Ceramsite prepared from waste incineration fly ash and preparation method thereof

By combining incinerated fly ash, fly ash, bentonite, zinc oxide modified benzooxazine and epoxy nanosilica and ball milling, granulation and calcining, ceramic granules with good flame retardant properties were prepared, and the current situation was solved There are problems of insufficient flame retardant effect of waste incineration fly ash ceramic granules and environmental pollution, which has achieved efficient recycling and environmental protection effects of garbage resources.

CN119038957APending Publication Date: 2024-11-29GUIZHOU LIANGJUYUAN ENVIRONMENTAL PROTECTION TECH CO LTD +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411186437.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The flame retardant effect of existing waste incineration fly ash ceramic granules is insufficient, and the environmental pollution problem has not been effectively solved.

Method used

Use 55-80% incineration fly ash, 15-30% fly ash, 20-25% bentonite, 5-7% zinc oxide to modify benzooxazine and 2-6% epoxy nanosilicon dioxide The combination of the ceratops and pelletizing and calcining process was prepared with good flame retardant properties.

Benefits of technology

The ceramic granules modify the flame retardant mechanism of sulfur, silicon, boron and polyphenylene sulfide in benzooxazine through zinc oxide to form a protective carbon layer and a vitreous cover layer, which significantly improves the thermal decomposition temperature and high temperature resistance and reduces the Environmental pollution and efficient recycling of garbage resources are achieved.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of building materials, and discloses ceramsite prepared from waste incineration fly ash and a preparation method thereof.The preparation method includes the steps that the incineration fly ash, fly ash, bentonite, zinc oxide modified benzoxazine and epoxy nano-silica are put into a stirring mixer to be evenly mixed, then ball milling, granulation and calcination are conducted, and the ceramsite is obtained; the ceramsite prepared from the waste incineration fly ash is obtained. A sulfur element, a silicon element, a boron element and a benzoxazine structure contained in zinc oxide modified benzoxazine in the ceramsite jointly form a flame-retardant system, and polyphenylene sulfide and zinc oxide also have a flame-retardant effect; and benzoxazine can form a heat-resistant phenolic resin structure at a high temperature, and continuously reacts with the epoxy nano silicon dioxide to generate crosslinking to form a second protective layer, so that the ceramsite shows higher thermal decomposition temperature and high temperature resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of building materials, in particular to ceramsite prepared by utilizing fly ash from garbage incineration and a preparation method thereof. Background Art

[0002] With the development of society, cities generate a large amount of garbage every year. In order to effectively destroy the corrosive substances and pathogenic microorganisms in the garbage and reduce the amount of garbage, the garbage is usually incinerated. A large amount of residue will be generated after the incineration of the garbage. How to effectively recycle the residue is the key to solving the problem. Ceramic granule is a lightweight aggregate produced by foaming in a rotary kiln. It is widely used in pavement materials, concrete, thermal insulation materials and other fields. Therefore, the residue is applied to the raw materials of ceramic granule to achieve the purpose of recycling. For example, patent CN101905967B discloses a fly ash sintered brick made by washing fly ash from the incineration of domestic waste and a preparation method thereof. The invention turns the fly ash from the incineration of domestic waste into treasure and achieves the purpose of protecting resources, but its flame retardant effect is not improved. Summary of the invention

[0003] 1. Technical issues to be solved

[0004] In view of the deficiencies in the prior art, the present invention provides a ceramsite prepared by utilizing fly ash from garbage incineration and a preparation method thereof, which has good flame retardant effect and reduces environmental pollution.

[0005] (II) Technical solution

[0006] To achieve the above object, the present invention provides the following technical solution: a ceramsite prepared by using waste incineration fly ash, comprising the following components by weight: 55-80 parts by weight of incineration fly ash, 15-30 parts by weight of fly ash, 20-25 parts by weight of bentonite, 5-7 parts by weight of zinc oxide modified benzoxazine, and 2-6 parts by weight of epoxy nano-silica.

