Morphology-adjustable mesoporous metal-polypolyphenol nanoparticles as well as preparation method and application thereof
By using formaldehyde prepolymerized tannic acid and m-trimethylbenzene as a pore expander, mesoporous metal-polyphenol nanoparticles were prepared by adjusting the reaction conditions. This solved the problem of unstable metal-polyphenol network structure, achieving high loading rate and tunable morphology, and improving the antioxidant properties and stability of fragrances.
Patent Information
- Application Number
- CN202411182141.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-08-27
AI Technical Summary
Existing metal-polyphenol network structures are not dense and have thin shells, which makes the fragrance prone to collapse and the core material to leak. Furthermore, the morphology is not adjustable, making it difficult to meet the requirements of high load rate and structural stability.
Mesoporous metal-polyphenol nanoparticles with tunable morphology were prepared by using formaldehyde prepolymerized tannic acid and m-trimethylbenzene as pore expanders and by adjusting the molar ratio of metal to polyphenol, stirring time, and the ratio of ethanol to deionized water. These nanoparticles formed solid or hollow shell structures, achieving high loading rate and structural stability.
The prepared mesoporous metal-polyphenol nanoparticles have high loading rate and stable structure, which can effectively improve the antioxidant properties of fragrances and solve the problem of poor chemical stability of easily oxidized fragrances through dual protection at both physical and chemical levels.
Smart Images

Figure CN119039602A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metal polyphenol materials, and in particular to a mesoporous metal-polyphenol nanoparticle with adjustable morphology, a preparation method and application thereof. Background Art
[0002] Metal-polyphenol networks are widely used as a multifunctional material for the coating and delivery of active substances. Polyphenols are widely present in various plants in nature, contain abundant phenolic hydroxyl groups, and have good adhesion, antibacterial, antioxidant, anti-inflammatory and anticancer effects. The polyhydroxy structure of polyphenols enables them to produce dynamic coordination bonds dominated by pH with various metals to form supramolecular network structures. Since polyphenols retain a large number of phenolic hydroxyl groups after coordination and complexation with metals, they still have good adhesion, antibacterial and antioxidant properties. At the same time, the metal-polyphenol network also has the characteristics of good biocompatibility, high mechanical strength and pH-responsive disassembly. At present, metal-polyphenol networks have been applied to the field of fragrance emulsions. The metal-polyphenol network film is in situ coated on the surface of the fragrance emulsion to form a capsule. The physical coating effect and antioxidant properties of the capsule shell can effectively solve the problem of poor chemical stability of easily oxidized fragrances. However, the existing metal-polyphenol network structure is not dense and the shell is thin, which makes it very easy to collapse and cause the core material to leak.
[0003] Therefore, there is an urgent need to develop metal-polyphenol nanoparticles with high loading rate, stable structure and adjustable morphology for use in the fields of flavor encapsulation and the like. Summary of the invention
[0004] The purpose of the present invention is to overcome the defects of the above-mentioned prior art and provide a morphology-adjustable mesoporous metal-polyphenol nanoparticle and its preparation method and application. The obtained mesoporous metal-polyphenol nanoparticle has a high loading rate and a stable structure, and can improve the antioxidant properties of spices.
[0005] The purpose of the present invention can be achieved by the following technical solutions:
[0006] The present invention provides a method for preparing mesoporous metal-polyphenol nanoparticles with adjustable morphology, comprising the following steps:
[0007] S1. First, add poloxamer 407 to ethanol and deionized water, then add ammonia water, stir to dissolve, then add tannic acid (TA) and formaldehyde, stir to obtain a polytannic acid (pTA) dispersion;
[0008] S2, first add poloxamer 407 to ethanol, stir to dissolve, then add the pTA dispersion obtained in S1 and m-trimethylbenzene, sonicate, then add the metal compound aqueous solution, stir, centrifuge, wash, and vacuum dry to obtain mesoporous metal-polyphenol (meso-pTA-MPN) nanoparticles;
[0009] The particle size of the mesoporous metal-polyphenol nanoparticles can be adjusted by the amount of the metal compound in S2, wherein the molar ratio of tannic acid to the metal compound is 1:(1-11);
[0010] The pore size of the mesoporous metal-polyphenol nanoparticles can be adjusted by the stirring time in S2, wherein the stirring time is 5s to 24h;
[0011] The structure of the mesoporous metal-polyphenol nanoparticles can be adjusted by the amount of ethanol and deionized water used, wherein the volume ratio of ethanol to deionized water is 1:1 or 1:(1.47-4). The ethanol is the sum of the volume of ethanol in the pTA dispersion obtained in S1 and the volume of ethanol added in S2, and the deionized water is the volume of deionized water in the pTA dispersion obtained in S1.
