of lamellar porous cobalt chloride.

[0133] S11: Prepare 2 mol / L cobalt chloride metal liquid.

[0134] S12: spray-dry the cobalt chloride metal solution at 240°C until the D 50 is 10μm.

[0135] S13: Take 2 kg of the above dry material and put it into a sagger, and sinter it at high temperature in a box furnace at a heating rate of 4°C / min, raise the temperature to 560°C, and keep it warm for 5 hours to finally obtain a flaky porous cobalt chloride material (chemical formula: CoCl2).

[0136] S2: Preparation of single crystal lithium cobalt oxide.

[0137] The sintered product was mixed with lithium carbonate (the molar ratio of Co in the sintered product to Li in the lithium carbonate was 1:1) to obtain a mixture; the mixture was calcined at 800° C. for 20 h to obtain a lithium cobalt oxide positive electrode material with a single crystal structure.

[0138] Example 7

[0139] This embodiment provides a single crystal lithium cobalt oxide, and the preparation method thereof includes:

[0140] S1: Preparation of lamellar porous cobalt chloride.

[0141] S11: Prepare 2.5 mol / L cobalt chloride liquid.

[0142] S12: spray-dry the cobalt chloride metal solution at 250°C until the D 50 is 20μm.

[0143] S13: Take 2 kg of the above dry material and put it into a sagger, and sinter it at high temperature in a box furnace at a heating rate of 6°C / min, raise the temperature to 580°C, and keep it warm for 0.5h to finally obtain a flaky porous cobalt chloride material (chemical formula: CoCl2).

[0144] S2: Preparation of single crystal lithium cobalt oxide.

[0145] The sintered product was mixed with lithium carbonate (the molar ratio of Co in the sintered product to Li in the lithium carbonate was 1:1.02) to obtain a mixture; the mixture was calcined at 1100° C. for 4 h to obtain a lithium cobalt oxide positive electrode material with a single crystal structure.

[0146] Comparative Example 1

[0147] The difference between this comparative example and Example 1 is that the spray drying temperature is 120°C.

[0148] Comparative Example 2

[0149] The difference between this comparative example and Example 1 is that the spray drying temperature is 400°C.

[0150] Comparative Example 3

[0151] The difference between this comparative example and Example 1 is that the sintering temperature is 350°C.

[0152] Comparative Example 4

[0153] The difference between this comparative example and Example 1 is that the heating rate during the sintering process is 10° C. / min.

[0154] Comparative Example 5

[0155] The difference between this comparative example and Example 1 is that ordinary cobalt chloride powder (with a particle size of 15 μm) is used instead of the flaky porous cobalt chloride.

[0156] Test Example 1

[0157] The tap density, specific surface area, particle size distribution and pore volume of the flaky porous cobalt chloride obtained in step S1 of Examples 1 to 7 and the material obtained in step S1 of Comparative Example 3 were tested, and the results are shown in Table 1.

[0158] Table 1 Test results

[0159] <![CDATA[TD(g / cm 3 )]]> <![CDATA[BET(m 2 / g)]]> <![CDATA[D V10 (μm)]]> <![CDATA[D V50 (μm)]]> <![CDATA[D V90 (μm)]]> <![CDATA[Pore volume (cm 3 / g)]]> Example 1 1.21 2.10 7.14 12.61 40.48 0.20 Example 2 1.14 1.95 8.59 15.73 60.59 0.16 Example 3 1.22 2.14 4.52 8.61 22.34 0.24 Example 4 1.35 2.52 8.40 10.44 40.71 0.28 Example 5 1.29 2.44 11.42 18.85 60.68 0.26 Example 6 1.35 3.45 10.58 16.86 55.72 0.31 Example 7 1.68 2.87 12.13 20.51 58.67 0.28 Comparative Example 3 2.21 0.82 12.48 15.29 40.25 0.08

[0160] Test Example 2

[0161] The lithium cobalt oxide prepared in step S2 of Examples 1 to 7 and step S2 of Comparative Examples 1 to 5 can be used as the positive electrode material to assemble a full battery. The positive electrode material, the conductive agent Super P, and the binder polyvinylidene fluoride (PVDF) are dispersed in a nitrogen methyl pyrrolidone (NMP) solvent at a mass ratio of 96:2:2, and stirred evenly to obtain an electrode slurry. The electrode slurry is coated on the surface of an aluminum foil, vacuum-baked at 120°C for 12 hours, rolled, and cut to obtain a positive electrode sheet; with a graphite negative electrode, a 1mol / L LiPF6 / (EC+DEC+DMC) electrolyte (volume ratio 1:1:1) and a PP / PE / PP three-layer separator are used to prepare a soft-pack battery. The charge and discharge tests were carried out at 4.48V / 0.2C and 0.33C test conditions at 25°C, respectively, and the results are shown in Table 2.