[0007] Preferably, the preparation method of the zinc oxide modified benzoxazine is:

[0008] (1) Under nitrogen protection, acetylated polyphenylene sulfide powder is added to anhydrous toluene solvent, and then 3-aminopropyltriethoxysilane is slowly added dropwise, and acetic acid and 4A molecular sieve are continuously added, and the reaction is carried out at 80-100° C. for 8-12 hours. After the reaction, the mixture is filtered, washed, and subjected to Soxhlet extraction with ethanol solution for 22-24 hours, and dried to constant weight to obtain organosilicon-grafted modified polyphenylene sulfide;

[0009] (2) adding hexamethyldisiloxane and organosilicon-grafted polyphenylene sulfide to acetonitrile solvent, stirring evenly, adding chloroplatinic acid catalyst thereto, reacting at 65-80° C. for 5-8 hours, and then performing reduced pressure distillation after the reaction, filtering and drying to obtain tertiary amino polyphenylene sulfide;

[0010] (3) adding 4-hydroxybenzyl chloride to N,N-dimethylformamide solvent, stirring and mixing, and continuing to add tertiary amino polyphenylene sulfide, reacting at 60-90° C. for 7-10 hours, rotary distilling after the reaction, washing and drying to obtain phenol-based polyphenylene sulfide;

[0011] (4) Adding boric acid-modified zinc oxide, an aqueous solution of formaldehyde, and phenol-based polyphenylene sulfide into toluene solvent, fully dissolving them, and carrying out a cyclization reaction at 65-90° C. for 10-14 hours. After the reaction, distillation under reduced pressure is performed, the product is washed with deionized water, and the crude product is recrystallized from dichloromethane to obtain zinc oxide-modified benzoxazine.

[0012] Preferably, the mass ratio of acetylated polyphenylene sulfide, 3-aminopropyltriethoxysilane, acetic acid and 4A molecular sieve in (1) is 1.2-1.8:1:0.02-0.04:0.7-1.0.

[0013] Preferably, the mass ratio of hexamethyldisiloxane, organosilicon grafted modified polyphenylene sulfide, and chloroplatinic acid catalyst in (2) is 1:1.1-1.3:0.01-0.02.

[0014] Preferably, the mass ratio of 4-hydroxybenzyl chloride to tertiary amino polyphenylene sulfide in (3) is 1.1-1.3:1.

[0015] Preferably, the mass ratio of the boric acid-modified zinc oxide, the formaldehyde aqueous solution, and the phenol-based polyphenylene sulfide in (4) is 1:1.3-1.5:1.1-1.2.

[0016] Preferably, the preparation method of the boric acid modified zinc oxide in (4) is: ultrasonically disperse 5-7 parts by weight of amino zinc oxide in a xylene solvent, and after ultrasonic dispersion, add 6-10 parts by weight of 4-aminophenylboric acid, introduce nitrogen protection, mix evenly, react at 75-90°C for 7-10 hours, and after the reaction, cool to room temperature, filter, and wash to obtain boric acid modified zinc oxide modified aluminum oxide.

[0017] Preferably, the preparation method of the ceramsite prepared using waste incineration fly ash is: incineration fly ash, fly ash, bentonite, zinc oxide modified benzoxazine, and epoxy nano-silica are put into a stirring mixer and mixed evenly, and then ball milled (ball milled to an average particle size of 120 microns), granulated, and calcined at a calcination temperature of 1200-1270°C to obtain ceramsite prepared using waste incineration fly ash.

[0018] (III) Beneficial technical effects

[0019] The invention provides ceramsite prepared by using the garbage incineration fly ash by putting incineration fly ash, fly ash, bentonite, zinc oxide modified benzoxazine and epoxy nano silicon dioxide into a stirring mixer and mixing them evenly, then performing ball milling, granulation and calcination.

[0020] The sulfur, silicon, boron and benzoxazine structure contained in the zinc oxide modified benzoxazine in the ceramsite together constitute a flame retardant system, and polyphenylene sulfide and zinc oxide themselves also have flame retardant effects; the sulfur element can release strong acids such as sulfuric acid under high temperature conditions, which can promote the dehydration of the substrate into carbon, forming a protective carbon layer, which has a flame retardant effect, and the silicon element will absorb a large amount of heat during the thermal decomposition process, reduce the temperature of the material, and slow down the combustion rate. The boron element melts at high temperature and covers the surface of the material to form a protective glass coating layer, which effectively isolates oxygen and external heat sources, thereby slowing down or preventing further combustion of the material. In addition, benzoxazine will form a heat-resistant phenolic resin structure at high temperature, continue to react with epoxy nano-silicon dioxide, cross-link, and form a second protective layer, so that the ceramsite exhibits a higher thermal decomposition temperature and high temperature resistance, while reducing environmental pollution, recycling garbage resources, and playing an environmental protection role. DETAILED DESCRIPTION

