Low-wear high-wear-resistance polytetrafluoroethylene-based composite material and preparation method thereof

By preparing low-wear and high-wear-resistant polytetrafluoroethylene (PTFE) vinyl composite materials, the problem of insufficient wear resistance of PTFE piston rings under high load and high temperature conditions was solved, and the wear resistance and self-lubricating properties of the material were improved, thus extending the service life of the components.

CN119039719APending Publication Date: 2024-11-29WUXI JIUAN SHUNCHANG COMPRESSOR PARTS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410867129.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-18
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The polytetrafluoroethylene piston rings used in existing new hydrogen compressors have insufficient wear resistance under high load and high temperature conditions, resulting in a short service life.

Method used

The material is made of low-wear and high-wear-resistant polytetrafluoroethylene composite material, which includes polytetrafluoroethylene, pitch-coated modified titanium dioxide whiskers, basalt fibers and nano-oxide particles. It is mixed and molded through a specific process to form an interlaced structure to improve the wear resistance and self-lubrication of the material.

Benefits of technology

It significantly improves the wear resistance and self-lubricating properties of the material, extends the service life of components, and meets the needs of long-term wear-resistant applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119039719A_ABST
    Figure CN119039719A_ABST
Patent Text Reader

Abstract

The invention discloses a low-wear high-wear-resistance polytetrafluoroethylene-based composite material and a preparation method thereof. The composite material is prepared from the following components in percentage by weight: 60 to 75 percent of polytetrafluoroethylene, 10 to 25 percent of poly-p-hydroxybenzoate, 5 to 10 percent of asphalt coated modified titanium oxide whisker, 5 to 10 percent of basalt fiber and 1 to 5 percent of nano oxide particles. The asphalt-coated modified titanium oxide whisker is prepared by the following steps: dissolving modified asphalt in an organic solvent, adding titanium oxide whisker while stirring, and heating until the organic solvent is completely volatilized to finish coating; the coated titanium oxide whiskers are subjected to carbonization treatment, and the carbonization treatment process comprises the steps that the temperature is increased to 310 DEG C at the speed of 2 DEG C / min, the constant temperature is kept for 2 h, the temperature is continuously increased to 1000 DEG C at the speed of 22 DEG C / min, and the constant temperature is kept for 2 h. The material is suitable for the fields where long-term wear-resistant application is needed, such as bearings, sliding blocks, sealing pieces and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of inorganic material composites, and in particular to a low-wear and high-wear-resistant polytetrafluoroethylene-based composite material and a preparation method thereof. Background Art

[0002] At present, most of the new hydrogen compressors in the hydrogenation units of chemical plants use reformed hydrogen, which has a low purity (about 91%) and contains about 9% light hydrocarbon components. The light hydrocarbons will condense in the compressor cylinder. If the upstream PSA absorption unit does not treat well, activated carbon powder will be entrained in the hydrogen. If the oil injection amount is not appropriate, the powder and lubricating oil will mix to form a grinding paste, causing rapid damage to the piston ring and even cylinder pulling.

[0003] The piston rings and support rings used in new hydrogen compressors are filled with polytetrafluoroethylene. The wear resistance of polytetrafluoroethylene is still insufficient in certain high-load and high-temperature applications, resulting in a piston ring service life of only about 2-3 months. Summary of the invention

[0004] The object of the present invention is to provide a low-wear and high-wear-resistant polytetrafluoroethylene-based composite material and a preparation method thereof in view of the above-mentioned problems.

[0005] On the one hand, the low-wear and high-wear-resistant polytetrafluoroethylene-based composite material provided by the present invention comprises the following components in weight percentage: 60-75% polytetrafluoroethylene, 10-25% polyparahydroxybenzoate, 5-10% asphalt-coated modified titanium oxide whiskers, 5-10% basalt fibers and 1-5% nano-oxide particles;

[0006] The asphalt-coated modified titanium oxide whisker is prepared by the following steps:

[0007] Dissolve the modified asphalt in an organic solvent, add titanium oxide whiskers while stirring, and heat until the organic solvent is completely volatilized to complete the coating;

[0008] The coated titanium oxide whiskers were carbonized, wherein the carbonization process was as follows: heating to 310°C at 2°C / min, maintaining the temperature for 2 hours, and then heating to 1000°C at 22°C / min, maintaining the temperature for 2 hours.