[0012] Furthermore, when the volume ratio of ethanol to deionized water is 1:1, the structure of the mesoporous metal-polyphenol nanoparticles is a solid structure.
[0013] Furthermore, when the volume ratio of ethanol to deionized water is 1:(1.47-4), the structure of the mesoporous metal-polyphenol nanoparticles can be adjusted to a hollow shell structure with a hollow interior and a solid shell layer on the exterior.
[0014] Under low ethanol concentration conditions, metal and polyphenol transitionally grow on the surface of TMB oil droplets and self-assemble through the Frank-vander Merwe mode to form a hollow shell structure; under high ethanol concentrations, metal and polyphenol self-assemble separately in the water phase and self-assemble in the interface separation mode to form a solid structure. The mesoporous metal-polyphenol nanoparticles with the hollow shell structure only exist under the condition that the volume ratio of ethanol to deionized water is 1: (1.47-4), and the solid structure is the mesoporous metal-polyphenol nanoparticles commonly present in the present invention.
[0015] Furthermore, in S1, the mass ratio of poloxamer 407, ammonia water, TA and formaldehyde is 1:(1-4):1:(1-4).
[0016] Furthermore, in S1, the stirring time is 12 to 36 hours.
[0017] Furthermore, in S2, the mass ratio of poloxamer 407, TA, meta-trimethylbenzene and the metal compound is 1:(0.01-0.4):(1-5):(0.1-0.4).
[0018] Furthermore, in S2, the metal compound is any one of ferric chloride hexahydrate, anhydrous copper sulfate, and cobalt nitrate hexahydrate, the solvent for the centrifugal washing is ethanol and deionized water, and the vacuum drying temperature is 50-70°C.
[0019] Furthermore, in S2, the ultrasonic power is 200 W and the ultrasonic time is 2 minutes.
[0020] Furthermore, in S1 and S2, the stirring method is magnetic stirring, and the rotation speed is 400-600 rpm.
[0021] The present invention also provides a mesoporous metal-polyphenol nanoparticle with adjustable morphology, wherein the particle size of the mesoporous metal-polyphenol nanoparticle is 144.50-480.22 nm; the pore size of the nanoparticle is 2.33-12.56 nm;
[0022] The present invention also provides an application of mesoporous metal-polyphenol nanoparticles with adjustable morphology, wherein the mesoporous metal-polyphenol nanoparticles can be used to load spices, and the spices are citral, cinnamaldehyde or eugenol;
[0023] The specific fragrance loading process is as follows: first add poloxamer 407 to ethanol, then add the polytannic acid dispersion obtained in S1, as well as citral or cinnamaldehyde or eugenol, and a metal compound aqueous solution in sequence, stir, centrifuge and wash, and vacuum dry to obtain mesoporous metal-polyphenol nanoparticles loaded with different fragrances.
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] (1) The present invention uses formaldehyde to prepolymerize tannic acid to increase the molecular weight of tannic acid, thereby preparing mesoporous metal-polyphenol nanoparticles with stable structure, high loading rate and adjustable morphology, solving the problem of unstable and easy collapse of traditional metal-polyphenol network structure.
[0026] (2) The present invention can be used to prepare mesoporous metal-polyphenol nanoparticles of different particle sizes by adjusting the molar ratio of metal to polyphenol.
[0027] (3) The present invention uses m-trimethylbenzene as a pore-enlarging agent. Compared with traditional metal-polyphenol nanoparticles, mesoporous metal-polyphenol nanoparticles with larger surface pore size can be obtained, and the pore size of the particles can be controlled by simply adjusting the reaction time.