[0021] Reference "Organic Silicone Grafted Modified Polyphenylene Sulfide" Preparation of Acetylated Polyphenylene Sulfide: Dried PPS powder was suspended and dispersed in 200ml dichloromethane (purified after dehydration) for pre-swelling for 12 hours, and then poured into a 500ml flask equipped with a thermometer, a constant pressure dropping funnel, a condenser and a stirrer, and the upper end of the condenser was connected to a gas absorption device. After nitrogen was passed through for a while, 32.52g of anhydrous aluminum chloride powder was quickly added, and then 15ml of acetyl chloride was added to the constant pressure dropping funnel. In order to prevent the reaction from being too intense, the drop rate was controlled to 1 drop / 3S, and the mixture was stirred evenly. After all the materials were added, the mixture was first reacted in an ice water bath for 1.5r, then the temperature was raised to 38℃ and reacted for 3.5 hours until no HCl gas escaped, and then cooled to room temperature. The entire reaction solution was transferred into glacial hydrochloric acid (50 ml hydrochloric acid + 50 g ice) for decomposition, filtered, washed with 5% NaOH solution, then repeatedly washed with deionized water and ethanol solution, and vacuum dried at 80°C for 24 hours to obtain acetylated polyphenylene sulfide.

[0022] Preparation of amino zinc oxide: Weigh a certain amount of zinc oxide, add it to toluene solvent, ultrasonicate for 30-60 minutes, add silane coupling agent JH-M9002 and continue ultrasonic dispersion for 5-10 minutes, filter and dry to obtain amino zinc oxide.

[0023] Example 1

[0024] (1) Under nitrogen protection, acetylated polyphenylene sulfide powder is added to anhydrous toluene solvent, and then 3-aminopropyltriethoxysilane is slowly added dropwise, and acetic acid and 4A molecular sieve are continuously added, wherein the mass ratio of acetylated polyphenylene sulfide, 3-aminopropyltriethoxysilane, acetic acid, and 4A molecular sieve is 1.2:1:0.02:0.7, and the reaction is carried out at 80° C. for 8 hours. After the reaction is completed, the mixture is filtered, washed, and subjected to Soxhlet extraction with ethanol solution for 22 hours, and dried to constant weight to obtain organosilicon-grafted modified polyphenylene sulfide;

[0025] (2) adding hexamethyldisiloxane and organosilicon-grafted polyphenylene sulfide to acetonitrile solvent, stirring evenly, and continuing to add chloroplatinic acid catalyst thereto, wherein the mass ratio of hexamethyldisiloxane, organosilicon-grafted polyphenylene sulfide, and chloroplatinic acid catalyst is 1:1.1:0.01, reacting at 65° C. for 5 h, and then distilling under reduced pressure after the reaction, filtering and drying to obtain tertiary amino polyphenylene sulfide;

[0026] (3) adding 4-hydroxybenzyl chloride to N,N-dimethylformamide solvent, stirring and mixing, and continuing to add tertiary amino polyphenylene sulfide, wherein the mass ratio of 4-hydroxybenzyl chloride to tertiary amino polyphenylene sulfide is 1.1:1, reacting at 60° C. for 7 hours, rotary distilling after the reaction, washing and drying to obtain phenol-based polyphenylene sulfide;

[0027] (4) ultrasonically dispersing 5 parts by weight of amino zinc oxide into a xylene solvent, adding 6 parts by weight of 4-aminophenylboric acid after the ultrasonic dispersion is uniform, introducing nitrogen protection, mixing uniformly, reacting at 75° C. for 7 h, cooling to room temperature after the reaction, filtering, and washing to obtain boric acid-modified zinc oxide-modified aluminum oxide;

[0028] (5) adding boric acid-modified zinc oxide, an aqueous solution of formaldehyde, and phenol-based polyphenylene sulfide to a toluene solvent, wherein the mass ratio of boric acid-modified zinc oxide, the aqueous solution of formaldehyde, and phenol-based polyphenylene sulfide is 1:1.3:1.1, fully dissolving, and carrying out a cyclization reaction at 65° C. for 10 h. After the reaction, distillation under reduced pressure is performed, the product is washed with deionized water, and the crude product is recrystallized from dichloromethane to obtain zinc oxide-modified benzoxazine;

[0029] (6) 55 parts by weight of incineration fly ash, 15 parts by weight of fly ash, 20 parts by weight of bentonite, 5 parts by weight of zinc oxide-modified benzoxazine, and 2 parts by weight of epoxy nano-silica were put into a stirring mixer and mixed evenly, and then ball milled, granulated, and calcined at a calcination temperature of 1200° C. to obtain ceramsite prepared using waste incineration fly ash.