[0009] In some embodiments, the organic solvent is selected from carbon tetrachloride, benzene or a mixture thereof.

[0010] In some embodiments, the nano-oxide particles are selected from one or more of nano-aluminum oxide, nano-silicon oxide, nano-calcium oxide, nano-magnesium oxide, or nano-zinc oxide.

[0011] In some embodiments, the asphalt-coated modified titanium oxide whiskers have an average length of 5-10 μm and an average diameter of 0.2-0.5 μm, the basalt fibers have an average length of 20-50 μm and an average diameter of 4-6 μm, and the nano-oxide particles have a particle size of 10-100 nm.

[0012] In some embodiments, the titanium oxide whisker is a mesoporous titanium oxide whisker with a pore volume of 0.05-0.4 cm 3 / g, specific surface area>30m 2 / g

[0013] In some embodiments, the titanium oxide whiskers are prepared by the following steps:

[0014] Metatitanic acid and potassium carbonate are mixed uniformly at TiO2 / K2O=2.5 mol, and sintered at 600-800°C for 30 min to obtain a mixture of potassium dititanate and potassium tetratitanate;

[0015] The mixture of potassium dititanate and potassium tetratitanate is immersed in a hydrochloric acid solution and stirred until the potassium content in the solid phase is less than 5wt% of the product weight;

[0016] After washing with water and filtering, it is calcined in a muffle furnace at 500-800°C for 0.5-8h.

[0017] On the other hand, the present invention provides a method for preparing a low-wear and high-wear-resistant polytetrafluoroethylene-based composite material, comprising the following steps:

[0018] A polytetrafluoroethylene matrix, asphalt-coated modified titanium oxide whiskers, basalt fibers and nano-oxide particles are mixed to obtain a mixture, polyparahydroxybenzoate is dissolved in alcohol, and then added to the mixture, and dispersed by high-shear stirring, after being mixed evenly, the solvent is removed by suction filtering, and then dried;

[0019] First, add the dried mixed material into a metal mold, place it on a press, and heat it to 150°C for preheating;

[0020] After the temperature inside and outside the mold is constant, pre-press at a pressure of 3.5-7Mpa. Maintain the pressure and start a certain heating rate to the final molding temperature;

[0021] When the temperature is constant, release the pressure to let the air out, and then immediately apply the final molding pressure. The holding time depends on the size and thickness of the product.

[0022] Release the pressure, stop heating, move the mold onto the insulation blanket, slowly cool down to 200℃, then quickly cool down and demould at around 100℃.

[0023] In some embodiments, the final molding temperature is 20-200° C., and the final molding pressure is 20-200 MPa.

[0024] On the other hand, the low-wear and high-wear-resistant polytetrafluoroethylene-based composite material provided by the present invention is used in fields such as bearings, sliders, and seals that require long-term wear resistance.

[0025] On the other hand, the composite material obtained by the preparation method provided by the present invention is used in the fields of bearings, sliders, seals, etc. that require long-term wear resistance.

[0026] Compared with the prior art, the present invention has the following beneficial effects:

[0027] 1. The present invention interlaces coarse basalt fibers and fine titanium oxide whiskers to form a refractory fibrous filler. The fibers are interlaced to provide a load-bearing skeleton for the refractory polyparahydroxybenzoate, which has a binding effect on the polyparahydroxybenzoate. The exposed fiber part on the wear surface replaces the matrix and directly carries the load, which reduces the interaction between the resin and the dual surface, and makes the composite material subject to less shear force, thereby reducing friction and wear.

[0028] 2. The present invention improves the internal density of the composite material and the interfacial bonding strength by filling the nano-oxide particles. At the same time, the nano-oxide particles greatly increase the hardness of PTFE, and the plastic deformation caused by plowing under load is small, so that the composite material exhibits better wear resistance.