[0028] (4) The present invention can precisely control the shape of mesoporous metal-polyphenol nanoparticles by simply regulating the reaction system, and can obtain a hollow shell structure with a hollow interior and a solid shell layer on the exterior.
[0029] (5) The present invention prepares mesoporous metal-polyphenol nanoparticles loaded with spices by a one-step method, achieving dual protection of spices at the physical and chemical levels, and can effectively solve the problem of poor chemical stability of easily oxidized spices. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 This is a scanning electron micrograph of meso-pTA-MPN nanoparticles prepared in Example 1;
[0031] Figure 2 This is a transmission electron microscopy image of meso-pTA-MPN nanoparticles prepared in Example 1;
[0032] Figure 3 It is the UV spectra of pTA, ferric chloride and meso-pTA-MPN shown in Example 1;
[0033] Figure 4 This is a scanning electron micrograph of meso-pTA-MPN nanoparticles prepared in Example 2;
[0034] Figure 5 This is a scanning electron micrograph of meso-pTA-MPN nanoparticles prepared in Example 3;
[0035] Figure 6 The scanning electron micrographs of meso-pTA-MPN nanoparticles prepared with different metal usage amounts in Example 4;
[0036] Figure 7 is a scanning electron micrograph of the hollow shell meso-pTA-MPN shown in Example 5;
[0037] Figure 8 is a transmission electron microscopy image of the hollow shell meso-pTA-MPN shown in Example 5;
[0038] Fig. 9 is a scanning electron micrograph of meso-pTA-MPN with different mesopore sizes as shown in Example 6;
[0039] Fig.10 is a scanning electron micrograph of meso-pTA-MPN nanoparticles loaded with different fragrances as shown in Example 7;
[0040] Fig.11 This is the ABTS scavenging effect of meso-pTA-MPN shown in Example 8. DETAILED DESCRIPTION
[0041] The present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. Any features such as preparation means, materials, structures or composition ratios not clearly described in this technical solution are regarded as common technical features disclosed in the prior art.
[0042] The reactions in all the embodiments of the present invention were carried out at room temperature.
[0043] Example 1
[0044] A method for preparing mesoporous metal-polyphenol nanoparticles with adjustable morphology comprises the following steps:
[0045] S1. Preparation of pTA dispersion:
[0046] Weigh 0.20 g of poloxamer 407, add it to a mixed solution of 5.00 mL of ethanol and 25.00 mL of deionized water, stir thoroughly to dissolve, use a pipette to take 0.5 mL of ammonia water and add it to the above solution, and stir for 1 h; weigh 0.20 g of tannic acid, add it to the above solution, stir thoroughly to dissolve, use a pipette to take 0.40 mL of formaldehyde solution and add it to the above solution, and stir for 24 h to obtain a pTA dispersion;
[0047] S2. Preparation of meso-pTA-MPN nanoparticles:
[0048] Weigh 1.00 g of poloxamer 407, add it to 20.00 mL of ethanol, stir thoroughly to dissolve, add the pTA dispersion obtained in S1 to the above solution, and stir thoroughly; use a pipette to take 1.20 mL of m-trimethylbenzene and add it to the above solution, use an ultrasonic cell crusher, and ultrasonicate at 200 W for 2 minutes to obtain a composite micelle emulsion; then weigh 0.10 g of ferric chloride hexahydrate and add it to 2.00 mL of deionized water to prepare an aqueous solution of ferric chloride, add the aqueous solution of ferric chloride to the above composite micelle emulsion, and stir for 24 hours; after the reaction is completed, wash the solution twice with 50% ethanol solution, wash once with deionized water, and vacuum dry at 50°C for 12 hours to obtain meso-pTA-MPN nanoparticles.
[0049] The meso-pTA-MPN nanoparticles prepared in Example 1 were characterized by scanning electron microscopy. Figure 1 As shown, the average particle size of the meso-pTA-MPN nanoparticles in the figure is 347.60 nm, and the scale bar in the figure is 200 nm.
[0050] The meso-pTA-MPN nanoparticles prepared in Example 1 were characterized by transmission electron microscopy. Figure 2 As shown, the scale bar in the figure is 200nm.