[0030] Example 2

[0031] (1) under nitrogen protection, acetylated polyphenylene sulfide powder was added to anhydrous toluene solvent, and then 3-aminopropyltriethoxysilane was slowly added dropwise, and acetic acid and 4A molecular sieve were continuously added, wherein the mass ratio of acetylated polyphenylene sulfide, 3-aminopropyltriethoxysilane, acetic acid and 4A molecular sieve was 1.8:1:0.04:1.0, and the mixture was reacted at 100° C. for 12 h. After the reaction, the mixture was filtered, washed, and subjected to Soxhlet extraction with ethanol solution for 24 h, and dried to constant weight to obtain organosilicon-grafted modified polyphenylene sulfide;

[0032] (2) adding hexamethyldisiloxane and organosilicon-grafted modified polyphenylene sulfide to acetonitrile solvent, stirring evenly, and continuing to add chloroplatinic acid catalyst thereto, wherein the mass ratio of hexamethyldisiloxane, organosilicon-grafted modified polyphenylene sulfide, and chloroplatinic acid catalyst is 1:1.3:0.02, reacting at 80° C. for 8 h, and then performing reduced pressure distillation after completion, filtering, and drying to obtain tertiary amino polyphenylene sulfide;

[0033] (3) adding 4-hydroxybenzyl chloride to N,N-dimethylformamide solvent, stirring and mixing, and continuing to add tertiary amino polyphenylene sulfide, wherein the mass ratio of 4-hydroxybenzyl chloride to tertiary amino polyphenylene sulfide is 1.3:1, reacting at 90° C. for 10 hours, rotary distilling after the reaction, washing and drying to obtain phenol-based polyphenylene sulfide;

[0034] (4) ultrasonically dispersing 7 parts by weight of amino zinc oxide in a xylene solvent, adding 10 parts by weight of 4-aminophenylboric acid after the ultrasonic dispersion is uniform, introducing nitrogen protection, mixing uniformly, reacting at 90° C. for 10 h, cooling to room temperature after the reaction, filtering, and washing to obtain boric acid-modified zinc oxide-modified aluminum oxide;

[0035] (5) adding boric acid-modified zinc oxide, an aqueous solution of formaldehyde, and phenol-based polyphenylene sulfide to a toluene solvent, wherein the mass ratio of boric acid-modified zinc oxide, the aqueous solution of formaldehyde, and phenol-based polyphenylene sulfide is 1:1.5:1.2, fully dissolving, and carrying out a cyclization reaction at 90° C. for 14 hours. After the reaction, distillation under reduced pressure is performed, the product is washed with deionized water, and the crude product is recrystallized from dichloromethane to obtain zinc oxide-modified benzoxazine;

[0036] (6) 80 parts by weight of incineration fly ash, 30 parts by weight of fly ash, 25 parts by weight of bentonite, 7 parts by weight of zinc oxide-modified benzoxazine, and 6 parts by weight of epoxy nano-silica were put into a stirring mixer and mixed evenly, and then ball-milled, granulated, and calcined at a calcination temperature of 1270° C. to obtain ceramsite prepared using waste incineration fly ash.

