Method for preparing in-situ SiC-high-entropy ceramic anti-ablation composite coating through one-step method

The preparation of SiC-high entropy ceramic ablation-resistant composite coating by one-step discharge plasma sintering solves the problems of long-term coating preparation, high porosity and insufficient thickness in the prior art, and achieves high-temperature ablation resistance and high-induced ablation Density coating extends the service life of aerospace equipment.

CN119039018AActive Publication Date: 2024-11-29XIAN TECH UNIV

Patent Information

Application Number
CN202410950112.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-11-29
Estimated Expiration
2044-07-16

AI Technical Summary

Technical Problem

The existing ultra-high temperature ablation-resistant ceramic coating preparation technology has problems such as time-consuming, high porosity, performance differences caused by layered structures and insufficient coating thickness, which cannot meet the service requirements of spacecraft in high-temperature and high-pressure environments.

Method used

The SiC-high-entropy ceramic anti-ablation composite coating was prepared by one-step method, and the SiC transition layer and (Ti Zr Hf Ta)X high-entropy ceramic coating were simultaneously generated by discharge plasma sintering method to shorten the reaction time and improve density and binding force. .

Benefits of technology

Achieve high-temperature ablation resistance and high density SiC-high entropy ceramic composite coating, extending the service life of aerospace equipment in extreme environments, and improving the stability of the coating through multi-primary component design and low residual thermal stress. sex.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119039018A_ABST
    Figure CN119039018A_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing an in-situ SiC-high-entropy ceramic anti-ablation composite coating by a one-step method, the composite coating takes SiC as a transition layer and (Ti Zr Hf Ta) X as a high-entropy ceramic anti-ablation coating, and X is B or C. The composite coating is prepared by sintering by a one-step method, so that the reaction time is greatly shortened; the prepared composite coating has high-temperature ablation resistance and high density, and a new thought is provided for preparation of the high-entropy ceramic ablation-resistant coating.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of anti-ablation protective coatings, and specifically relates to a one-step method for preparing an in-situ SiC-high entropy ceramic anti-ablation composite coating. Background Art

[0002] Spacecraft must withstand harsh service environments when working. If ultra-high temperature materials are not used for effective thermal protection, they will not be able to complete the necessary flight work. Carbon-based materials are widely used in hot-end components of aerospace equipment. However, carbon will ablate in a high temperature, high pressure and high speed environment of 2000℃, which seriously affects its service life. Therefore, it is necessary to prepare ultra-high temperature anti-ablation ceramic coatings on carbon-based surfaces.

[0003] The existing technology for preparing ultra-high temperature anti-ablation ceramic coatings mainly includes three types of preparation technologies: chemical vapor deposition, chemical vapor deposition to prepare a transition layer and a combination of thermal spraying to prepare an anti-ablation coating, and magnetron sputtering to prepare an anti-ablation coating.

[0004] Among them, the process of chemical vapor deposition is time-consuming and requires the introduction of hydrogen as a protective reducing gas in the furnace, which is dangerous. If a transition layer needs to be prepared, the cycle of chemical vapor deposition will be even longer. The most important problems of thermal spraying are concentrated in two points. On the one hand, the thermal spray coating is formed by the stacking and collision of molten or semi-molten tiny particles, which leads to a certain porosity of the coating. Sometimes, due to poor selection of thermal spraying process parameters, poor powder processing and poor preparation process of substrate pretreatment, the prepared coating has a large number of pores, which will cause uneven coating and decreased overall mechanical properties of the coating; on the other hand, the prepared coating is a typical layered structure, which may cause the bonding force between the coatings to be not as good as laser cladding and the organization of each part of the coating is not uniform, resulting in certain differences in the performance of the coatings. The most important problem with magnetron sputtering coatings is that the coating thickness is very thin, generally about 3μm, which is far from meeting the requirements of ablation resistance.