[0162] Table 2 Test results

[0163]

[0164]

[0165] It can be seen from Table 2 that the battery prepared by the lithium cobalt oxide positive electrode material provided by the embodiment of the present invention has better discharge capacity and capacity retention rate than the battery prepared by the lithium cobalt oxide positive electrode material provided by the comparative example.

[0166] In summary, the flaky porous cobalt chloride provided by the present invention has a higher tap density, a larger specific surface area and porosity, and a relatively uniform pore size, which is beneficial to increasing the sintering activity. When mixed with a lithium source and calcined, its flaky porous structure is also beneficial to the uniform diffusion of lithium ions into the bulk phase of the material, making the lithium ion distribution more uniform, which is beneficial to improving the electrochemical performance of the positive electrode material and the battery.

[0167] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A flaky porous cobalt chloride, characterized in that: The chemical formula of the flaky porous cobalt chloride is M x Co 1-x Cl2, 0≤x≤0.5, M is a metal element other than cobalt; The flaky porous cobalt chloride has at least one of the following characteristics: Feature 1: The tap density of the flaky porous cobalt chloride is not less than 1 g / cm 3 ; Feature 2: The specific surface area of ​​the flaky porous cobalt chloride is not less than 1.8 m 2 / g; Feature 3: The D of the flaky porous cobalt chloride v10 Not less than 4.5μm; Feature 4: D of the flaky porous cobalt chloride v50 Not less than 8.5μm; Feature 5: The D of the flaky porous cobalt chloride v90 Not less than 20μm; Feature 6: The pore volume of the flaky porous cobalt chloride is not less than 0.10 cm 3 / g; Preferably, 0≤x≤0.04; Preferably, M includes at least one of Al, Ti, Cr, Mn, Fe, Ni, Cu, Zn, Sn, Zr, Mo, Nb, Y, W, In and Ge.

2. A method for preparing the flaky porous cobalt chloride according to claim 1, characterized in that: The following steps are involved: According to a preset chemical formula, a metal mixture matching M and Co in the chemical formula is spray-dried to obtain a precursor with a hollow structure; The precursor is sintered to obtain the flaky porous cobalt chloride.

3. The preparation method according to claim 2, characterized in that: The sources of the metals in the metal mixture are all in the form of chloride salts; Preferably, the total concentration of the metal salts in the metal mixture is 1 mol / L to 3 mol / L.

4. The preparation method according to claim 2, characterized in that: The spray drying temperature is 150℃~350℃; Preferably, the spray drying temperature is 240°C to 260°C; Preferably, the D of the dried material obtained after spray drying is 50 4μm~25μm.

5. The preparation method according to claim 2, characterized in that: The sintering temperature is 400°C to 580°C, and the sintering time is 0.5h to 12h; Preferably, the sintering temperature is not less than 500°C and less than 580°C, and the sintering time is 2h to 5h; Preferably, the heating rate during the sintering process is 4° C. / min to 6° C. / min.

6. A single crystal cobalt oxide, characterized in that: The single crystal cobalt oxide is obtained by sintering the flaky porous cobalt chloride according to claim 1 at a temperature not lower than 580°C.

7. A single crystal lithium cobalt oxide, characterized in that: The raw materials for preparing the single-crystalline lithium cobalt oxide include the flaky porous cobalt chloride according to claim 1 and / or the single-crystalline cobalt oxide according to claim 6.

8. A method for preparing single crystal lithium cobalt oxide according to claim 7, characterized in that: The method comprises the following steps: mixing a cobalt source and a lithium source and then calcining the mixture; wherein the cobalt source comprises the flaky porous cobalt chloride according to claim 1 and / or the single crystal cobalt oxide according to claim 6; Preferably, the molar ratio of cobalt in the cobalt source to lithium in the lithium source is 1:1 to 1:1.05; Preferably, the calcination temperature is 800°C to 1100°C, and the calcination time is 4h to 20h; Preferably, the calcination temperature is 900°C to 950°C.

9. A positive electrode sheet, characterized in that: The active material in the positive electrode sheet includes the single crystal lithium cobalt oxide as claimed in claim 7.

10. A battery, characterized in that: The battery comprises the positive electrode sheet according to claim 9.

Citation Information

Patent Citations

  • Preparation method of nanoscale multi-element alloy

    CN111545767A

  • Monatomic metal doped alpha-cobalt hydroxide nanosheet as well as preparation method and application thereof

    CN114592213A

  • Preparation method of carbon monoxide synergistic denitration powder catalyst

    CN117563613A

  • Spray conversion process for the production of nanophase composite powders

    US5352269A