[0051] Figure 3The UV spectra of pTA, ferric chloride, and meso-pTA-MPN show that an obvious LMCT band appears at a wavelength of 400 to 600 nm, which proves the coordination of iron ions with polyphenols.
[0052] Example 2
[0053] A method for preparing mesoporous metal-polyphenol nanoparticles with adjustable morphology comprises the following steps:
[0054] S1. Preparation of pTA dispersion:
[0055] Weigh 0.20 g of poloxamer 407, add it to a mixed solution of 5.00 mL of ethanol and 25.00 mL of deionized water, stir thoroughly to dissolve, use a pipette to take 0.5 mL of ammonia water and add it to the above solution, and stir for 1 h; weigh 0.20 g of tannic acid, add it to the above solution, stir thoroughly to dissolve, use a pipette to take 0.40 mL of formaldehyde solution and add it to the above solution, and stir for 24 h to obtain a pTA dispersion;
[0056] S2. Preparation of meso-pTA-MPN nanoparticles:
[0057] Weigh 1.00 g of poloxamer 407, add it to 20.00 mL of ethanol, stir thoroughly to dissolve, add the pTA dispersion obtained in S1 to the above solution, and stir thoroughly; use a pipette to take 1.20 mL of m-trimethylbenzene and add it to the above solution, use an ultrasonic cell crusher, ultrasonicate at 200 W for 2 minutes to obtain a composite micelle emulsion; then weigh 0.10 g of anhydrous copper sulfate and add it to 2.00 mL of deionized water to prepare a copper sulfate aqueous solution, add the copper sulfate aqueous solution to the above composite micelle emulsion, and stir for 24 hours; after the reaction is completed, wash the solution twice with 50% ethanol solution, wash once with deionized water, and vacuum dry at 50°C for 12 hours to obtain meso-pTA-MPN nanoparticles.
[0058] The meso-pTA-MPN nanoparticles prepared in Example 2 were characterized by scanning electron microscopy. Figure 4 As shown, the average particle size of the meso-pTA-MPN nanoparticles in the figure is 242.65 nm, and the scale bar in the figure is 200 nm.
[0059] Example 3
[0060] A method for preparing mesoporous metal-polyphenol nanoparticles with adjustable morphology comprises the following steps:
[0061] S1. Preparation of pTA dispersion:
[0062] Weigh 0.20 g of poloxamer 407, add it to a mixed solution of 5.00 mL of ethanol and 25.00 mL of deionized water, stir thoroughly to dissolve, use a pipette to take 0.5 mL of ammonia water and add it to the above solution, and stir for 1 h; weigh 0.20 g of tannic acid, add it to the above solution, stir thoroughly to dissolve, use a pipette to take 0.40 mL of formaldehyde solution and add it to the above solution, and stir for 24 h to obtain a pTA dispersion;
[0063] S2. Preparation of meso-pTA-MPN nanoparticles:
[0064] Weigh 1.00 g of poloxamer 407, add it to 20.00 mL of ethanol, stir thoroughly to dissolve, add the pTA dispersion obtained in S1 to the above solution, and stir thoroughly; use a pipette to take 1.20 mL of m-trimethylbenzene and add it to the above solution, use an ultrasonic cell crusher, and ultrasonicate at 200 W for 2 minutes to obtain a composite micelle emulsion; then weigh 0.10 g of cobalt nitrate hexahydrate and add it to 2.00 mL of deionized water to prepare a cobalt nitrate aqueous solution, add the cobalt nitrate aqueous solution to the above composite micelle emulsion, and stir for 24 hours; after the reaction is completed, wash the solution twice with 50% ethanol solution, wash once with deionized water, and vacuum dry at 50°C for 12 hours to obtain meso-pTA-MPN nanoparticles.
[0065] The meso-pTA-MPN nanoparticles prepared in Example 3 were characterized by scanning electron microscopy. Figure 5 As shown, the average particle size of the meso-pTA-MPN nanoparticles in the figure is 349.15 nm, and the scale bar in the figure is 200 nm.