[0029] 3. The present invention coats mesoporous titanium oxide whiskers with asphalt and then carbonizes them. On the one hand, the asphalt adsorbed in the mesopores on the surface of the titanium oxide whiskers is carbonized into graphite and remains on the surface of the whiskers, which improves the self-lubricating property of the whiskers and thus plays a friction-reducing role. On the other hand, the carbonization temperature is as high as 1000°C, which improves the crystallization degree of the titanium oxide whiskers, improves the strength of the titanium oxide whiskers, and plays a wear-resistant role. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 The cross-sectional SEM image (х400) of the composite material obtained in Example 1;

[0031] Figure 2 The friction performance results of Example 1 and Comparative Examples 1-3 are shown;

[0032] Figure 3 The wear performance results of Example 1 and Comparative Examples 1-3 are shown;

[0033] Figure 4 This is the wear morphology of Comparative Example 1 under the conditions of 200N and 1.4m / s;

[0034] Figure 5 This is the wear morphology of comparative example 2 under the conditions of 200N and 1.4m / s;

[0035] Figure 6 This is the wear morphology of Example 1 under the conditions of 200N and 1.4m / s;

[0036] Figure 7 This is the wear morphology of comparative example 3 under the conditions of 200N and 1.4m / s. DETAILED DESCRIPTION

[0037] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.

[0038] Embodiment 1:

[0039] Metatitanic acid and potassium carbonate were mixed uniformly at TiO2 / K2O=2.5 mol, and sintered at 600°C for 30 min to obtain a mixture of potassium dititanate and potassium tetratitanate;

[0040] The mixture of potassium dititanate and potassium tetratitanate is immersed in a hydrochloric acid solution and stirred until the potassium content in the solid phase is less than 5wt% of the product weight;

[0041] After washing and filtering, the mixture was calcined in a muffle furnace at 600°C for 4 h to obtain titanium oxide whiskers. The most probable pore size of the obtained titanium oxide whiskers was 3 nm and the specific surface area was 85 m 2 / g, pore volume is 0.1cm 3 / g;

[0042] Dissolve the modified asphalt in carbon tetrachloride and benzene, add titanium oxide whiskers while stirring, and heat until the carbon tetrachloride and benzene are completely volatilized to complete the coating;

[0043] The coated titanium oxide whiskers were carbonized, wherein the carbonization process was as follows: heating to 310°C at 2°C / min, maintaining the temperature for 2h, and then heating to 1000°C at 22°C / min, maintaining the temperature for 2h;

[0044] 700 g of polytetrafluoroethylene matrix, 50 g of asphalt-coated modified titanium oxide whisker, 50 g of basalt fiber and 30 g of nano magnesium oxide particles are mixed to obtain a mixture, 170 g of polyparahydroxybenzoate is dissolved in alcohol, and then added to the mixture, and dispersed by high shear stirring. After mixing evenly, the solvent is removed by suction filtering and then dried;

[0045] First, add the dried mixed material into a metal mold, place it on a press, and heat it to 150°C for preheating;

[0046] After the temperature inside and outside the mold is constant, pre-press at a pressure of 5Mpa;

[0047] Maintaining the pressure, a certain heating rate was started to increase the temperature to the final molding temperature of 200°C;

[0048] When the temperature is constant, release the pressure to let the air out, and then immediately apply the final molding pressure of 100MPa. The holding time depends on the size and thickness of the product.

[0049] Release the pressure, stop heating, move the mold onto the insulation blanket, slowly cool down to 200℃, then quickly cool down and demould at around 100℃.

[0050] The cross-sectional SEM image of the composite material prepared in Example 1 is as follows: Figure 1 As shown, the interlaced fibers provide a load-bearing skeleton for the refractory polyparaben, and the nano-oxide particles fill the composite material tightly.

[0051] Comparative Example 1: The difference from Example 1 is that pure polyparahydroxybenzoate is used instead of the composite material.

[0052] Comparative Example 2: The difference from Example 1 is that a mixture of basalt fiber and polyparaben is used instead of the composite material.

[0053] Comparative Example 3: The difference from Example 1 is that a mixture of nano magnesium oxide and polyparaben is used instead of the composite material.