[0005] In view of the above reasons, it is urgent to study an anti-ablation composite coating with excellent corrosion resistance. Summary of the invention

[0006] In order to overcome the above problems, the present invention proposes a one-step method for preparing an in-situ SiC-high entropy ceramic anti-ablation composite coating, wherein the composite coating uses SiC as a transition layer and (Ti Zr Hf Ta)X as a high entropy ceramic anti-ablation coating, where X is B or C. The composite coating is prepared in one step by spark plasma sintering, which greatly shortens the reaction time. The prepared composite coating has high-temperature anti-ablation performance and high density, which provides a new idea for the preparation of high-entropy ceramic anti-ablation coatings, thereby completing the present invention.

[0007] Specifically, the purpose of the present invention is to provide the following aspects:

[0008] On the one hand, a SiC-high entropy ceramic anti-ablation composite coating is provided, wherein the composite coating uses SiC as a transition layer and (Ti Zr Hf Ta)X as a high entropy ceramic anti-ablation coating, wherein X is B or C.

[0009] On the other hand, a method for preparing the SiC-high entropy ceramic anti-ablation composite coating according to the first aspect is provided, the method comprising:

[0010] Step 1, mixing a Ti source, a Zr source, a Hf source and a Ta source and ball-milling them to obtain a ball-milled product;

[0011] Step 2, pressing the ball-milled product and Si powder on a graphite substrate to obtain a pressed product;

[0012] Step 3: sintering the pressed product to obtain the SiC-high entropy ceramic anti-ablation composite coating.

[0013] The beneficial effects of the present invention include:

[0014] (1) The SiC-high entropy ceramic anti-ablation composite coating provided by the present invention has high-temperature anti-ablation performance, and there is a strong bonding force between the transition layer and the high entropy ceramic anti-ablation coating. The density of the high entropy ceramic anti-ablation coating is 97.13%.

[0015] (2) The method for preparing the SiC-high entropy ceramic anti-ablation composite coating provided by the present invention simultaneously prepares the SiC transition layer and the high entropy ceramic anti-ablation coating in a one-step method by spark plasma sintering, which greatly shortens the reaction time and is more conducive to achieving precise control.

[0016] (3) The present invention provides a method for preparing a SiC-high entropy ceramic anti-ablation composite coating. The SiC transition layer is a SiC transition layer generated in situ by reacting with carbon by placing Si powder on the surface of a graphite substrate during spark plasma sintering. This effectively alleviates the thermal mismatch between the transition layer and the high entropy ceramic anti-ablation coating, thereby improving the high-temperature anti-ablation performance of the high entropy ceramic anti-ablation coating.

[0017] (4) The present invention provides a method for preparing a SiC-high entropy ceramic anti-ablation composite coating. The prepared single-phase (TiZrHfTa)X series high entropy ceramic anti-ablation coating has a multi-principal component design, where X is C or B. It has a unique single-phase solid solution structure and low residual thermal stress, which can extend the service life in extreme environments. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] By reading the detailed description of the preferred specific embodiments below, various other advantages and benefits of the present invention will become clear to those of ordinary skill in the art. The drawings in the specification are only used for the purpose of illustrating the preferred embodiments and are not considered to be limitations of the present invention. Obviously, the drawings described below are only some embodiments of the present invention. For those of ordinary skill in the art, other drawings can also be obtained based on these drawings without creative work.

[0019] In the attached picture:

[0020] Figure 1 The XRD spectrum of the high entropy ceramic anti-ablation coating in the SiC-high entropy ceramic anti-ablation composite coating prepared in Example 1 is shown;

[0021] Figure 2 A macroscopic image of the SiC-high entropy ceramic anti-ablation composite coating prepared in Example 1 is shown;

[0022] Figure 3 The cross-sectional morphology of the SiC-high entropy ceramic anti-ablation composite coating prepared in Example 1 is shown;

[0023] Figure 4 The element distribution diagram of Ti, Zr, Hf, Ta, Si and C in the SiC-high entropy ceramic anti-ablation composite coating prepared in Example 1 is shown;

[0024] Figure 5 The XRD spectrum of the high entropy ceramic anti-ablation coating in the SiC-high entropy ceramic anti-ablation composite coating prepared in Example 3 is shown;