[0066] Example 4
[0067] By adjusting the amount of ferric chloride hexahydrate used, meso-pTA-MPN nanoparticles with different particle sizes can be obtained.
[0068] S1. Preparation of pTA dispersion:
[0069] Weigh 0.20 g of poloxamer 407, add it to a mixed solution of 5.00 mL of ethanol and 25.00 mL of deionized water, stir thoroughly to dissolve, use a pipette to take 0.5 mL of ammonia water and add it to the above solution, and stir for 1 h; weigh 0.20 g of tannic acid, add it to the above solution, stir thoroughly to dissolve, use a pipette to take 0.40 mL of formaldehyde solution and add it to the above solution, and stir for 24 h to obtain a pTA dispersion;
[0070] S2. Preparation of meso-pTA-MPN nanoparticles:
[0071] Weigh 1.00 g of poloxamer 407, add it to 20.00 mL of ethanol, stir thoroughly to dissolve, add the pTA dispersion obtained in S1 to the above solution, and stir thoroughly; use a pipette to take 1.20 mL of m-trimethylbenzene and add it to the above solution, use an ultrasonic cell crusher, ultrasonicate at 200 W for 2 minutes to obtain a composite micellar emulsion; weigh 0.03, 0.10, 0.15, 0.21, 0.27, and 0.33 g of ferric chloride hexahydrate, respectively, and add them to 2.00 mL of deionized water to prepare an aqueous solution of ferric chloride, add the aqueous solution of ferric chloride to the above composite micellar emulsion, and stir for 24 hours; after the reaction is completed, wash the solution twice with 50% ethanol solution, wash once with deionized water, and vacuum dry at 50°C for 12 hours to obtain meso-pTA-MPN nanoparticles of different particle sizes.
[0072] The meso-pTA-MPN nanoparticles prepared in Example 4 were characterized by scanning electron microscopy. Figure 6 As shown, the particle size of the meso-pTA-MPN nanoparticles in the figure can be controlled in the range of 144.50 to 480.22 nm, and the scale bar in the figure is 200 nm. Among them, Figure ⅰ shows the meso-pTA-MPN nanoparticles obtained by adding 0.03g of ferric chloride hexahydrate, with a particle size of 144.50nm, Figure ⅱ shows the meso-pTA-MPN nanoparticles obtained by adding 0.10g of ferric chloride hexahydrate, with a particle size of 209.74nm, Figure ⅲ shows the meso-pTA-MPN nanoparticles obtained by adding 0.15g of ferric chloride hexahydrate, with a particle size of 251.89nm, Figure ⅳ shows the meso-pTA-MPN nanoparticles obtained by adding 0.21g of ferric chloride hexahydrate, with a particle size of 313.24nm, Figure ⅴ shows the meso-pTA-MPN nanoparticles obtained by adding 0.27g of ferric chloride hexahydrate, with a particle size of 347.6nm, and Figure ⅵ shows the meso-pTA-MPN nanoparticles obtained by adding 0.33g of ferric chloride hexahydrate, with a particle size of 480.22nm.
[0073] Example 5
[0074] By adjusting the amount of ethanol and deionized water used, meso-pTA-MPNs with different structures can be obtained.
[0075] S1. Preparation of pTA dispersion:
[0076] Weigh 0.20 g of poloxamer 407, add it to a mixed solution of 5.00 mL of ethanol and 25.00 mL of deionized water, stir thoroughly to dissolve, use a pipette to take 0.5 mL of ammonia water and add it to the above solution, and stir for 1 h; weigh 0.20 g of tannic acid, add it to the above solution, stir thoroughly to dissolve, use a pipette to take 0.40 mL of formaldehyde solution and add it to the above solution, and stir for 24 h to obtain a pTA dispersion;
[0077] S21. Preparation of meso-pTA-MPN nanoparticles:
[0078] Weigh 0.50 g of poloxamer 407, add it to 1.25 mL of ethanol, stir thoroughly to dissolve, add the pTA dispersion obtained in S1 to the above solution, and stir thoroughly; use a pipette to take 0.50 mL of m-trimethylbenzene and add it to the above solution, use an ultrasonic cell crusher, and ultrasonicate at 200 W for 2 minutes to obtain a composite micelle emulsion; weigh 0.10 g of ferric chloride hexahydrate and add it to 2.00 mL of deionized water to prepare an aqueous solution of ferric chloride, add the aqueous solution of ferric chloride to the above composite micelle emulsion, and stir for 24 hours; after the reaction is completed, wash the solution twice with 50% ethanol solution, wash once with deionized water, and vacuum dry at 50°C for 12 hours to obtain meso-pTA-MPN nanoparticles.