[0037] Example 3

[0038] (1) Under nitrogen protection, acetylated polyphenylene sulfide powder is added to anhydrous toluene solvent, and then 3-aminopropyltriethoxysilane is slowly added dropwise, and acetic acid and 4A molecular sieve are continuously added, wherein the mass ratio of acetylated polyphenylene sulfide, 3-aminopropyltriethoxysilane, acetic acid, and 4A molecular sieve is 1.6:1:0.03:0.85, and the reaction is carried out at 90° C. for 10 hours. After the reaction is completed, the mixture is filtered, washed, and subjected to Soxhlet extraction with ethanol solution for 23 hours, and dried to constant weight to obtain organosilicon-grafted modified polyphenylene sulfide;

[0039] (2) adding hexamethyldisiloxane and organosilicon-grafted modified polyphenylene sulfide to acetonitrile solvent, stirring evenly, and continuing to add chloroplatinic acid catalyst, wherein the mass ratio of hexamethyldisiloxane, organosilicon-grafted modified polyphenylene sulfide, and chloroplatinic acid catalyst is 1:1.2:0.015, reacting at 72° C. for 6.5 hours, and then distilling under reduced pressure after the reaction, filtering and drying to obtain tertiary amino polyphenylene sulfide;

[0040] (3) adding 4-hydroxybenzyl chloride to N,N-dimethylformamide solvent, stirring and mixing, and continuing to add tertiary amino polyphenylene sulfide, wherein the mass ratio of 4-hydroxybenzyl chloride to tertiary amino polyphenylene sulfide is 1.2:1, reacting at 75° C. for 8.5 hours, rotary distilling after the reaction, washing and drying to obtain phenol-based polyphenylene sulfide;

[0041] (4) ultrasonically dispersing 6 parts by weight of amino zinc oxide into a xylene solvent, and after the ultrasonic dispersion is uniform, adding 8 parts by weight of 4-aminophenylboric acid, passing nitrogen protection, mixing uniformly, reacting at 82° C. for 8.5 hours, cooling to room temperature after the reaction, filtering, and washing to obtain boric acid-modified zinc oxide-modified aluminum oxide;

[0042] (5) adding boric acid-modified zinc oxide, an aqueous solution of formaldehyde, and phenol-based polyphenylene sulfide to a toluene solvent, wherein the mass ratio of boric acid-modified zinc oxide, the aqueous solution of formaldehyde, and phenol-based polyphenylene sulfide is 1:1.4:1.15, fully dissolving, and carrying out a cyclization reaction at 77° C. for 12 h. After the reaction, distillation under reduced pressure is performed, the product is washed with deionized water, and the crude product is recrystallized from dichloromethane to obtain zinc oxide-modified benzoxazine;

[0043] (6) 67 parts by weight of incineration fly ash, 22.5 parts by weight of fly ash, 22.5 parts by weight of bentonite, 6 parts by weight of zinc oxide-modified benzoxazine, and 4 parts by weight of epoxy nano-silica were put into a stirring mixer and mixed evenly, and then ball-milled, granulated, and calcined at a calcination temperature of 1235° C. to obtain ceramsite prepared using waste incineration fly ash.

[0044] Comparative Example 1

[0045] This comparative example is different from Example 3 in that zinc oxide is not added to modify the benzoxazine.

[0046] Comparative Example 2

[0047] The difference between this comparative example and Example 3 is that no epoxy nano-silica is added.

[0048] The limiting oxygen index of the material was tested using an oxygen index meter, and the combustion grade of the material was tested using a horizontal and vertical combustion instrument. The test results are shown in Table 1.

[0049] Table 1: Flame retardancy tests.

[0050] project Limiting oxygen index (%) Combustion level Example 1 32 V-0 Example 2 33 V-0 Example 3 32 V-0 Comparative Example 1 21 V-1 Comparative Example 2 20 V-1

[0051] It can be seen from Table 1 that Examples 1-3 of the present invention have better flame retardant effects than Comparative Examples 1-2.

[0052] The performance indexes of the ceramsite prepared in the above-mentioned embodiments were tested with reference to GB / T 17431-2010 “Lightweight aggregate and its test methods”. The test results are shown in Table 2.

[0053] Table 2: Bulk density and cylinder pressure strength tests.

[0054] project <![CDATA[Bulk density / kg / m 3 > Cylinder pressure strength / MPa Example 1 580 4.1 Example 2 570 4.3 Example 3 580 4.1 Comparative Example 1 570 4.1 Comparative Example 2 580 4.2

[0055] It can be seen from Table 2 that the embodiments of the present invention and the comparative examples have better bulk density and cylinder pressure strength.

[0056] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. A ceramsite prepared from fly ash from garbage incineration, It is characterized in that The invention comprises the following components by weight: 55-80 parts by weight of incineration fly ash, 15-30 parts by weight of fly ash, 20-25 parts by weight of bentonite, 5-7 parts by weight of zinc oxide modified benzoxazine, and 2-6 parts by weight of epoxy nano-silicon dioxide.