[0025] Figure 6 The XRD spectrum of the high entropy ceramic anti-ablation coating in the SiC-high entropy ceramic anti-ablation composite coating prepared in Example 4 is shown;

[0026] Figure 7 The XRD spectrum of the high entropy ceramic anti-ablation coating in the SiC-high entropy ceramic anti-ablation composite coating prepared in Example 5 is shown. DETAILED DESCRIPTION

[0027] The following will refer to the attached Figures 1 to 7 Specific embodiments of the present invention are described in more detail. Although specific embodiments of the present invention are shown in the accompanying drawings, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments described herein. On the contrary, these embodiments are provided to enable a more thorough understanding of the present invention and to fully convey the scope of the present invention to those skilled in the art.

[0028] It should be noted that certain words are used in the specification and claims to refer to specific components. Those skilled in the art should understand that technicians may use different nouns to refer to the same component. This specification and claims do not use the difference in nouns as a way to distinguish components, but use the difference in the functions of the components as the criterion for distinction. As mentioned throughout the specification and claims, "including" or "comprising" is an open term, so it should be interpreted as "including but not limited to". The subsequent description of the specification is a preferred embodiment of the present invention, but the description is based on the general principles of the specification and is not intended to limit the scope of the present invention. The scope of protection of the present invention shall be determined by the attached claims.

[0029] In the description of the present invention, it should be noted that the terms "upper", "lower", "inner", "outer", "front", "rear", etc. indicate positions or positional relationships based on the working state of the present invention, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first", "second", "third", and "fourth" are only used for descriptive purposes and cannot be understood as indicating or implying relative importance.

[0030] To facilitate understanding of the embodiments of the present invention, further explanation will be given below by taking specific embodiments as examples in conjunction with the accompanying drawings, and each of the accompanying drawings does not constitute a limitation on the embodiments of the present invention.

[0031] On the one hand, according to the SiC-high entropy ceramic anti-ablation composite coating provided by the present invention, the composite coating uses SiC as a transition layer and (Ti Zr Hf Ta)X as a high entropy ceramic anti-ablation coating, wherein X is B or C.

[0032] Furthermore, the molar ratio of Ti, Zr, Hf and Ta in the high entropy ceramic anti-ablation coating is equimolar.

[0033] Wherein, the thickness of the transition layer is 28-40 μm, and the thickness of the high-entropy ceramic anti-ablation coating is 180-210 μm.

[0034] On the other hand, according to the method for preparing the SiC-high entropy ceramic anti-ablation composite coating provided by the present invention, the method comprises:

[0035] Step 1, mixing a Ti source, a Zr source, a Hf source and a Ta source and ball-milling them to obtain a ball-milled product;

[0036] Step 2, pressing the ball-milled product and the Si source on a graphite substrate to obtain a pressed product;

[0037] Step 3: sintering the pressed product to obtain the SiC-high entropy ceramic anti-ablation composite coating.

[0038] The preparation method of the SiC-high entropy ceramic anti-ablation composite coating is described in detail below.

[0039] Step 1, mixing and ball-milling a Ti source, a Zr source, a Hf source and a Ta source to obtain a ball-milled product.

[0040] In step 1, the Ti source provides Ti, the Zr source provides Zr, the Hf source provides Hf, and the Ta source provides Ta. Ti has the characteristics of low density, excellent mechanical strength, plasticity, and good heat resistance; the surface of Zr is easy to form an oxide film, which is corrosion-resistant. At high temperatures, it can react with non-metallic elements and many metal elements to form a solid solution; Hf is associated with Zr, has plasticity, and is stable in the air; Ta is ductile and has a small thermal expansion coefficient. These elements all have good corrosion resistance. They can be used as corrosion-resistant components in composite coatings, and change physical and chemical properties by forming intermetallic compounds or through solute atom effects to improve the hardness, wear resistance, and high-temperature oxidation resistance of the composite coating; in addition, the thermal expansion coefficients of Ti, Zr, Hf, and Ta are similar, which means that they are less likely to produce thermal stress when the temperature changes, thereby improving the thermal stability of the coating.