[0079] S22. Preparation of meso-pTA-MPN nanoparticles:
[0080] Weigh 1.00 g of poloxamer 407, add it to 12.00 mL of ethanol, stir thoroughly to dissolve, add the pTA dispersion obtained in S1 to the above solution, and stir thoroughly; use a pipette to take 1.00 mL of m-trimethylbenzene and add it to the above solution, use an ultrasonic cell crusher, and ultrasonicate at 200 W for 2 minutes to obtain a composite micelle emulsion; weigh 0.10 g of ferric chloride hexahydrate and add it to 2.00 mL of deionized water to prepare an aqueous solution of ferric chloride, add the aqueous solution of ferric chloride to the above composite micelle emulsion, and stir for 24 hours; after the reaction is completed, wash the solution twice with 50% ethanol solution, wash once with deionized water, and vacuum dry at 50°C for 12 hours to obtain meso-pTA-MPN nanoparticles.
[0081] The meso-pTA-MPN nanoparticles prepared in Example 5 were characterized by scanning electron microscopy and transmission electron microscopy, as shown in the figure. Figure 7 and 8 The morphology of the meso-pTA-MPN nanoparticles in the figure is hollow shell particles. The average particle size of the hollow shell particles in the figure is 388.67±40.31 nm, and the scale bar in the figure is 200 nm.
[0082] Example 6
[0083] By adjusting the stirring time in S2, meso-pTA-MPN nanoparticles with different pore sizes can be obtained.
[0084] S1. Preparation of pTA dispersion:
[0085] Weigh 0.20 g of poloxamer 407, add it to a mixed solution of 5.00 mL of ethanol and 25.00 mL of deionized water, stir thoroughly to dissolve, use a pipette to take 0.5 mL of ammonia water and add it to the above solution, and stir for 1 h; weigh 0.20 g of tannic acid, add it to the above solution, stir thoroughly to dissolve, use a pipette to take 0.40 mL of formaldehyde solution and add it to the above solution, and stir for 24 h to obtain a pTA dispersion;
[0086] S2. Preparation of meso-pTA-MPN nanoparticles:
[0087] Weigh 1.00 g of poloxamer 407, add it to 20.00 mL of ethanol, stir thoroughly to dissolve, add the pTA dispersion obtained in S1 to the above solution, and stir thoroughly; use a pipette to take 2.00 mL of m-trimethylbenzene and add it to the above solution, use an ultrasonic cell crusher, ultrasonicate at 200 W for 2 minutes to obtain a composite micellar emulsion; weigh 0.10 g of ferric chloride hexahydrate and add it to 2.00 mL of deionized water to prepare an aqueous solution of ferric chloride, add the aqueous solution of ferric chloride to the above composite micellar emulsion, and take the products obtained by stirring for 5 seconds, 5 minutes, 10 minutes, 30 minutes, and 24 hours respectively; after the reaction is completed, wash the solution twice with 50% ethanol solution, wash once with deionized water, and vacuum dry at 50°C for 12 hours to obtain meso-pTA-MPN nanoparticles with different pore sizes.
[0088] The meso-pTA-MPN prepared in Example 6 was characterized by scanning electron microscopy, as shown in the figure. Fig. 9 The pore size of the meso-pTA-MPN nanoparticles can be controlled in the range of 2.33 to 12.56 nm, and the scale bar in the figure is 200 nm. The average pore size of the meso-pTA-MPN nanoparticles prepared by stirring for 5 seconds is 8.32 nm, the average pore size of the meso-pTA-MPN nanoparticles prepared by stirring for 5 minutes is 10.94 nm, the average pore size of the meso-pTA-MPN nanoparticles prepared by stirring for 10 minutes is 11.44 nm, the average pore size of the meso-pTA-MPN nanoparticles prepared by stirring for 30 minutes is 12.56 nm, and the average pore size of the meso-pTA-MPN nanoparticles prepared by stirring for 24 hours is 2.33 nm.