[0054] Performance Test:

[0055] The friction and wear properties of the composite material of Example 1 were investigated using a double-ring end face contact form of an MPX-2000 wear tester. Experimental conditions: load 150N, sliding speed 0.7m / s, 1.4m / s, the dual part is 45# steel, and the material and the dual part are polished with 900-mesh metallographic sandpaper before the test. The material was cleaned with alcohol before and after the test, placed in an oven at 120°C and dried for 8 hours, and the difference between the two masses was taken as the wear amount. The wear amount was measured using an electronic balance with an accuracy of 0.1mg. The friction coefficient and wear rate were both taken as stable stage values. Each data was obtained from 3 samples. A QUANTA-200 scanning electron microscope (SEM) was used to analyze the wear surface of the composite material, and an optical microscope was used to analyze the morphology of the dual surface.

[0056] Among them, the friction performance results are as follows Figure 2 The wear performance results are shown in Figure 3As shown, Comparative Example 1 is recorded as Sample 1, Comparative Example 2 is recorded as Sample 2, Example 1 is recorded as Sample 3, and Comparative Example 3 is recorded as Sample 4.

[0057] from Figure 2 It can be seen that

[0058] The nanoparticle-filled polyparahydroxybenzoate material can increase the overall friction coefficient at a sliding speed of 200N and 0.7m / s, while the fiber material and PTFE filler-filled polyparahydroxybenzoate material reduce the friction coefficient of the composite material, among which the composite material of Example 1 has the best friction performance. When the sliding speed is increased from 0.7m / s to 1.4m / s, the composite material filled with nanoparticles fails within a few minutes due to excessive wear, and the friction coefficients of the composite material filled with fiber material and the composite material of Example 1 both show a decreasing trend.

[0059] from Figure 3 It can be seen that under the condition of sliding speed of 0.7 m / s, the filling of fillers improves the wear performance of the composite materials to varying degrees, among which the wear performance of the composite material in Example 1 is still the best. When the sliding speed is increased from 0.7 m / s to 1.4 m / s, the wear rate of pure polyparaben increases from 5.04×10 -8 cm 3 / Nm increased sharply to 1.85×10 -5 cm 3 / Nm, an increase of 367 times. The single filling of basalt fiber improves the sensitivity of Ekonol wear to speed changes. Among them, the wear performance of the composite material of Example 1 is almost not affected by the sliding speed.

[0060] Wear surface morphology analysis of composite materials of Sample 1-4 Figure 4-7 As shown,

[0061] Figure 4 This is the wear morphology of pure polyparaben under 200N and 1.4m / s conditions. The wear surface is arranged with parallel furrows. This is the result of the plowing effect caused by the abrasive particles generated during the friction process and the micro-protrusions on the dual surface penetrating into the material surface. Figure 5 This is the wear morphology of the basalt fiber and polyparaben mixture. The exposed fiber part replaces the matrix to play a load-bearing role, which reduces the embedding and cutting action of the abrasive particles, inhibits the expansion of the furrow, and thus reduces wear. Figure 6 is the wear morphology of the composite material of Example 1, compared with Figure 5 The wear surface is relatively smooth. It can be seen that the composite material of Example 1 improves the wear performance. Figure 7This is the wear morphology of the mixture of nano-magnesium oxide and polyparaben, showing traces of crushing and plowing.

[0062] The composite material of Example 1 was made into a piston ring and then subjected to performance and bench tests:

[0063] The performance data is shown in the following table:

[0064] project Numeric unit density 2.35 g / cm hardness 65 Shao D Elongation 420 % Compressive strength 35 Mpa

[0065] The bench test was conducted on Example 1. The secondary piston ring made of the composite material was installed on a new hydrogen compressor for testing. After a cumulative operation of 1,200 hours, the wear amount was 12.4 mg, equivalent to a radial wear of 10.33 mg / 1,000 hours, which is far lower than the allowable wear amount of the piston ring and fully meets the use requirements. If calculated based on the wear amount in the later period, the service life of the piston ring can reach more than 15,000 hours.

[0066] From the experimental results, it can be seen that the rolling friction component prepared by using the composite material of Example 1 of the present invention can maintain high compressive strength and low wear rate in a high load and high temperature environment, thereby extending the service life of the component. This material is suitable for fields requiring long-term wear resistance, such as bearings, sliders, seals, etc.

[0067] Finally, it should be noted that: technicians in this industry should understand that the present invention is not limited to the above-mentioned implementation cases. The above-mentioned embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which shall fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.