[0041] Furthermore, the Ti source, Zr source, Hf source and Ta source are carbides or borides, namely TiC, ZrC, HfC, TaC or TiB, ZrB, HfB, TaB.

[0042] According to the present invention, each element of Ti, Zr, Hf and Ta plays a unique role, and more importantly, each element cooperates with each other, so that the obtained composite coating has excellent performance.

[0043] In step 1, the mixing ratio of the Ti source, Zr source, Hf source and Ta source is an equimolar ratio.

[0044] In step 1, the ball milling efficiency is closely related to the ball milling parameters.

[0045] The ball loading amount is determined according to the required ball milling efficiency to achieve the best impact and grinding state. The ball-to-material weight ratio is 3-7:1, preferably 4-6:1, for example 5:1.

[0046] In step 1, the ball milling speed is 100-300 r / min, preferably 100-260 r / min, for example 250 r / min.

[0047] According to the present invention, as the ball milling speed increases, the powder particles of the Ti source, Zr source, Hf source and Ta source are refined and distributed more evenly, thereby improving the mechanical properties of the prepared composite coating; however, an excessively fast ball milling speed causes the Ti source, Zr source, Hf source and Ta source to be neither stirred nor crushed, and may also cause segregation, thereby causing the density of the prepared composite coating to be reduced.

[0048] In step 1, the ball milling time is 4 to 12 hours, preferably 4 to 10 hours, and more preferably 6 hours.

[0049] In the present invention, the ball milling time is very important to improve the dispersion degree of Ti source, Zr source, Hf source and Ta source and the mechanical properties of the obtained composite coating. As the ball milling time increases, the raw materials are dispersed more and more evenly, but if the ball milling time is too long, the refinement effect is not obvious, but the activity of each raw material is continuously increased during the ball milling process, and the work hardening is serious.

[0050] Step 2: Pressing the ball-milled product and the Si source on a graphite substrate to obtain a pressed product.

[0051] According to a preferred embodiment, step 2 comprises the following steps:

[0052] Step 2-1, spreading the Si source on the graphite substrate and performing a pressing operation to obtain a pre-pressed product;

[0053] Step 2-2: Spread the ball-milled material onto the pre-pressed material, and perform secondary pressing to obtain the pressed material.

[0054] In step 2-1, the graphite substrate provides a carbon source for the composite coating, and the Si source and the SiC transition layer generated in situ by the graphite substrate during the sintering process effectively alleviate the thermal mismatch between the graphite substrate and the high-entropy ceramic anti-ablation coating, thereby improving the high-temperature anti-ablation performance of the high-entropy ceramic anti-ablation coating.

[0055] In step 2-1, the Si source is Si powder, which forms a SiC transition layer with C, which is more stable.

[0056] In step 2-1, the pressing pressure is 5 to 35 MPa, preferably 15 to 30 MPa, and more preferably 30 MPa.

[0057] In step 2-1, the pressing time is 10 to 20 min, preferably 15 to 20 min, and more preferably 15 min.

[0058] In step 2-2, the mass of the ball-milled material is set according to the thickness of the high-entropy ceramic anti-ablation coating. Generally, the mass ratio of the ball-milled material to the Si source is (10-20):1, preferably (15-17):1, and more preferably 15:1.

[0059] In step 2-2, the pressing pressure is 5 to 35 MPa, preferably 15 to 30 MPa, and more preferably 30 MPa.

[0060] In step 2-2, the pressing time is 10 to 40 min, preferably 15 to 30 min, and more preferably 20 min.

[0061] In steps 2-1 and 2-2, the powder adhesion and consistency are increased by pressing.

[0062] Step 3: sintering the pressed product to obtain the SiC-high entropy ceramic anti-ablation composite coating.

[0063] According to a preferred embodiment, the sintering includes: heating from room temperature to 1600°C to 2200°C at a heating rate of 30 to 100°C / min, keeping the temperature for 3 to 10 minutes, and maintaining the sintering pressure at 10 to 30 MPa.