[0089] Example 7
[0090] The meso-pTA-MPN nanoparticles prepared in this example can be used to load fragrances.
[0091] S1. Preparation of pTA dispersion:
[0092] Weigh 0.20 g of poloxamer 407, add it to a mixed solution of 5.00 mL of ethanol and 25.00 mL of deionized water, stir thoroughly to dissolve, use a pipette to take 0.5 mL of ammonia water and add it to the above solution, and stir for 1 h; weigh 0.20 g of tannic acid, add it to the above solution, stir thoroughly to dissolve, use a pipette to take 0.40 mL of formaldehyde solution and add it to the above solution, and stir for 24 h to obtain a pTA dispersion;
[0093] S2. Preparation of meso-pTA-MPN nanoparticles:
[0094] Weigh 1.00 g of poloxamer 407, add it to 20.00 mL of ethanol, stir thoroughly to dissolve, add the pTA dispersion obtained in S1 to the above solution, and stir thoroughly; use a pipette to take 2.00 mL of citric acid, cinnamaldehyde, and eugenol respectively and add them to the above solution, use an ultrasonic cell crusher, and ultrasonicate at 200 W for 2 minutes to obtain a composite micelle emulsion; weigh 0.10 g of ferric chloride hexahydrate and add it to 2.00 mL of deionized water to prepare an aqueous solution of ferric chloride, add the aqueous solution of ferric chloride to the above composite micelle emulsion, and stir for 24 hours; after the reaction is completed, wash the solution twice with 50% ethanol solution, wash once with deionized water, and vacuum dry at 50°C for 12 hours to obtain meso-pTA-MPN nanoparticles loaded with different fragrances.
[0095] The meso-pTA-MPN nanoparticles prepared in Example 7 were characterized by scanning electron microscopy. As shown in Figure 10, the average particle sizes of the three meso-pTA-MPN loaded with spices were 174.49 nm, 197.31 nm, and 207.68 nm, respectively, and the scale in the figure was 200 nm. Figure ⅰ shows meso-pTA-MPN nanoparticles loaded with citral, with a particle size of 174.94 nm, Figure ⅱ shows meso-pTA-MPN nanoparticles loaded with cinnamaldehyde, with a particle size of 197.31 nm, and Figure ⅲ shows meso-pTA-MPN nanoparticles loaded with eugenol, with a particle size of 207.68 nm.
[0096] Example 8
[0097] In vitro experiments were conducted on the meso-pTA-MPN nanoparticles prepared by stirring for 30 minutes in Example 6 to demonstrate that they have good flavoring and antioxidant effects.
[0098] The meso-pTA-MPN nanoparticles were dispersed in anhydrous ethanol to form a 5.00 mg / mL dispersion, and a 7.00 mM solution of 2,2-azino-bis(3-ethyl-benzothiazole-6-sulfonic acid) diammonium salt (ABTS) and a 2.45 mM potassium persulfate (K2S2O8) solution were prepared, and a phosphate buffer solution (PBS, 10.00 mM, pH = 7.40) was prepared; the ABTS solution and K2S2O8 The solutions were mixed at a mass ratio of 1:3-7 and placed in the dark for 24 hours as a stock solution; the stock solution was mixed with different sample solutions at a mass ratio of 147:80, 147:200, and 147:400 (i.e., the concentrations of the meso-pTA-MPN dispersions were 4.00 g / mL, 10.00 g / mL, and 20.00 g / mL), incubated in the dark for 30 minutes, and then transferred to a cuvette, and the absorbance was measured at 734 nm.
[0099] like Fig.11 As shown in the figure, with the increase of sample concentration, its absorbance at 734 nm decreases continuously, indicating that the meso-pTA-MPN material has good antioxidant properties.
[0100] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.