Claims

1. Low wear and high wear resistance polytetrafluoroethylene based composite material, characterized by: The invention comprises the following components in weight percentage: 60-75% of polytetrafluoroethylene, 10-25% of polyparahydroxybenzoate, 5-10% of asphalt-coated modified titanium oxide whiskers, 5-10% of basalt fibers and 1-5% of nano oxide particles; The asphalt-coated modified titanium oxide whisker is prepared by the following steps: Dissolve the modified asphalt in an organic solvent, add titanium oxide whiskers while stirring, and heat until the organic solvent is completely volatilized to complete the coating; The coated titanium oxide whiskers were carbonized, wherein the carbonization process was as follows: heating to 310°C at 2°C / min, maintaining the temperature for 2 hours, and then heating to 1000°C at 22°C / min, maintaining the temperature for 2 hours.

2. The low-wear and high-wear-resistant polytetrafluoroethylene-based composite material according to claim 1, characterized in that: The organic solvent is selected from carbon tetrachloride, benzene or a mixture thereof.

3. The low-wear and high-wear-resistant polytetrafluoroethylene-based composite material according to claim 1, characterized in that: The nano-oxide particles are selected from one or more of nano-aluminum oxide, nano-silicon oxide, nano-calcium oxide, nano-magnesium oxide or nano-zinc oxide.

4. The low-wear and high-wear-resistant polytetrafluoroethylene-based composite material according to claim 1, characterized in that: The asphalt-coated modified titanium oxide whiskers have an average length of 5-10 μm and an average diameter of 0.2-0.5 μm, the basalt fibers have an average length of 20-50 μm and an average diameter of 4-6 μm, and the nano-oxide particles have a particle size of 10-100 nm.

5. The low-wear and high-wear-resistant polytetrafluoroethylene-based composite material according to claim 1, characterized in that: The titanium oxide whisker is a mesoporous titanium oxide whisker with a pore volume of 0.05-0.4 cm 3 / g, specific surface area>30m 2 / g.

6. The low-wear and high-wear-resistant polytetrafluoroethylene-based composite material according to claim 5, characterized in that: The titanium oxide whisker is prepared by the following steps: Metatitanic acid and potassium carbonate are mixed uniformly at TiO2 / K2O=2.5 mol, and sintered at 600-800°C for 30 min to obtain a mixture of potassium dititanate and potassium tetratitanate; The mixture of potassium dititanate and potassium tetratitanate is immersed in a hydrochloric acid solution and stirred until the potassium content in the solid phase is less than 5wt% of the product weight; After washing with water and filtering, it is calcined in a muffle furnace at 500-800°C for 0.5-8h.

7. A method for preparing a low-wear and high-wear-resistant polytetrafluoroethylene-based composite material, characterized in that: The following steps are involved: A polytetrafluoroethylene matrix, asphalt-coated modified titanium oxide whiskers, basalt fibers and nano-oxide particles are mixed to obtain a mixture, polyparahydroxybenzoate is dissolved in alcohol, and then added to the mixture, and dispersed by high-shear stirring, after being mixed evenly, the solvent is removed by suction filtering, and then dried; First, add the dried mixed material into a metal mold, place it on a press, and heat it to 150°C for preheating; After the temperature inside and outside the mold is constant, pre-press at a pressure of 3.5-7Mpa, maintain the pressure, and start a certain heating rate to the final molding temperature; When the temperature is constant, release the pressure to let the air out, and then immediately apply the final molding pressure. The holding time depends on the size and thickness of the product. Release the pressure, stop heating, move the mold onto the insulation blanket, slowly cool down to 200℃, then quickly cool down and demould at around 100℃.

8. The preparation method according to claim 7, characterized in that: The final molding temperature is 20-200° C., and the final molding pressure is 20-200 MPa.

9. Use of the low-wear and high-wear-resistant polytetrafluoroethylene-based composite material according to any one of claims 1 to 6 in the fields of bearings, sliders, seals, etc. that require long-term wear resistance.

10. Use of the composite material obtained by the preparation method according to claim 7 or 8 in the fields of bearings, sliders, seals, etc. that require long-term wear resistance.