[0064] Among them, if the sintering temperature is slightly lower, it will take a longer time to form a high-entropy ceramic anti-ablation coating with a single solid solution structure, and the interface strength between the transition layer and the coating is not high; if the temperature is too low, a high-entropy ceramic anti-ablation coating with a single solid solution structure cannot be formed at all. The sintering time must match the sintering temperature, and a lower temperature requires a longer insulation time. It is necessary to avoid overburning at higher temperatures, and to avoid grain growth caused by long-term insulation at lower temperatures. A lower heating rate will cause grain growth, and a higher heating rate can shorten the sintering time and improve efficiency, but it may cause overburning. It is more suitable within the above parameter range.

[0065] Among them, the sintering is spark plasma sintering, which integrates ion activation, hot pressing and resistance heating, has a fast heating rate, short sintering time, uniform grains, is conducive to controlling the fine structure of the sintered body, and obtains high density of the material. These advantages lead to the improvement of the material structure and can be effectively used to synthesize high entropy ceramics.

[0066] Furthermore, spark plasma sintering is used on the surface of the graphite substrate to simultaneously prepare the SiC transition layer and the high-entropy ceramic anti-ablative coating in one step, which greatly shortens the reaction time. Moreover, since the desired composite coating is obtained in one step by spark plasma sintering, the bonding force between the transition layer and the high-entropy ceramic anti-ablative coating is stronger, the high-entropy ceramic anti-ablative coating is denser, and it is more conducive to achieving precise control.

[0067] In a further preferred embodiment, the sintering comprises: heating from room temperature to 2000°C to 2200°C at a heating rate of 50 to 100°C / min, keeping the temperature for 7 to 10 minutes, and maintaining the sintering pressure at 15 MPa to 30 MPa.

[0068] In a further preferred embodiment, the sintering comprises: heating from room temperature to 2000° C. at a heating rate of 100° C. / min, keeping the temperature for 10 minutes, and maintaining the sintering pressure at 30 MPa.

[0069] In step 3, after sintering, the temperature is preferably lowered to 500-700° C. at a cooling rate of 20-100° C. / min, and then naturally cooled to room temperature.

[0070] Among them, the cooling rate is selected according to the thickness of the high-entropy ceramic anti-ablative coating. Symmetrical cooling to a certain temperature and then natural cooling is beneficial to protecting the performance of the high-entropy ceramic anti-ablative coating. Direct cooling after sintering will cause the high-entropy ceramic anti-ablative coating to crack during the rapid cooling process.

[0071] More preferably, after sintering, the temperature is lowered to 700-1000° C. at a cooling rate of 50-100° C. / min, and then naturally cooled to room temperature.

[0072] More preferably, after sintering, the temperature is lowered to 600° C. at a cooling rate of 66° C. / min, and then naturally cooled to room temperature.

[0073] In step 3, the normal temperature is generally 0-40°C, for example 25°C.

[0074] In step 3, a suitable DC pulse current needs to be set before sintering. The DC pulse current is usually set to 300-800A, preferably 300A. When the sintering is completed and the temperature is lowered to the required temperature, such as 600°C, the DC pulse current is turned off, and then naturally cooled to room temperature.

[0075] In step 3, before sintering, the sample is evacuated to below 6 Pa to prevent oxidation of the sample during high-temperature sintering and to improve the densification of the sample.

[0076] Furthermore, during the sintering process, an inert gas such as argon or helium is used as a protective gas, for example, argon is used as a protective gas. The protective gas needs to be introduced from before sintering to the cooling stage at room temperature after the sintering is completed. The protective gas is introduced to prevent the sintered sample from further reacting with residual oxygen at high temperature.

[0077] The present invention is further described below through specific examples, but these examples are merely exemplary and do not constitute any limitation to the scope of protection of the present invention.

[0078] Example 1

[0079] 1 mol TiC, 1 mol ZrC, 1 mol HfC and 1 mol TaC were mixed and placed in a ball mill for ball milling at 250 r / min for 6 h with a ball-to-material weight ratio of 5:1. After the ball milling, the ball-milled material was obtained for use.