Claims
1. A method for preparing morphology-adjustable mesoporous metal-polyphenol nanoparticles, characterized in that: The following steps are involved: S1. First, add poloxamer 407 to ethanol and deionized water, then add ammonia water, stir to dissolve, then add tannic acid and formaldehyde, stir to obtain a polytannic acid dispersion; S2, first add poloxamer 407 to ethanol, then add the polytannic acid dispersion obtained in S1, m-trimethylbenzene, and a metal compound aqueous solution in sequence, stir, centrifuge, wash, and vacuum dry to obtain mesoporous metal-polyphenol nanoparticles; The particle size of the mesoporous metal-polyphenol nanoparticles can be adjusted by the amount of the metal compound in S2, wherein the molar ratio of tannic acid to the metal compound is 1:(1-11); The pore size of the mesoporous metal-polyphenol nanoparticles can be adjusted by the stirring time in S2, wherein the stirring time is 5s to 24h; The structure of the mesoporous metal-polyphenol nanoparticles can be adjusted by the usage of ethanol and deionized water, wherein the volume ratio of ethanol to deionized water is 1:1 or 1:(1.47-4).
2. The method for preparing morphology-adjustable mesoporous metal-polyphenol nanoparticles according to claim 1, characterized in that: In S1, the mass ratio of poloxamer 407, ammonia water, tannic acid and formaldehyde is 1:(1-4):1:(1-4), and the stirring time is 12-36 hours.
3. The method for preparing morphology-adjustable mesoporous metal-polyphenol nanoparticles according to claim 1, characterized in that: In S2, the mass ratio of poloxamer 407, tannic acid, meta-trimethylbenzene and metal compound is 1:(0.01-0.4):(1-5):(0.1-0.4).
4. The method for preparing morphology-adjustable mesoporous metal-polyphenol nanoparticles according to claim 1, characterized in that: In S2, the metal compound is any one of ferric chloride hexahydrate, anhydrous copper sulfate, and cobalt nitrate hexahydrate.
5. The method for preparing morphology-adjustable mesoporous metal-polyphenol nanoparticles according to claim 1, characterized in that: In S2, the solvents for the centrifugal washing are ethanol and deionized water.
6. The method for preparing morphology-adjustable mesoporous metal-polyphenol nanoparticles according to claim 1, characterized in that: In S2, the vacuum drying temperature is 50-70°C.
7. The method for preparing morphology-adjustable mesoporous metal-polyphenol nanoparticles according to claim 1, characterized in that: In S1 and S2, the stirring method is magnetic stirring, and the rotation speed is 400-600 rpm.
8. The method for preparing morphology-adjustable mesoporous metal-polyphenol nanoparticles according to claim 1, characterized in that: The mesoporous metal-polyphenol nanoparticles can be adjusted to have a hollow shell structure with a hollow interior and a solid shell layer on the exterior, wherein the volume ratio of ethanol to deionized water is 1:(1.47-4).
9. A mesoporous metal-polyphenol nanoparticle prepared by the method according to any one of claims 1 to 8, characterized in that: The particle size of the mesoporous metal-polyphenol nanoparticles is 144.50-480.22 nm; the pore size of the nanoparticles is 2.33-12.56 nm.
10. A use of the mesoporous metal-polyphenol nanoparticles as claimed in claim 9, characterized in that: The mesoporous metal-polyphenol nanoparticles can be used to load spices, and the spices include any one of citral, cinnamaldehyde or eugenol; The specific fragrance loading process is as follows: first add poloxamer 407 to ethanol, then add the polytannic acid dispersion obtained in S1, as well as citral or cinnamaldehyde or eugenol, and a metal compound aqueous solution in sequence, stir, centrifuge and wash, and vacuum dry to obtain mesoporous metal-polyphenol nanoparticles loaded with different fragrances.
Citation Information
Patent Citations
Single micelle metal-polyphenol nano material as well as preparation and application thereof
CN116725966A
Large-aperture mesoporous metal-polyphenol complex nanosphere and preparation method thereof
CN117229559A
Metal polyphenol nanoparticle, preparation method thereof and application of metal polyphenol nanoparticle in preparation of TMEM16A inhibitor
CN117510880A
Cited By
Novel metal-polyphenol microspheres as well as preparation method and application thereof
CN121265809A