2. The ceramsite prepared by utilizing fly ash from garbage incineration according to claim 1, It is characterized in that The preparation method of the zinc oxide modified benzoxazine is: (1) Under nitrogen protection, acetylated polyphenylene sulfide powder is added to anhydrous toluene solvent, and then 3-aminopropyltriethoxysilane is slowly added dropwise, and acetic acid and 4A molecular sieve are continuously added, and the reaction is carried out at 80-100° C. for 8-12 hours. After the reaction, the mixture is filtered, washed, and subjected to Soxhlet extraction with ethanol solution for 22-24 hours, and dried to constant weight to obtain organosilicon-grafted modified polyphenylene sulfide; (2) adding hexamethyldisiloxane and organosilicon-grafted polyphenylene sulfide to acetonitrile solvent, stirring evenly, adding chloroplatinic acid catalyst thereto, reacting at 65-80° C. for 5-8 hours, and then performing reduced pressure distillation after the reaction, filtering and drying to obtain tertiary amino polyphenylene sulfide; (3) adding 4-hydroxybenzyl chloride to N,N-dimethylformamide solvent, stirring and mixing, and continuing to add tertiary amino polyphenylene sulfide, reacting at 60-90° C. for 7-10 hours, rotary distilling after the reaction, washing and drying to obtain phenol-based polyphenylene sulfide; (4) Adding boric acid-modified zinc oxide, an aqueous solution of formaldehyde, and phenol-based polyphenylene sulfide into toluene solvent, fully dissolving them, and carrying out a cyclization reaction at 65-90° C. for 10-14 hours. After the reaction, distillation under reduced pressure is performed, the product is washed with deionized water, and the crude product is recrystallized from dichloromethane to obtain zinc oxide-modified benzoxazine.

3. The ceramsite prepared by utilizing fly ash from garbage incineration according to claim 2, It is characterized in that The mass ratio of acetylated polyphenylene sulfide, 3-aminopropyltriethoxysilane, acetic acid and 4A molecular sieve in (1) is 1.2-1.8:1:0.02-0.04:0.7-1.

0.

4. The ceramsite prepared by utilizing fly ash from garbage incineration according to claim 2, It is characterized in that The mass ratio of hexamethyldisiloxane, organosilicon grafted modified polyphenylene sulfide and chloroplatinic acid catalyst in (2) is 1:1.1-1.3:0.01-0.

02.

5. The ceramsite prepared by utilizing fly ash from garbage incineration according to claim 2, It is characterized in that The mass ratio of 4-hydroxybenzyl chloride to tertiary amino polyphenylene sulfide in (3) is 1.1-1.3:

1.

6. The ceramsite prepared by utilizing fly ash from garbage incineration according to claim 2, It is characterized in that The mass ratio of the boric acid-modified zinc oxide, the formaldehyde aqueous solution and the phenol-based polyphenylene sulfide in (4) is 1:1.3-1.5:1.1-1.

2.

7. The ceramsite prepared by utilizing fly ash from garbage incineration according to claim 2, It is characterized in that The preparation method of the boric acid modified zinc oxide in (4) is as follows: 5-7 parts by weight of amino zinc oxide is ultrasonically dispersed in a xylene solvent, after the ultrasonic dispersion is uniform, 6-10 parts by weight of 4-aminophenylboric acid is added, nitrogen is introduced for protection, the mixture is mixed uniformly, and the mixture is reacted at 75-90° C. for 7-10 hours. After the reaction, the mixture is cooled to room temperature, filtered, and washed to obtain boric acid modified zinc oxide modified aluminum oxide.

8. A method for preparing ceramsite prepared by using fly ash from waste incineration as claimed in any one of claims 1 to 7, It is characterized in that The preparation method of the ceramsite prepared by using waste incineration fly ash is as follows: incineration fly ash, fly ash, bentonite, zinc oxide modified benzoxazine, and epoxy nano-silica are put into a stirring mixer and mixed evenly, and then ball milled, granulated, and calcined at a calcination temperature of 1200-1270° C. to obtain the ceramsite prepared by using waste incineration fly ash.

Citation Information

Patent Citations

  • Fly ash baked brick prepared by washed incineration fly ash of house refuse and preparation method thereof

    CN101905967B