[0080] Afterwards, a graphite substrate with a diameter of 30 mm and a mass of 13.55 g was placed on a graphite mold, Si powder was spread on the graphite substrate, and pressed on a tablet press at a pressure of 30 MPa for 15 min to complete a primary pressing to obtain a pre-pressed product, and then a ball mill (the mass ratio of the ball mill to the Si source was 15:1) was spread on the pre-pressed product, and pressed at a pressure of 30 MPa for 20 min to complete a secondary pressing to obtain a pressed product;

[0081] A graphite mold with a pressed object is placed in the furnace of a spark plasma sintering system, and the system is evacuated to below 6 Pa. Argon is introduced into the sintering system, and the DC pulse current is set to 300 A. The sintering is performed according to the following procedure: the temperature is increased from room temperature (25°C) to 2000°C at a heating rate of 100°C / min, and then the temperature is kept at 10 minutes. The sintering pressure is maintained at 30 MPa; then the temperature is reduced to 600°C at a cooling rate of 66°C / min, and the DC pulse current is turned off. The system is naturally cooled to room temperature to obtain a SiC-high entropy ceramic anti-ablation composite coating.

[0082] Figure 1 The XRD spectrum of the high entropy ceramic anti-ablation coating in the prepared SiC-high entropy ceramic anti-ablation composite coating is shown, and it can be seen that a single solid solution structure (FCC) has been formed.

[0083] Figure 2 The macroscopic image of the prepared SiC-high entropy ceramic anti-ablation composite coating is shown; Figure 3 The cross-sectional morphology of the prepared SiC-high entropy ceramic anti-ablation composite coating is shown. It can be seen that the thickness of the transition layer is about 40 μm, the thickness of the high entropy ceramic anti-ablation coating is 210 μm, the degree of densification is high, and there are no obvious holes. After testing, its density is 97.13%.

[0084] Figure 4 The element distribution diagram of Ti, Zr, Hf, Ta, Si and C in the prepared SiC-high entropy ceramic anti-ablation composite coating is shown, and the percentage content of the elements shown is shown in the following table:

[0085]

[0086] Example 2

[0087] 1 mol TiC, 1 mol ZrC, 1 mol HfC and 1 mol TaC were mixed and placed in a ball mill for ball milling at 250 r / min for 6 h with a ball-to-material weight ratio of 5:1. After the ball milling, the ball-milled material was obtained for use.

[0088] Afterwards, a graphite substrate with a diameter of 30 mm and a mass of 13.54 g was placed on a graphite mold, Si powder was spread on the graphite substrate, and pressed on a tablet press at a pressure of 30 MPa for 15 min to complete the primary pressing to obtain a pre-pressed product, and then a ball mill (the mass ratio of the ball mill to the Si source was 15:1) was spread on the pre-pressed product, and pressed at a pressure of 30 MPa for 20 min to complete the secondary pressing to obtain a pressed product;

[0089] A graphite mold with a pressed object is placed in the furnace of a spark plasma sintering system, and the vacuum is evacuated to below 6 Pa. Argon is introduced into the sintering system, and the DC pulse current is set to 350 A. The sintering is performed according to the following procedure: the temperature is increased from room temperature (25°C) to 1900°C at a heating rate of 100°C / min, and then the temperature is kept for 10 minutes. The sintering pressure is maintained at 30 MPa; then the temperature is reduced to 600°C at a cooling rate of 66°C / min, and the DC pulse current is turned off. The SiC-high entropy ceramic anti-ablation composite coating is naturally cooled to room temperature to obtain.

[0090] After testing, the thickness of the transition layer is 35μm and the thickness of the high-entropy ceramic anti-ablation coating is 200μm.

[0091] Example 3

[0092] 1 mol TiC, 1 mol ZrC, 1 mol HfC and 1 mol TaC were mixed and placed in a ball mill for ball milling at 250 r / min for 6 h with a ball-to-material weight ratio of 5:1. After the ball milling, the ball-milled material was obtained for use.

[0093] Afterwards, a graphite substrate with a diameter of 30 mm and a mass of 13.55 was placed on a graphite mold, Si powder was spread on the graphite substrate, and pressed on a tablet press at a pressure of 30 MPa for 15 min to complete the primary pressing to obtain a pre-pressed product, and then a ball mill (the mass ratio of the ball mill to the Si source was 15:1) was spread on the pre-pressed product, and pressed at a pressure of 30 MPa for 20 min to complete the secondary pressing to obtain a pressed product;

[0094] A graphite mold with a pressed object is placed in the furnace of a spark plasma sintering system, and the vacuum is evacuated to below 6 Pa. Argon is introduced into the sintering system, and the DC pulse current is set to 660A. The sintering is performed according to the following procedure: the temperature is increased from room temperature 25°C to 1700°C at a heating rate of 100°C / min, and the temperature is kept for 10 minutes. The sintering pressure is maintained at 30MPa; then the temperature is reduced to 600°C at a cooling rate of 66°C / min, and the DC pulse current is turned off. The SiC-high entropy ceramic anti-ablation composite coating is naturally cooled to room temperature to obtain.

[0095] After testing, the thickness of the transition layer is 30μm and the thickness of the high-entropy ceramic anti-ablation coating is 190μm.

[0096] Example 4

[0097] 1 mol TiC, 1 mol ZrC, 1 mol HfC and 1 mol TaC were mixed and placed in a ball mill for ball milling at 250 r / min for 6 h with a ball-to-material weight ratio of 5:1. After the ball milling, the ball-milled material was obtained for use.

[0098] Afterwards, a graphite substrate with a diameter of 30 mm and a mass of 13.45 g was placed on a graphite mold, Si powder was spread on the graphite substrate, and pressed on a tablet press at a pressure of 30 MPa for 15 min to complete the primary pressing to obtain a pre-pressed product, and then a ball mill (the mass ratio of the ball mill to the Si source was 15:1) was spread on the pre-pressed product, and pressed at a pressure of 30 MPa for 20 min to complete the secondary pressing to obtain a pressed product;

[0099] A graphite mold with a pressed object is placed in the furnace of a spark plasma sintering system, and the vacuum is evacuated to below 6 Pa. Argon is introduced into the sintering system, and the DC pulse current is set to 800 A. The sintering is performed according to the following procedure: the temperature is increased from room temperature (25°C) to 1600°C at a heating rate of 100°C / min, and then the temperature is kept for 10 minutes. The sintering pressure is maintained at 30 MPa; then the temperature is reduced to 600°C at a cooling rate of 66°C / min, and the DC pulse current is turned off. The SiC-high entropy ceramic anti-ablation composite coating is naturally cooled to room temperature to obtain.

[0100] After testing, the thickness of the transition layer is 28μm and the thickness of the high-entropy ceramic anti-ablation coating is 180μm.

[0101] Example 5

[0102] 1 mol TiC, 1 mol ZrC, 1 mol HfC and 1 mol TaC were mixed and placed in a ball mill for ball milling at 250 r / min for 6 h with a ball-to-material weight ratio of 5:1. After the ball milling, the ball-milled material was obtained for use.

[0103] Afterwards, a carbon base with a diameter of 30 mm and a mass of 13.44 g was placed on a graphite mold, Si powder was spread on the graphite substrate, and pressed on a tablet press at a pressure of 30 MPa for 15 min to complete the primary pressing to obtain a pre-pressed product, and then a ball mill (the mass ratio of the ball mill to the Si source was 15:1) was spread on the pre-pressed product, and pressed at a pressure of 30 MPa for 20 min to complete the secondary pressing to obtain a pressed product;

[0104] A graphite mold with a pressed object is placed in the furnace of a spark plasma sintering system, and the system is evacuated to below 6 Pa. Argon is introduced into the sintering system, and the DC pulse current is set to 800 A. The sintering is performed according to the following procedure: the temperature is increased from room temperature (25°C) to 1500°C at a heating rate of 100°C / min, and then the temperature is kept at 10 minutes. The sintering pressure is maintained at 30 MPa; then the temperature is reduced to 600°C at a cooling rate of 66°C / min, and the DC pulse current is turned off. The system is naturally cooled to room temperature to obtain a SiC-high entropy ceramic anti-ablation composite coating.

[0105] After testing, the thickness of the transition layer is 28μm and the thickness of the high-entropy ceramic anti-ablation coating is 200μm.

[0106] Figure 5 The XRD spectrum of the high entropy ceramic anti-ablation coating in the SiC-high entropy ceramic anti-ablation composite coating prepared in Example 3 is shown; Figure 6 The XRD spectrum of the high entropy ceramic anti-ablation coating in the SiC-high entropy ceramic anti-ablation composite coating prepared in Example 4 is shown; Figure 7 The XRD spectrum of the high entropy ceramic anti-ablation coating in the SiC-high entropy ceramic anti-ablation composite coating prepared in Example 5 is shown. It can be seen that the main peak of the high entropy ceramic anti-ablation coating in Example 5 appears to be split peaks and does not form a single solid solution phase.

[0107] The present invention is described in detail above in combination with preferred embodiments and exemplary examples. However, it should be noted that these specific embodiments are only illustrative explanations of the present invention and do not constitute any limitation on the protection scope of the present invention. Without exceeding the spirit and protection scope of the present invention, various improvements, equivalent substitutions or modifications may be made to the technical content of the present invention and its embodiments, which all fall within the protection scope of the present invention. The protection scope of the present invention shall be subject to the attached claims.

Claims

1. A SiC-high entropy ceramic anti-ablation composite coating, characterized in that: The composite coating uses SiC as a transition layer and (Ti Zr Hf Ta)X as a high-entropy ceramic anti-ablation coating, wherein X is B or C.

2. The composite coating according to claim 1, characterized in that: Preferably, the molar ratio of Ti, Zr, Hf and Ta in the high entropy ceramic anti-ablation coating is equimolar.

3. The composite coating according to claim 1, characterized in that: The thickness of the transition layer is 28-40 μm, and the thickness of the high-entropy ceramic anti-ablation coating is 180-210 μm.

4. A method for preparing the SiC-high entropy ceramic anti-ablation composite coating according to claim 1, characterized in that: The method comprises: Step 1, mixing a Ti source, a Zr source, a Hf source and a Ta source and ball-milling them to obtain a ball-milled product; Step 2, pressing the ball-milled product and Si powder on a graphite substrate to obtain a pressed product; Step 3: sintering the pressed product to obtain the SiC-high entropy ceramic anti-ablation composite coating.

5. The method according to claim 4, characterized in that In step 1, the Ti source is TiC or TiB, and the Zr source is ZrC or ZrB.

6. The method according to claim 4, characterized in that In step 1, the ball milling speed is 100 to 300 r / min.

7. The method according to claim 4, characterized in that In step 1, the ball milling time is 4 to 12 hours.

8. The method according to claim 4, characterized in that The step 2 comprises the following steps: Step 2-1, spreading the Si source on the graphite substrate and performing a pressing operation to obtain a pre-pressed product; Step 2-2: Spread the ball-milled material onto the pre-pressed material, and perform secondary pressing to obtain the pressed material.

9. The method according to claim 8, characterized in that In step 2-1, the Si source is Si powder.

10. The method according to claim 8, characterized in that In step 3, the sintering temperature is 1600°C to 2200°C.

Citation Information

Patent Citations

  • Method for preparing ZrB2-SiC anti-ablation coating from in-situ reaction

    CN103145454A

  • C / C composite material superhigh temperature ceramic coating, and preparation method thereof

    CN108530110A

  • SiC / HfB2-SiC-La2O3 / SiC ultra-high temperature oxidation resistant composite coating on graphite matrix

    CN111960830A

  • Long-life multi-element rare earth environmental barrier coating and preparation method thereof

    CN117051351A

  • Thermal and / or environmental barrier coating system

    EP3670481A1

Cited By

  • SiC-high-entropy carbide composite ceramic with high-temperature oxidation resistance as well as preparation method and application of SiC-high-entropy carbide composite ceramic

    CN119797943A

  • SiC-high-entropy carbide composite ceramic with high-temperature oxidation resistance and preparation method and application thereof

    CN119797943B